Preparation method of aluminum alloy material suitable for bending forming

Through the preparation method of alloy materials of Si, Fe, Cu, Mn, Mg, Cr, Zn, Ti, B and other elements, combined with a variety of heat treatment and deformation technologies, the problem of cracking and rebound of traditional aluminum alloy materials during bending and forming is solved. , achieves high strength, corrosion resistance and precision machining performance, and meets the needs of complex parts.

CN118957368APending Publication Date: 2024-11-15CIXI YIMEIJIA ALUMINUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411015400.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional aluminum alloy materials are prone to cracking during bending and forming, resulting in an increase in product scrapping rate and an increase in production costs. There is a large rebound after bending, which cannot meet the requirements of precision manufacturing.

Method used

The preparation method of alloy materials using Si, Fe, Cu, Mn, Mg, Cr, Zn, Ti, B and other elements includes smelting, refining, homogenizing heat treatment, extrusion deformation, hot rolling treatment, solid solution quenching and pre-stretching In other steps, by controlling the temperature and processing parameters, the mechanical properties and processing properties of the alloy are optimized.

Benefits of technology

It achieves good bending forming performance of aluminum alloy materials, improves the strength and corrosion resistance of the materials, meets the processing needs of complex parts, and reduces production costs and processing cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy casting, in particular to a preparation method of an aluminum alloy material suitable for bending forming, which comprises the following steps: step 1, providing Si powder, Fe powder, Cu powder, Mn powder, Mg powder, Cr powder, Ti powder, Zn powder, Al-3B intermediate alloy and Al powder; secondly, Si powder, Fe powder, Cu powder, Mn powder, Mg powder, Cr powder, Ti powder, Zn powder, the Al-3B intermediate alloy and Al powder are heated to the first temperature, smelting, refining, melt purification and grain refinement are conducted in sequence, and a first aluminum alloy ingot is obtained after solidification; thirdly, the first aluminum alloy ingot is subjected to homogenizing heat treatment, and a second aluminum alloy ingot is obtained; fourthly, the second aluminum alloy ingot is heated and subjected to extrusion deformation treatment, and a third aluminum alloy ingot is obtained; fifthly, the third aluminum alloy ingot is sequentially subjected to hot rolling treatment and solid solution quenching treatment, and a fourth aluminum alloy ingot is obtained; and sixthly, the fourth aluminum alloy ingot is sequentially subjected to pre-stretching treatment, artificial aging treatment and natural cooling, and the aluminum alloy material suitable for bending forming is obtained. The aluminum alloy material obtained through the preparation method not only has good bending forming performance, but also has high strength and good corrosion resistance, and can meet the machining requirements of various complex parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy casting, and in particular to a method for preparing an aluminum alloy material suitable for bending and forming. Background Art

[0002] Aluminum alloy materials are widely used in the fields of automobile, aerospace, construction and electronics due to their light weight, high strength, corrosion resistance and good processing performance. In these applications, the bending forming performance of aluminum alloy materials is particularly critical because it directly affects the design freedom and production efficiency of the product. However, although traditional aluminum alloy materials perform well in many aspects, there are still some significant problems in the bending forming process. Traditional aluminum alloy materials often crack during bending forming. This is mainly due to the insufficient plasticity and toughness of aluminum alloy materials, which cannot effectively cope with the stress and strain generated during the bending process. Cracking not only leads to an increase in product scrap rate, but also increases production costs and processing cycles. Traditional aluminum alloy materials often have large springback after bending forming. Excessive springback will lead to a decrease in product precision and cannot meet the requirements of precision manufacturing. In order to solve this problem, it is usually necessary to add additional processing steps, such as secondary bending or correction treatment, which not only increases production costs, but also reduces production efficiency. These problems in the existing technology currently limit the application of aluminum alloy materials in the field of high-precision bending forming process. Therefore, it is necessary to develop a new type of aluminum alloy material and its preparation method to improve its bending forming performance and meet the growing market demand. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing an aluminum alloy material suitable for bending and forming in view of the deficiencies in the prior art.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] An aluminum alloy material suitable for bending and forming, characterized in that, by mass percentage, it comprises:

[0006]

[0007]

[0008] A method for preparing the aluminum alloy material suitable for bending and forming as described above, comprising the steps of:

[0009] Step 1, providing Si powder, Fe powder, Cu powder, Mn powder, Mg powder, Cr powder, Ti powder, Zn powder, Al-3B master alloy, and Al powder;

[0010] Step 2: heating Si powder, Fe powder, Cu powder, Mn powder, Mg powder, Cr powder, Ti powder, Zn powder, Al-3B master alloy, and Al powder to a first temperature, sequentially performing smelting, refining, melt purification, and grain refinement to obtain a first aluminum alloy ingot after solidification;

[0011] Step 3: performing homogenization heat treatment on the first aluminum alloy ingot to obtain a second aluminum alloy ingot;

[0012] Step 4: heating the second aluminum alloy ingot and performing extrusion deformation treatment to obtain a third aluminum alloy ingot;

[0013] Step 5, sequentially performing hot rolling treatment and solution quenching treatment on the third aluminum alloy ingot to obtain a fourth aluminum alloy ingot;

[0014] Step 6: The fourth aluminum alloy ingot is subjected to a pre-stretching treatment and an artificial aging treatment in sequence, and is cooled naturally to obtain an aluminum alloy material suitable for bending.

[0015] Preferably, in step 2,

[0016] The first temperature is a melt temperature of 740°C-760°C;

[0017] The melt is purified by argon gas with a gas flow rate of 4m3 / h-4.5m3 / h;

[0018] The refiner used for grain refinement is TiB2.

[0019] Preferably, in step three, the temperature of the homogenization heat treatment is 500° C.-590° C., and the time is 24 h-30 h.

[0020] Preferably, in step 4, the extrusion deformation process includes:

[0021] The extrusion barrel in the extrusion deformation device is preheated to 400°C-450°C, the second aluminum alloy ingot is preheated to 400°C-420°C, and the extrusion deformation is performed to a preset shape. At the same time, the extruded product is air-cooled to complete the extrusion deformation process.

[0022] Preferably, in step 5, the hot rolling treatment adopts a small number of passes and a large reduction rolling.

[0023] The rolling with a small number of passes and a large reduction comprises: heating the third aluminum alloy ingot to 350° C.-400° C., then rolling it on a rolling mill, and then performing annealing.

[0024] Preferably, in step five, the solution quenching treatment includes: quenching the third aluminum alloy ingot after hot rolling at a temperature of 540°C±5°C, heating time of 2h-3h, holding time of 2h-3h, and then water-cooling quenching within 20 seconds to obtain a fourth aluminum alloy ingot.

[0025] Preferably, in step six, the pre-stretching treatment includes: heating the fourth aluminum alloy ingot to 200° C.-300° C., stretching the fourth aluminum alloy ingot by a stretching machine, and cooling the ingot to room temperature after the stretching is completed.

[0026] Preferably, in step six, the aging temperature of artificial aging is 150° C.-170° C., the aging time of artificial aging is 8 h-24 h, and the temperature is naturally lowered to obtain an aluminum alloy material suitable for bending.

[0027] The present invention adopts the above technical solution, and has the following technical effects compared with the prior art:

[0028] The present invention adopts Si, Fe, Cu, Mn, Mg, Cr, Zn, Ti, B, and Al element as a matrix to optimize the mechanical properties and processing properties of the alloy, thereby achieving a good bending forming effect; the present invention performs a homogenization heat treatment on a first aluminum alloy ingot to eliminate the residual stress inside the material and improve the uniformity of the material; then, the second aluminum alloy ingot subjected to the homogenization heat treatment is subjected to an extrusion deformation treatment, and a third aluminum alloy ingot with a preset shape is obtained by controlling parameters such as the extrusion temperature and the extrusion speed; during the extrusion process, the extruded product is air-cooled to control the cooling speed and temperature distribution of the material, thereby further improving the performance of the material; and the third aluminum alloy ingot is subjected to a hot rolling treatment and a solid solution quenching treatment. The hot rolling treatment adopts a rolling method with a small number of passes and a large reduction to reduce the deformation resistance of the material and improve the plasticity of the material; the pre-stretching treatment stretches the material through a stretching machine to eliminate the residual stress inside the material and improve the dimensional stability of the material; the artificial aging treatment controls the aging temperature and aging time to enable the material to obtain stable structure and performance; the aluminum alloy material obtained by the preparation method of the present invention not only has good bending forming performance, but also has high strength and good corrosion resistance, and can meet the processing requirements of various complex parts. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0031] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0032] Example 1

[0033] This embodiment provides an aluminum alloy material suitable for bending and forming, characterized in that, by mass percentage, it includes:

[0034]

[0035] A method for preparing the aluminum alloy material suitable for bending and forming as described above, comprising the steps of:

[0036] Step 1, providing Si powder, Fe powder, Cu powder, Mn powder, Mg powder, Cr powder, Ti powder, Zn powder, Al-3B master alloy, and Al powder;

[0037] Step 2: heating the Si powder, the Fe powder, the Cu powder, the Mn powder, the Mg powder, the Cr powder, the Ti powder, the Zn powder, the Al-3B master alloy, and the Al powder to a melt temperature of 740° C., sequentially performing smelting, refining, melt purification, and grain refinement using a refiner TiB2, and obtaining a first aluminum alloy ingot after solidification;

[0038] The melt is purified by argon gas with a gas flow rate of 4m 3 / h;

[0039] Step 3: performing homogenization heat treatment on the first aluminum alloy ingot to obtain a second aluminum alloy ingot;

[0040] Wherein, the temperature of the homogenization heat treatment is 500°C and the time is 24h;

[0041] Step 4: heating the second aluminum alloy ingot and performing extrusion deformation treatment to obtain a third aluminum alloy ingot;

[0042] The extrusion deformation treatment includes: preheating the extrusion barrel in the extrusion deformation device to 400° C., preheating the second aluminum alloy ingot to 400° C., extruding and deforming the ingot to a preset shape, and air cooling the extruded product, thereby completing the extrusion deformation treatment;

[0043] Step 5, sequentially performing hot rolling treatment and solution quenching treatment on the third aluminum alloy ingot to obtain a fourth aluminum alloy ingot;

[0044] The hot rolling treatment adopts a small number of passes and a large reduction rolling, and the small number of passes and a large reduction rolling comprises: heating the third aluminum alloy ingot to 350° C., then rolling it on a rolling mill, and then performing an annealing treatment;

[0045] The solution quenching treatment comprises: quenching the third aluminum alloy ingot after hot rolling at a temperature of 540°C ± 5°C, heating for 2 hours, holding for 2 hours, and then water-cooling quenching for less than 20 seconds to obtain a fourth aluminum alloy ingot;

[0046] Step six, heating the fourth aluminum alloy ingot to 200°C, stretching the fourth aluminum alloy ingot through a stretching machine, cooling to room temperature after stretching, performing artificial aging treatment after pre-stretching treatment, the aging temperature is 150°C, the aging time of the artificial aging is 8h, and after completing the artificial aging treatment, the temperature is naturally lowered to obtain an aluminum alloy material suitable for bending forming.

[0047] Example 2

[0048] This embodiment provides an aluminum alloy material suitable for bending and forming, characterized in that, by mass percentage, it includes:

[0049]

[0050] A method for preparing the aluminum alloy material suitable for bending and forming as described above, comprising the steps of:

[0051] Step 1, providing Si powder, Fe powder, Cu powder, Mn powder, Mg powder, Cr powder, Ti powder, Zn powder, Al-3B master alloy, and Al powder;

[0052] Step 2: heating the Si powder, the Fe powder, the Cu powder, the Mn powder, the Mg powder, the Cr powder, the Ti powder, the Zn powder, the Al-3B master alloy, and the Al powder to a melt temperature of 760° C., sequentially performing smelting, refining, melt purification, and grain refinement using a refiner TiB2, and obtaining a first aluminum alloy ingot after solidification;

[0053] The melt is purified by argon gas with a gas flow rate of 4.5 m 3 / h;

[0054] Step 3: performing homogenization heat treatment on the first aluminum alloy ingot to obtain a second aluminum alloy ingot;

[0055] Wherein, the temperature of the homogenization heat treatment is 590°C and the time is 30h;

[0056] Step 4: heating the second aluminum alloy ingot and performing an extrusion deformation treatment to obtain a third aluminum alloy ingot;

[0057] The extrusion deformation process includes: preheating the extrusion barrel in the extrusion deformation device to 450° C., preheating the second aluminum alloy ingot to 420° C., extruding and deforming it to a preset shape, and air cooling the extruded product, thereby completing the extrusion deformation process;

[0058] Step 5, sequentially performing hot rolling treatment and solution quenching treatment on the third aluminum alloy ingot to obtain a fourth aluminum alloy ingot;

[0059] The hot rolling treatment adopts a small number of passes and a large reduction rolling, and the small number of passes and a large reduction rolling comprises: heating the third aluminum alloy ingot to 400° C., then rolling it on a rolling mill, and then performing an annealing treatment;

[0060] The solution quenching treatment comprises: quenching the third aluminum alloy ingot after hot rolling at a temperature of 540°C ± 5°C, heating time of 3 hours, holding time of 3 hours, and then water-cooling quenching within 20 seconds to obtain a fourth aluminum alloy ingot;

[0061] Step six, heating the fourth aluminum alloy ingot to 300°C, stretching the fourth aluminum alloy ingot through a stretching machine, cooling to room temperature after stretching, completing the pre-stretching treatment, and performing artificial aging treatment at a temperature of 170°C. The artificial aging time is 24 hours. After completing the artificial aging treatment, the ingot is cooled naturally to obtain an aluminum alloy material suitable for bending.

[0062] In summary, the present invention adopts Si, Fe, Cu, Mn, Mg, Cr, Zn, Ti, B, and Al element as a matrix to optimize the mechanical properties and processing properties of the alloy, thereby achieving a good bending forming effect; the present invention performs a homogenization heat treatment on the first aluminum alloy ingot to eliminate the residual stress inside the material and improve the uniformity of the material; then, the second aluminum alloy ingot that has undergone the homogenization heat treatment is subjected to an extrusion deformation treatment, and a third aluminum alloy ingot with a preset shape is obtained by controlling parameters such as the extrusion temperature and the extrusion speed; during the extrusion process, the extruded product is air-cooled to control the cooling rate and temperature distribution of the material, thereby further improving the performance of the material; the third aluminum alloy ingot is subjected to a hot rolling treatment and a solid solution quenching treatment. The hot rolling treatment adopts a rolling method with a small number of passes and a large reduction to reduce the deformation resistance of the material and improve the plasticity of the material; the pre-stretching treatment stretches the material through a stretching machine to eliminate the residual stress inside the material and improve the dimensional stability of the material; the artificial aging treatment controls the aging temperature and aging time to enable the material to obtain stable structure and performance; the aluminum alloy material obtained by the preparation method of the present invention not only has good bending forming performance, but also has high strength and good corrosion resistance, and can meet the processing requirements of various complex parts.

[0063] The above description is only a preferred embodiment of the present invention, and does not limit the implementation mode and protection scope of the present invention. For those skilled in the art, it should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the specification of the present invention should be included in the protection scope of the present invention.

Claims

1. An aluminum alloy material suitable for bending, characterized in that: In terms of mass percentage, it includes:

2. A method for preparing an aluminum alloy material suitable for bending and forming as claimed in claim 1, characterized in that the steps include: Step 1, providing Si powder, Fe powder, Cu powder, Mn powder, Mg powder, Cr powder, Ti powder, Zn powder, Al-3B master alloy, and Al powder; Step 2: heating the Si powder, the Fe powder, the Cu powder, the Mn powder, the Mg powder, the Cr powder, the Ti powder, the Zn powder, the Al-3B master alloy, and the Al powder to a first temperature, and sequentially performing smelting, refining, melt purification, and grain refinement to obtain a first aluminum alloy ingot after solidification; Step 3: performing homogenization heat treatment on the first aluminum alloy ingot to obtain a second aluminum alloy ingot; Step 4: heating the second aluminum alloy ingot and performing extrusion deformation treatment to obtain a third aluminum alloy ingot; Step 5, sequentially performing hot rolling treatment and solution quenching treatment on the third aluminum alloy ingot to obtain a fourth aluminum alloy ingot; Step six: subjecting the fourth aluminum alloy ingot to a pre-stretching treatment and an artificial aging treatment in sequence, and naturally cooling the ingot to obtain an aluminum alloy material suitable for bending and forming.

3. The method for preparing an aluminum alloy material suitable for bending and forming according to claim 2, characterized in that: In the step 2, The first temperature is a melt temperature of 740°C-760°C; The melt is purified by argon gas with a gas flow rate of 4m 3 / h-4.5m 3 / h; The grain refinement agent used is TiB2.

4. The method for preparing an aluminum alloy material suitable for bending and forming according to claim 2, characterized in that: In the step three, the temperature of the homogenization heat treatment is 500° C.-590° C., and the time is 24 h-30 h.

5. The method for preparing an aluminum alloy material suitable for bending and forming according to claim 2, characterized in that: In the step 4, the extrusion deformation process includes: The extrusion barrel in the extrusion deformation device is preheated to 400°C-450°C, the second aluminum alloy ingot is preheated to 400°C-420°C, and extrusion deformation is performed to a preset shape. At the same time, the extruded product is air-cooled to complete the extrusion deformation process.

6. The method for preparing an aluminum alloy material suitable for bending and forming according to claim 2, characterized in that: In step 5, the hot rolling process is performed by rolling with a small number of passes and a large reduction. The rolling with a small number of passes and a large reduction comprises: heating the third aluminum alloy ingot to 350° C.-400° C., then rolling it on a rolling mill, and then performing annealing treatment.

7. The method for preparing an aluminum alloy material suitable for bending and forming according to claim 2, characterized in that: In step five, the solution quenching treatment includes: setting the quenching temperature of the third aluminum alloy ingot after hot rolling to 540°C±5°C, heating time to 2h-3h, holding time to 2h-3h, and then water-cooling quenching within 20 seconds to obtain a fourth aluminum alloy ingot.

8. The method for preparing an aluminum alloy material suitable for bending and forming according to claim 2, characterized in that: In the step six, the pre-stretching treatment includes: heating the fourth aluminum alloy ingot to 200° C.-300° C., stretching the fourth aluminum alloy ingot by a stretching machine, and cooling the ingot to room temperature after the stretching is completed.

9. The method for preparing an aluminum alloy material suitable for bending and forming according to claim 2, characterized in that: In the step six, the aging temperature of the artificial aging is 150° C.-170° C., the aging time of the artificial aging is 8 h-24 h, and the temperature is naturally lowered to obtain an aluminum alloy material suitable for bending.