Biomedical Mn alloy and preparation method and application thereof
Mn alloy materials prepared by specific proportions of Mn, Fe, Cu and C elements are prepared into rods or silk materials in combination with the process, which solves the shortcomings of existing alloy materials in terms of mechanical properties, degradation rate and biocompatibility, and achieves the goal of achieving Excellent performance and safety of biomedical materials.
Patent Information
- Application Number
- CN202410992512.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-15
AI Technical Summary
When existing biomedical alloy materials are implanted in the body, they have insufficient mechanical properties, unpleasant degradation rate or biotoxicity, resulting in adverse reactions and long-term foreign body retention problems, making it difficult to meet the mechanical strength, degradation rate and biocompatibility at the same time. sexual requirements.
Mn alloy materials prepared with specific proportions of Mn, Fe, Cu and C elements are prepared into bars or wire materials through vacuum smelting, homogenization, turning, hot rolling, annealing and drawing processes to form excellent microstructure. A mixed structure including equiaxed crystals and deformed crystals promotes grain refinement and corrosion degradation.
It realizes excellent mechanical properties and moderate degradation rate of Mn alloy materials, has good biocompatibility and low biotoxicity, and is suitable for medical devices and medical implants, avoiding long-term rejection reactions caused by non-degradable materials and Secondary surgery.
Smart Images

Figure CN118957371A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of biomedical materials, and in particular to a method for preparing a biomedical Mn alloy. Background Art
[0002] At present, biomedical wires are mainly made of non-degradable alloys such as 316L stainless steel, Ti alloy and Co-Cr alloy, as well as degradable alloys such as Mg alloy, Zn alloy and Fe alloy. The preparation process of 316L stainless steel and Ti alloy wires is relatively mature, with low production cost and excellent mechanical properties. However, 316L stainless steel and Ti alloy wires have poor corrosion resistance and wear resistance. After implantation in the body, they are prone to produce harmful micron-sized metal fragments or metal ions due to corrosion and wear, which in turn triggers immune or allergic reactions, produces chronic inflammation, and causes bone dissolution around the implant. Co-Cr alloy wire has high specific strength, good wear resistance, low pitting tendency, and is insensitive to stress corrosion; however, this material is expensive and contains a large amount of biotoxic elements such as Co and Ni. After implantation in the body, it will release a small amount of Co-Cr particles, which often leads to adverse conditions such as chromosome aberrations, local soft tissue allergies and systemic Co poisoning. In addition, the alloy wire is difficult to remove and degrade after being implanted in the body, and will remain in the patient's body for a long time as a foreign body, which will aggravate the above-mentioned negative effects and lead to a prolonged dual antiplatelet treatment time.
[0003] Mg alloy, Zn alloy and Fe alloy wires generally do not contain biotoxic elements. After implantation in the body, they can provide sufficient mechanical support within the prescribed treatment time and then be excreted from the body through normal physiological metabolic pathways, which can avoid the above-mentioned adverse reactions caused by the non-degradable wires. However, the strength and plasticity of Mg alloy wires are low, and the degradation rate is too fast. The vascular stents made of them can only maintain mechanical integrity in the blood vessels for 1-3 months. Premature degradation and collapse of the stent often lead to adverse problems such as vascular recoil, restenosis in the stent and thrombosis in the stent. Although Zn alloy wires have good biocompatibility and moderate degradation rate, their tensile strength is low. Fe alloy wires have excellent mechanical and processing properties, and they have less changes in the local microenvironment of tissues after implantation in the body, and their corrosion byproducts usually do not produce systemic toxicity. However, the degradation rate of Fe alloy wires is too slow, and the woven vascular stents remain almost intact 4 years after implantation in the blood vessel. The strong corrosion products produced by degradation often remain in situ and are easily wrapped by the new intima, thereby hindering the regeneration of vascular tissue.
[0004] Therefore, how to prepare an alloy material that can be used to prepare wires for use in the field of medical devices and medical implants, while also having good mechanical strength, a moderate degradation rate, good biocompatibility, and no biological toxicity, is a difficult problem that needs to be urgently solved in the field of medical devices and biomedical materials. Summary of the invention
[0005] In view of the deficiencies of the above prior art, the present invention provides a biomedical Mn alloy and a preparation method and application thereof. The Mn alloy material of the present invention is prepared from four elements of Mn, Fe, Cu and C in a specific composition ratio. This Mn alloy has the advantages of excellent mechanical strength, moderate degradation rate, good biocompatibility, and no biological toxicity. It can be processed into rods or wires of different sizes and is widely used in the field of medical devices, especially as a material for preparing medical implants. It is specifically achieved through the following technologies.
[0006] In a first aspect of the present invention, a biomedical Mn alloy is provided, wherein the composition, by mass fraction, is composed of 60-75wt.%, 22-37wt.%, 2.75-4.25wt.% of Mn, and 0.25-0.75wt.% of C; the microstructure of the biomedical Mn alloy rod contains only equiaxed crystals, and the size of the equiaxed crystals is 12-25μm; In the microstructure of the biomedical Mn alloy wire, the number of deformed crystals and equiaxed crystals is (0.5-1.5):1, and the size of the equiaxed crystals is 0.15-0.65 μm; or, the microstructure of the biomedical Mn alloy wire contains only equiaxed crystals, and the size of the equiaxed crystals is 2.2-2.8 μm.
[0007] It should be understood that the biomedical Mn alloy provided by the present invention is divided into two material forms, rods and wires, according to the differences in actual application scenarios. These two material forms have the above-mentioned corresponding microstructures. The microstructure of the Mn alloy rod contains only equiaxed crystals. The microstructure of the Mn alloy wire can be a mixed structure containing both deformed crystals and equiaxed crystals in an amount of (0.5-1.5): 1, or it can be a structure containing only equiaxed crystals, depending on the differences in processing technology.
[0008] The Mn alloy provided by the present invention has Mn as the main element component, the Mn electrode potential is lower than that of Fe, and when the Mn content is 60-75wt.%, the alloy is an austenite phase with low magnetic susceptibility. The present invention also adds Fe, Cu and C elements to the Mn alloy material. After in-depth research by the inventors of the present invention, it was found that the microstructure of the rods and wires of the Mn alloy presents a structure containing only equiaxed crystals, or a mixture of deformed crystals and equiaxed crystals.
[0009] It is easy to know that no matter how the Mn alloy provided by the present invention is prepared, as long as it meets the above-mentioned element composition and the above-mentioned microstructure requirements, it belongs to the protection scope of the present invention.
[0010] In the Mn alloy of the present invention, when the C content is 0.25-0.75wt.%, it can play a role of solid solution strengthening, and dispersed fine carbides will be generated in the microstructure during smelting, which promotes grain nucleation and restricts grain growth, thereby playing a role of grain refinement. During subsequent processing and heat treatment, the fine dispersed carbides are oxidized to form dispersed black oxides, which play a role of second phase strengthening, and form a micro galvanic corrosion pair with the matrix, accelerating the corrosion degradation of the Mn alloy.
[0011] Grain refinement can not only play a role in grain refinement and strengthening, but also increase the grain boundary density and accelerate the intergranular corrosion of the alloy, ultimately significantly improving the mechanical and degradation properties of the Mn alloy.
[0012] When the Cu content is 2.75-4.25wt.%, it can be completely dissolved in the alloy without forming precipitation, and play a solid solution strengthening role together with C. 2+ It has a strong antibacterial effect, can promote the growth of smooth muscle cells and help the recovery of angiogenesis and blood vessel reconstruction.
[0013] The Mn alloy provided by the present invention is based on Mn, and the electrode potential of Mn is lower than that of Fe and can stabilize the austenite phase; the theoretical degradation rate of the corresponding wire is higher than that of the Fe wire, and only contains the austenite phase with low magnetic susceptibility, and has excellent magnetic resonance imaging performance, and is suitable for the preparation of medical devices such as degradable vascular stents.
[0014] In terms of the degradation rate of Mn alloy wire: the present invention uses Mn with a lower electrode potential than Fe as the base, and the drawn wire (equiaxed crystal size is 0.15-0.65μm) and the energized annealed wire (equiaxed crystal size is 2.2-2.8μm) have fine grains, high grain boundary density and strong intergranular corrosion, and a large amount of black oxides that can form micro-galvanic corrosion pairs with the matrix are dispersed in the organization. The prepared Φ3 rotary forged annealed Mn alloy round rod is statically immersed in Hank's solution for 1-14 days, and the degradation rate reaches 0.16-0.25mm·year -1 The same method was used to test the Φ0.1 drawn Mn alloy wire, and the degradation rate was higher than that of the round rod, reaching 0.20-0.30mm·year -1 Therefore, the Mn alloy material of the present invention, whether it is a wire or a rod, basically meets the degradation rate of the degradable vascular stent of 0.20 mm·year -1 service requirements.
[0015] In terms of biocompatibility and biotoxicity: Mn, Fe, Cu and C are all constant elements in the human body or elements that can play important physiological functions. These elements have very good biocompatibility and lower biotoxicity.
[0016] Furthermore, the composition of the biomedical Mn alloy provided by the present invention is composed of 60wt.%, 35-37wt.% Fe, 2.75-4.25wt.% Cu, and 0.25-0.75wt.% C in terms of mass fraction.
[0017] Furthermore, the biomedical Mn alloy provided by the present invention consists of 60wt.%, 36wt.%, 3.5wt.% of Mn, and 0.5wt.% of Fe.
[0018] Furthermore, the composition of the biomedical Mn alloy provided by the present invention is composed of 75wt.%, 20-22wt.% of Mn, 2.75-4.25wt.%, and 0.25-0.75wt.% of C by mass fraction.
[0019] Furthermore, the biomedical Mn alloy provided by the present invention consists of 75wt.%, 21wt.%, 3.5wt.%, and 0.5wt.% of Mn.
[0020] The second aspect of the present invention also provides a method for preparing biomedical Mn alloy wire, comprising the following steps: taking pure Mn, Fe, Cu and C particles and mixing them uniformly, and vacuum melting them to obtain a cast alloy round rod; The cast alloy round bar is subjected to homogenization, turning, hot rolling, first annealing, rotary forging, second annealing and grinding in sequence to obtain a rotary forging annealed Mn alloy bar that meets the size requirements. The Mn alloy bar has a microstructure containing only equiaxed crystals, and the size of the equiaxed crystals is 12-25 μm.
[0021] Alternatively, based on the above preparation method, the Mn alloy rod is further drawn to obtain a drawn Mn alloy wire that meets the size requirements. In the microstructure of the drawn Mn alloy wire, the number of deformed crystals and equiaxed crystals is (0.5-1.5):1, and the size of the equiaxed crystals is 0.15-0.65 μm.
[0022] Those skilled in the art should be aware that in the preparation method of the above-mentioned Mn alloy of the present invention, the pure Mn, Fe, Cu and C particles selected can be commercially available materials that meet medical grade requirements.
[0023] Generally, the purity of the pure Mn, Fe, Cu and C particles is not less than 99.99% of industrial pure Mn, Fe, Cu and C particles.
[0024] The above-mentioned preparation method of the Mn alloy of the present invention is to prepare a rotary forging annealed Mn alloy rod by vacuum melting, homogenizing, turning, hot rolling, first annealing, rotary forging, second annealing and grinding of pure Mn, Fe, Cu and C particles in a specific proportion.
[0025] When the rotary forging annealed Mn alloy rod is used to further prepare the wire, a drawing (single-pass drawing / multi-pass drawing) process is performed after grinding to obtain a drawn Mn alloy wire.
[0026] Those skilled in the art should also be aware that each of the above-mentioned processing stages can be implemented using commonly used technologies in the industry, and the process parameters of each processing stage can be implemented using conventional or easily known technologies.
[0027] Optionally, in the above preparation method of the present invention, the temperature of the homogenization treatment is 1050-1150° C., and the treatment time is 4-8 hours.
[0028] Optionally, in the above preparation method of the present invention, the hot rolling temperature is 850-950° C., and the deformation amount is 85-95%.
[0029] Optionally, in the above preparation method of the present invention, the temperature of the first annealing is 950-1050° C., and the annealing time is 0.5-1.5 h.
[0030] Optionally, in the above preparation method of the present invention, the temperature of rotary forging is 400-500° C., and the deformation amount is 85-95%.
[0031] Optionally, in the above preparation method of the present invention, the temperature of the second annealing is 800-1000° C., and the annealing time is 0.2-0.8 h.
[0032] Optionally, in the above-mentioned preparation method of the present invention, when multiple drawing passes are adopted, the cold drawing deformation of each drawing pass is 40-90%, and the total drawing deformation is 99.7-99.9%.
[0033] Furthermore, the drawn Mn alloy wire is subjected to an electric annealing treatment to obtain an electric annealed Mn alloy wire; the conditions for the electric annealing treatment are: annealing at a current of 0.65-0.85 A for 3-30 seconds.
[0034] The inventors of the present invention have found that, based on the above preparation method, the drawn Mn alloy wire is subjected to an electric annealing treatment in the above manner, so that it undergoes complete recrystallization during the electric annealing, eliminating the residual stress of drawing; the deformed grains are equiaxed, the equiaxed crystals grow (the size is 2.2-2.8μm), and the plasticity is restored, which can further improve the comprehensive mechanical properties of the Mn alloy wire. The microstructure of the Mn alloy wire after electric annealing contains only equiaxed crystals, and the size of the equiaxed crystals is 2.2-2.8μm.
[0035] Furthermore, the condition of the power-on annealing treatment is: annealing at a current of 0.7 A for 30 seconds.
[0036] Optionally, the first annealing treatment method is: annealing at 950-1050° C. for 0.5-1.5 h.
[0037] Optionally, the second annealing treatment method is: annealing at 800-1000° C. for 0.2-0.8 h.
[0038] Furthermore, the rotary forging annealed round bar is subjected to a single-pass drawing process, and the drawing deformation amount is 99.7-99.9%.
[0039] In the third aspect of the present invention, the present invention also provides the use of the above biomedical Mn alloy in the preparation of medical devices.
[0040] Furthermore, in the application method of the above-mentioned biomedical Mn alloy, the medical devices include but are not limited to sutures, implant stents, bone nails, bone needles, hemostatic clips, wire anchors, screws, bone plates, bone sleeves, intramedullary nails, anastomosis devices, orthodontic archwires, pacemaker wires and venous filters.
[0041] It is easy for a person skilled in the art to understand that, according to the above different uses, Mn alloy rods or wires of different sizes (diameters) can be selected.
[0042] Furthermore, for example, the Mn alloy rod can be used as bone nails, bone needles, hemostatic clips, wire anchors, screws, bone plates, bone sleeves and other common human or animal implant materials in surgery. The specific size of the Mn alloy rod can be appropriately adjusted according to actual needs.
[0043] Furthermore, for example, the Mn alloy wire can be used as implant materials such as orthodontic archwires, pacemaker wires, and venous filters. The specific size of the Mn alloy wire can be appropriately adjusted according to actual needs.
[0044] Optionally, common alloy rods have common sizes such as Φ3. Optionally, common Mn alloy wire sizes include diameter (mm) parameters such as Φ0.1, Φ0.125, Φ0.15, Φ0.175, Φ0.2 and Φ0.25. Regardless of how the size is adjusted, these Mn alloy wires and rods belong to the protection scope of the present invention.
[0045] Compared with the prior art, the present invention is beneficial in that: 1. The present invention provides a biomedical Mn alloy, which has excellent mechanical properties through the synergistic combination of four elements of Mn, Fe, Cu and C in a specific ratio; The yield strength of the prepared Φ3 rotary forging annealed round rod reaches up to 262MPa, the tensile strength reaches up to 617MPa, the elongation reaches up to 47%, and the elastic modulus reaches up to 172GPa; it fully meets the requirements of tensile yield strength>200MPa, tensile strength>300MPa and elongation>18% for degradable vascular stents; The tensile strength of the prepared Φ0.1 drawn Mn alloy wire reaches up to 682MPa, and the elongation is generally between 18-24%.
[0046] 2. The degradation rate of the Mn alloy provided by the present invention is moderate. After static immersion in Hank's solution for 1-14 days, the degradation rate of the prepared Φ3 rotary forging annealed Mn alloy round rod reaches 0.16-0.25 mm·year -1 The degradation rate of the Φ0.1 drawn Mn alloy was 0.20-0.30 mm·year -1 , and has good biocompatibility and no biological toxicity. After the treatment is completed, the Mn alloy wire can be gradually and evenly degraded within a controllable time and completely absorbed by the human body, which can avoid long-term rejection reactions and secondary surgeries caused by the non-degradable wire, and can reduce the physical and economic burden on patients.
[0047] 3. The present invention provides a method for preparing biomedical Mn alloy wire, which comprises preparing a rotary forging annealed Mn alloy rod by vacuum melting, homogenization, turning, hot rolling, first annealing, rotary forging, second annealing, and grinding; and further preparing a drawn Mn alloy wire by single-pass / multi-pass drawing.
[0048] On this basis, the present invention further performs electrical annealing after drawing to eliminate residual drawing stress and further improve the comprehensive mechanical properties of the wire.
[0049] 4. In the method for preparing Mn alloy wire provided by the present invention, the alloy round rod after rotary forging and annealing can be drawn by multiple passes; or it can be directly formed by single-pass drawing, which is simple to process and saves production time and equipment. The equipment used in each process of the preparation method is relatively simple, which is suitable for scale-up production and promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 The scanning electron microscope images of the microstructure of the Φ0.1 Mn alloy wire (not annealed by electric current) of Example 1 at magnifications of 50,000 (left) and 100,000 (right); Figure 2 Scanning electron microscope images of the microstructure of the Φ0.1 Mn alloy wire (0.7A annealing for 30s) of Example 2 at magnifications of 10000 (left) and 30000 (right); Figure 3 The scanning electron microscope images of the microstructure of the Φ0.1 Mn alloy wire (0.75A annealing for 15s) of Example 3 at magnifications of 5000 (left) and 10000 (right); Figure 4 The scanning electron microscope images of the microstructure of the Φ0.1 Mn alloy wire (0.75A annealing for 30s) of Example 4 at magnifications of 5000 (left) and 10000 (right); Figure 5 The scanning electron microscope images of the microstructure of the Φ0.1 Mn alloy wire (0.8A annealing for 5s) of Example 5 at magnifications of 5000 (left) and 10000 (right); Figure 6 The scanning electron microscope images of the microstructure of the Φ0.1 Mn alloy wire (0.8A annealing for 10s) of Example 6 at magnifications of 10000 (left) and 30000 (right); Figure 7 The tensile curve of the annealed round bar of Example 1 (left figure) and the mechanical properties comparison of some traditional degradable Mg alloys, Zn alloys and Fe alloys of Comparative Example 3 (right figure); in the right figure, RF-800℃ means that the second annealing of Example 1 is annealing at 800℃ for 0.4h, and RF-1-1000℃ means that the second annealing of Example 1 is annealing at 1000℃ for 0.6h; Figure 8 The degradation weight loss per unit area and degradation rate changes of the Mn alloy wire prepared in Example 1 when statically immersed in Hank's solution for 1-14 days (left figure), and the comparison of the degradation rates of the traditional degradable Mg alloy wire, Zn alloy wire and Fe alloy wire in the literature (right figure); Figure 9-10 This is the cell compatibility test result of the Φ0.1 Mn alloy wire prepared in Example 2. DETAILED DESCRIPTION
[0051] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0052] In some specific implementation cases of the present invention, the composition of the Mn alloy is calculated by mass fraction and consists of Mn 60-75wt%, Fe 22-37wt%, Cu 2.75-4.25wt%, and C 0.25-0.75wt%.
[0053] Furthermore, in some specific implementation cases of the present invention, the composition of the Mn alloy consists of Mn 60wt.%, Fe 35-37wt.%, Cu 2.75-4.25wt.%, and C 0.25-0.75wt.%.
[0054] Furthermore, in some other specific implementation cases of the present invention, the composition of the Mn alloy consists of Mn 75wt.%, Fe20-22wt.%, Cu 2.75-4.25wt.%, and C 0.25-0.75wt.%.
[0055] Furthermore, the composition of the Mn alloy consists of Mn 60wt.%, Fe 36wt.%, Cu 3.5wt.%, and C 0.5wt.%.
[0056] Furthermore, the composition of the Mn alloy consists of Mn 75wt.%, Fe 21wt.%, Cu 3.5wt.%, and C 0.5wt.%.
[0057] In some specific implementation cases of the present invention, the biomedical Mn alloy wire (drawn state) provided by the present invention has a microstructure of a mixture of deformed crystals and equiaxed crystals, the number of deformed crystals and equiaxed crystals is (0.5-1.5):1, and the grain size is 0.15-0.65 μm.
[0058] In some specific implementation cases of the present invention, the biomedical Mn alloy wire (electrically annealed state) provided by the present invention contains only equiaxed crystals in its microstructure, and the size of the equiaxed crystals is 2.2-2.8 μm.
[0059] In some specific implementation cases of the present invention, the biomedical Mn alloy rod (spin-forging annealing state) provided by the present invention has a microstructure containing only equiaxed crystals, and the size of the equiaxed crystals is 12-25 μm.
[0060] In some specific implementation cases of the present invention, the preparation method of the Mn alloy wire is: Pure Mn, Fe, Cu and C particles are mixed evenly, and then put into a crucible of a vacuum induction melting furnace for vacuum melting to obtain a cast Mn alloy round rod; The cast alloy round bar is subjected to homogenization, turning, hot rolling, first annealing, rotary forging, second annealing, and grinding (finish grinding) in sequence to obtain a rotary forging annealed Mn alloy bar that meets the size requirements. The microstructure of this Mn alloy bar contains only equiaxed crystals, and the size of the equiaxed crystals is 12-25μm.
[0061] On this basis, the rotary forging annealed Mn alloy rod is also drawn to obtain a drawn Mn alloy wire that meets the size requirements. In the microstructure of the drawn Mn alloy wire, the number of deformed crystals and equiaxed crystals is (0.5-1.5):1, and the size of the equiaxed crystals is 0.15-0.65μm.
[0062] Those skilled in the art should know that the raw materials for preparing the Mn alloy wire are generally industrial pure Mn, pure Fe, pure Cu and pure C particles with a purity of not less than 99.99%.
[0063] In some other specific implementation cases of the present invention, based on the above-mentioned method for preparing the Mn alloy wire, the drawn Mn alloy wire is subjected to an electric annealing treatment with an electric current of 0.65-0.85A and an annealing time of 3-30s to produce a final electric annealed Mn alloy wire.
[0064] In some other specific implementation cases of the present invention, the current of the power-on annealing treatment is 0.7A, and the annealing time is 30s.
[0065] Those skilled in the art should also be aware that, in the Mn alloy wire preparation methods provided in some implementation cases of the present invention, process steps such as vacuum melting, homogenization, turning, hot rolling, first annealing, rotary forging, second annealing, grinding, and drawing (single-pass drawing / multi-pass drawing) can all be achieved using commonly used technologies in the industry, and the process parameters of each processing stage can use conventional or easily known technologies.
[0066] In some specific implementation cases of the present invention, the homogenization treatment conditions of the above-mentioned preparation method of the Mn alloy wire can be selected as: the temperature is 1050-1150° C., and the treatment time can be selected as 4-8 hours.
[0067] In some specific implementation cases of the present invention, in the method for preparing the above-mentioned Mn alloy wire, the hot rolling conditions can be selected as: a temperature of 850-950° C. and a deformation amount of 85-95%.
[0068] In some specific implementation cases of the present invention, in the method for preparing the above-mentioned Mn alloy wire, the conditions for the first annealing can be selected as: temperature of 950-1050° C., and annealing time of 0.5-1.5 h.
[0069] In some specific implementation cases of the present invention, in the method for preparing the above-mentioned Mn alloy wire, the conditions for rotary forging can be selected as: temperature of 400-500° C., and deformation of 85-95%.
[0070] In some specific implementation cases of the present invention, in the method for preparing the above-mentioned Mn alloy wire, the conditions for the second annealing can be selected as: temperature of 800-1000° C., and annealing time of 0.2-0.8 h.
[0071] In some specific implementation cases of the present invention, in the method for preparing the above-mentioned Mn alloy wire, when multiple drawing passes are adopted, the cold drawing deformation of each pass is 40-90%, and the total drawing deformation is 99.7-99.9%.
[0072] Those skilled in the art should also know that, in the method for preparing the Mn alloy wire, the homogenization treatment is for dissolving back and dispersing the precipitates in the structure; the turning is for removing the oxide layer on the surface of the alloy round rod; and the first annealing is for promoting the recrystallization of the alloy round rod.
[0073] It should be known to those skilled in the art that the size of the Mn alloy wire is adjusted according to the specific requirements of different medical devices. Common Mn alloy wire sizes include diameter parameters such as Φ0.1, Φ0.125, Φ0.15, Φ0.175, Φ0.2 and Φ0.25. Mn alloy wires of these sizes all fall within the scope of protection of the present invention.
[0074] Hot rolling, rotary forging and drawing are used to reduce the diameter of the alloy round bar; grinding is used to remove the surface oxide layer and smooth the surface of the alloy round bar, and the second annealing is used to promote the recrystallization of the alloy round bar. The equipment used to prepare Mn alloy wire includes vacuum induction melting furnace, box-type resistance furnace, precision lathe and grinder, small rolling mill, DC power supply and metal drawing machine. These common equipment in this field are easy to obtain and widely used.
[0075] Example 1 The Mn alloy wire provided in this embodiment is prepared by the following method: (1) Industrial pure Mn, pure Fe, pure Cu and pure C particles with a purity of 99.9% were mixed in a mass ratio of 60wt.%, 36wt.%, 3.5wt.% and 0.5wt.%, and then loaded into a crucible of a vacuum induction melting furnace (vacuum degree of 1×10 - 4 Pa) to obtain a Φ40 alloy cast round rod, namely Mn-36Fe-3.5Cu-0.5C; (2) The alloy cast round bars were homogenized, turned, hot rolled and annealed for the first time to obtain Φ10 hot-rolled annealed round bars. The homogenization temperature and time were 1100℃ and 6h, the turning depth was 2.5mm, the hot rolling temperature and deformation were 900℃ and 90%, and the first annealing temperature and time were 1000℃ and 1h; (3) The hot-rolled annealed round bar is subjected to rotary forging, secondary annealing and grinding to obtain a Φ3 rotary forged annealed round bar. The rotary forging temperature and deformation amount are 450°C and 90%; The second annealing temperature and time are 800℃ annealing for 0.4h, or 1000℃ annealing for 0.6h, and the grinding depth is 0.1mm; (4) The rotary forging annealed round bar with a smooth surface and no defects is subjected to multiple cold drawing processes. The diameter change of the round bar after each cold drawing process is: Φ3→Φ2→Φ1.5→Φ1→Φ0.75→Φ0.5→Φ0.25→Φ0.1, the total deformation is 99.9%, and the Mn alloy wire is obtained.
[0076] Embodiment 2-6 The preparation method of the Mn alloy wire provided in Examples 2-6 is based on the method in Example 1 (the second annealing method is annealing at 1000°C for 0.6h), and an electric annealing treatment is performed after drawing to obtain the final Mn alloy wire product. That is, the drawn Φ0.1 Mn alloy wire is annealed.
[0077] The power-on annealing methods of the present embodiments 2-6 are 0.7A current annealing for 30s, 0.75A current annealing for 15s, 0.75A current annealing for 30s, 0.8A current annealing for 5s and 0.8A current annealing for 10s.
[0078] Embodiment 7-11 The preparation methods of the Mn alloy wires provided in Examples 7-11 are basically the same as those in Example 2 (i.e., the electric annealing method is annealing with a current of 0.7 A for 30 seconds), except that the composition of the element components is changed in each example. The contents of the element components in the Mn alloy wires of Examples 7-11 are shown in Table 1 below, respectively, in terms of mass fraction.
[0079] Table 1 Mass proportion of each element composition of Mn alloy wire, %
[0080] Comparative Example 1 The alloy wire provided in this comparative example consists of 60wt.%, 36wt.%, and 4wt.% of Mn, ie, no C is contained, in terms of mass fraction.
[0081] The preparation method of the alloy wire is as follows: (1) Industrial pure Mn, pure Fe and pure Cu particles with a purity of 99.9% were mixed in a mass ratio of 60wt.%, 36wt.% and 4wt.%, and then loaded into a crucible of a vacuum induction melting furnace (vacuum degree of 1×10 -4 Pa) to obtain a Φ40 alloy cast round rod, namely Mn-36Fe-4Cu; (2) The alloy cast round bars were homogenized, turned, hot rolled and annealed for the first time to obtain Φ10 hot-rolled annealed round bars. The homogenization temperature and time were 1100℃ and 6h, the turning depth was 2.5mm, the hot rolling temperature and deformation were 900℃ and 90%, and the first annealing temperature and time were 1000℃ and 1h; (3) The hot-rolled annealed round bar is subjected to rotary forging, secondary annealing and grinding to obtain a Φ3 rotary forged annealed round bar. The rotary forging temperature and deformation amount are 450°C and 90%, the secondary annealing temperature and time are 1000°C and 0.6h, and the grinding depth is 0.1mm; (4) The rotary forging annealed round bar with a smooth surface and no defects is subjected to multiple cold drawing processes. The diameter change of the rotary forging annealed round bar after each cold drawing process is: Φ3→Φ2→Φ1.5→Φ1→Φ0.75→Φ0.5→Φ0.25→Φ0.1, the total deformation is 99.9%, and the Mn alloy wire is obtained.
[0082] Comparative Example 2 The alloy wire provided in this comparative example is composed of 60wt.%, 36wt.% Fe and 4wt.% Cu in terms of mass fraction, i.e., it does not contain C. The preparation method of the alloy wire in this comparative example is to perform an electric annealing treatment after drawing. The specific method is: (1) Industrial pure Mn, pure Fe and pure Cu particles with a purity of 99.9% were mixed in a mass ratio of 60wt.%, 36wt.% and 4wt.%, and then loaded into a crucible of a vacuum induction melting furnace (vacuum degree of 1×10 -4 Pa) to obtain a Φ40 alloy cast round rod, namely Mn-36Fe-4Cu; (2) The alloy cast round bars were homogenized, turned, hot rolled and annealed for the first time to obtain Φ10 hot-rolled annealed round bars. The homogenization temperature and time were 1100℃ and 6h, the turning depth was 2.5mm, the hot rolling temperature and deformation were 900℃ and 90%, and the first annealing temperature and time were 1000℃ and 1h; (3) The hot-rolled annealed round bar is subjected to rotary forging, secondary annealing and grinding to obtain a Φ3 rotary forged annealed round bar. The rotary forging temperature and deformation amount are 450°C and 90%, the secondary annealing temperature and time are 1000°C and 0.6h, and the grinding depth is 0.1mm; (4) The rotary forging annealed round bar with a smooth surface and no defects is subjected to multiple cold drawing processes. The diameter change of the rotary forging annealed round bar after each cold drawing process is: Φ3→Φ2→Φ1.5→Φ1→Φ0.75→Φ0.5→Φ0.25→Φ0.1, the total deformation is 99.9%; (5) The drawn Mn alloy wire of step (4) is subjected to electrical annealing, specifically annealing at a current of 0.7 A for 30 seconds; and a final product of the alloy wire in the electrical annealing state is obtained.
[0083] Comparative Example 3: Traditional biodegradable Mg alloy, Zn alloy and Fe alloy In this comparative example, conventional degradable Mg alloy, Zn alloy and Fe alloy rods with a size of Φ3 were prepared respectively, and their composition, mechanical properties and elongation are shown in Table 2. The conventional degradable Mg alloy, Zn alloy and Fe alloy rods with a size of Φ3 were subjected to a static immersion test in Hank's solution for 1-14 days to test the degradation rate.
[0084] In the table, taking "Fe-20Mn-3Cu" as an example, it means that the alloy is based on Fe, in which (by mass fraction) the Mn element content is 20wt.%, and the Cu element content is 3wt.%.
[0085] Table 2 Related properties of alloy bars
[0086] As can be seen from Table 2 above, the above-mentioned traditional biodegradable Mg alloys, Zn alloys and Fe alloys either have good mechanical properties but average elongation or degradation performance, or good elongation but insufficient mechanical properties. These alloy rods cannot take into account excellent mechanical properties, biocompatibility, good elongation and degradation rate.
[0087] Test Example 1: Comparison of microstructures of the Mn alloys prepared in Examples 1-6.
[0088] The microstructures of the Φ3 rotary forged annealed round rods, Φ0.1 drawn Mn alloy wires and Φ0.1 electrically annealed Mn alloy wires prepared in Examples 1-6 were observed after hot mounting, grinding and polishing.
[0089] from Figure 1 It can be seen that in Example 1, the Mn alloy wire undergoes incomplete dynamic recrystallization during multi-pass cold drawing, and the number of deformed crystals and equiaxed crystals in the drawn microstructure is equivalent, and the grain size is less than 1 μm (about 0.65 μm).
[0090] from Figure 2-6 It can be seen that the Mn alloy wires of Examples 2-6 that have been drawn and electrically annealed undergo complete recrystallization during electrical annealing, the deformed crystals in the structure gradually become equiaxed, and the equiaxed crystals grow. The wires oxidize during electrical annealing, and a small amount of dispersed black oxides are generated in their microstructure.
[0091] After annealing at 0.7A for 30s, 0.75A for 15s, 0.75A for 30s, 0.8A for 5s, and 0.8A for 10s, the equiaxed grain sizes in the microstructure of the Mn alloy wires of Examples 2-6 were 2.2μm, 2.7μm, 2.8μm, 2.6μm, and 2.8μm, respectively. It can be seen that in general, the equiaxed grain size increases with the increase of the energization time and current density.
[0092] Finally, after observation and statistics, it was found that the microstructure of the Φ3 rotary forging annealed round rod prepared in Example 1-6 contained only equiaxed crystals with a size of 12-25μm. The microstructure of the Φ0.1 drawn Mn alloy wire prepared in Example 1-6 contained both deformed crystals and equiaxed crystals, the number of deformed crystals and equiaxed crystals was (0.5-1.5):1, and the grain size was 0.15-0.65μm. The microstructure of the Φ0.1 electrically annealed Mn alloy wire prepared in Example 1-6 contained only equiaxed crystals with a size of 2.2-2.8μm.
[0093] After analysis, the smaller the equiaxed crystal size and the more uniform the size, the better the mechanical properties of the Mn alloy wire. As the current increases and the power-on time increases, the equiaxed crystal size gradually increases, and the strength of the Mn alloy wire gradually decreases. As the equiaxed crystal size of the Mn alloy wire increases and the equiaxed crystal size becomes more uniform, the plasticity of the Mn alloy wire gradually increases. As the current continues to increase and the time continues to increase, a loose oxide layer will form on the surface of the Mn alloy wire, resulting in a decrease in the plasticity of the Mn alloy wire.
[0094] Test Example 2: Mechanical property test of the Mn alloy wires prepared in Examples 1-11 and Comparative Examples 1-2.
[0095] The Φ0.1 Mn alloy wires prepared in Examples 1-11 and Comparative Examples 1-2 were subjected to a tensile test, and the obtained tensile strength (UTS) and elongation (EL) are shown in Table 3 below.
[0096] Table 3 Mechanical properties of Φ0.1 Mn alloy wire
[0097] As can be seen from Table 3 above, compared with Comparative Example 1, the tensile strength and elongation of the alloy wire of Example 1 have been significantly improved, which shows that the alloy composition of the present invention significantly improves the mechanical properties of the alloy material. After annealing at 0.7A current for 30s, 0.75A current for 15s and 30s, and 0.8A current for 5s and 10s, the tensile strength of the prepared Φ0.1 energized annealed Mn alloy wire is 682MPa, 614MPa, 598MPa, 557MPa and 514MPa, and the corresponding elongation is 22%, 18%, 23%, 20% and 21%. It can be seen that the tensile strength of the Mn alloy wire decreases with the increase of current density and energization time, but the elongation does not change significantly. After analysis, this may be related to the presence of a small amount of dispersed black oxide in the microstructure of the Mn alloy wire and the presence of a loose oxide layer of about 3.2μm on the surface.
[0098] Test Example 3: Mechanical property test of the Mn alloy bars prepared in Examples 1 and 7-11 and Comparative Example 1.
[0099] In this test example, tensile tests were performed on the Φ3 rotary forging annealed round bars prepared in Examples 1 and 7-11, and the Φ3 Mn alloy bars (without C) prepared in Comparative Example 1.
[0100] The tensile curve of the alloy rod of Example 1 is as follows: Figure 7 As shown in the left figure, the mechanical properties of the alloy rod of Example 1 and the traditional degradable Mg alloy, Zn alloy and Fe alloy of Comparative Example 3 are compared as shown in Figure 7 As shown in the right figure. Figure 7 RF-800°C indicates that the second annealing of Example 1 is annealing at 800°C for 0.4h, and RF-1-1000°C indicates that the second annealing of Example 1 is annealing at 1000°C for 0.6h. Figure 7 The right picture comes from existing literature.
[0101] The test results of the mechanical properties (yield strength YS, tensile strength UTS, elongation EL and elastic modulus E) of Examples 1 and 7-11 and Comparative Example 1 are shown in Table 4 below.
[0102] Table 4 Comparison of mechanical properties of Mn alloy bars
[0103] from Figure 6 As shown in Table 4 above, the Mn alloy bars prepared in Examples 1-11 have good plasticity and high strength. Among them, the Mn alloy bar of Example 1 has a maximum yield strength of 262 MPa, a maximum tensile strength of 617 MPa, a maximum elongation of 47%, and a maximum elastic modulus of 172 GPa. After rotary forging annealing, the comprehensive performance of the alloy is significantly better than that of traditional degradable Mg alloys, Zn alloys, and Fe alloys, and fully meets the requirements of tensile yield strength of degradable vascular stents>200 MPa, tensile strength>300 MPa, and elongation>18%.
[0104] Test Example 4: Degradation performance test of Φ3 rotary forging annealed Mn alloy bars prepared in Example 1 and Comparative Example 1.
[0105] The intermediate products "Φ3 rotary forged annealed round rods" prepared in Example 1 and Comparative Example 1 were subjected to static immersion tests in Hank's solution. The static immersion lasted for 14 days, and the degradation weight loss per unit area (mg·cm) was recorded after immersion for 1, 3, 7 and 14 days. -2 ) and degradation rate (mm·year -1 ). The test results are as follows Figure 8 and as shown in Table 5 below.
[0106] Table 5 Comparison of degradation properties of alloy materials
[0107] from Figure 8 As shown in Table 5 above, the degradation weight loss per unit area of the rotary forged annealed round rod of Example 1 after static immersion for 14 days is 3.46 mg·cm -2 , the degradation rate is 0.12mm·year -1 The degradation rate after static immersion for 14 days is lower than that of some Mg alloys, but higher than that of most Fe alloys and Zn alloys.
[0108] Test Example 5: Cell compatibility test of the Mn alloy wire of Example 2.
[0109] According to ISO10993-5:2009 standard, the cell compatibility test of the Mn alloy wire prepared in Example 2 was carried out by indirect extraction method. L929 cells were cultured in MEM medium supplemented with 10% fetal bovine serum and 1% (v / v) penicillin / streptomycin in an environment of 5% CO 2, 95% humidity and 37°C. The culture medium was changed every 2 to 3 days. When the cells reached 90% confluence, the cells were exposed to 0.25% trypsin containing 1mM EDTA solution for 3-5min for passage. After cleaning and sterilization, the Mn alloy wire was incubated in MEM medium supplemented with 10% fetal bovine serum and 1% (v / v) penicillin / streptomycin for 24h to prepare the leaching solution. The ratio of the leaching solution volume to the wire surface area was 1.25ml / cm 2 .
[0110] After culturing L-929 cells in the extract medium for 24, 48, and 72 hours, the cell viability was detected using live / dead cell imaging. The cells were first rinsed with 10% fetal bovine serum and then stained with Calcein AM / EthD-I solution. After staining, the cells were incubated in the dark at room temperature for 20 minutes and then photographed using a fluorescence microscope. The results are shown in Figure 2. Fig. 9 shown.
[0111] After quantifying the number of live and dead cells in the image, the cell viability was calculated using the following formula:
[0112] In the above formula, Cell AO Cell EB Indicates dead cells.
[0113] The survival rate of L929 cells after 24, 48 and 72 h of culture was as follows: Figure 9-10 As shown, the cell density is Fig.10 As shown in the left figure, the cell survival rate is Fig.10 As shown in the right figure. Figure 9-10 It can be seen that the cell density after culturing for 4, 24 and 72 hours is 28%, 49% and 90%, and the cell survival rate is 99.2%, 99.1% and 96.5%. This shows that the cell compatibility of the Mn-36Fe-3.5Cu-0.5C alloy wire prepared by the present invention is good, and L-929 cells grow well within the 72-hour culture time, and the cell number continues to increase.
[0114] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.
Claims
1. A biomedical Mn alloy, characterized in that: The composition is calculated by mass fraction, and consists of 60-75wt% of Mn, 22-37wt.% of Fe, 2.75-4.25wt.% of Cu, and 0.25-0.75wt.% of C. The microstructure of the biomedical Mn alloy rod contains only equiaxed crystals, and the size of the equiaxed crystals is 12-25μm. In the microstructure of the biomedical Mn alloy wire, the number of deformed crystals and equiaxed crystals is (0.5-1.5):1, and the size of the equiaxed crystals is 0.15-0.65 μm; or, the microstructure of the biomedical Mn alloy wire contains only equiaxed crystals, and the size of the equiaxed crystals is 2.2-2.8 μm.
2. The biomedical Mn alloy according to claim 1, characterized in that: Its composition, measured by mass fraction, consists of 60wt.%, 35-37wt.%, 2.75-4.25wt.%, and 0.25-0.75wt.% of Mn; or, consists of 75wt.%, 20-22wt.%, 2.75-4.25wt.%, and 0.25-0.75wt.% of Mn.
3. The biomedical Mn alloy according to claim 2, characterized in that: Composed of Mn 60wt.%, Fe 36wt.%, Cu 3.5wt.%, and C 0.5wt.%.
4. The biomedical Mn alloy according to claim 2, characterized in that: Composed of Mn 75wt.%, Fe 21wt.%, Cu 3.5wt.%, and C 0.5wt.%.
5. The method for preparing a biomedical Mn alloy according to any one of claims 1 to 4, characterized in that: The following steps are involved: Pure Mn, Fe, Cu and C particles are mixed evenly and vacuum smelted to obtain cast alloy round bars; The cast alloy round rod is subjected to homogenization, turning, hot rolling, first annealing, rotary forging, second annealing, and grinding in sequence to obtain a rotary forging annealed Mn alloy rod; Alternatively, the rotary forging annealed Mn alloy rod is further subjected to a drawing process to obtain a drawn Mn alloy wire.
6. The method for preparing the biomedical Mn alloy according to claim 5, characterized in that: The drawn Mn alloy wire is subjected to an electric annealing treatment to obtain an electric annealed Mn alloy wire; the conditions for the electric annealing treatment are: annealing for 3-30 seconds at a current of 0.65-0.85A.
7. The method for preparing the biomedical Mn alloy according to claim 6, characterized in that: The conditions for the power annealing treatment were: annealing at a current of 0.7 A for 30 seconds.
8. The method for preparing a biomedical Mn alloy according to any one of claims 5 to 7, characterized in that: The total drawing deformation of the rotary forging annealed Mn alloy rod is 99.7-99.9%.
9. Use of the biomedical Mn alloy according to any one of claims 1 to 4 in the preparation of medical devices.
10. The use according to claim 9, characterized in that: The medical devices include, but are not limited to, sutures, implant stents, bone nails, bone pins, hemostatic clips, wire anchors, screws, bone plates, bone sleeves, intramedullary nails, staplers, orthodontic archwires, pacemaker wires, and venous filters.