Production process of anti-splashing anti-oxidation tungsten steel material
By employing high-pressure pressing, heat treatment, and surface treatment processes, combined with rare earth element oxidants and a protective atmosphere, the problem of oxidation of tungsten steel materials at high temperatures has been solved, improving its oxidation resistance and mechanical strength, making it suitable for high-temperature and high-stress environments.
Patent Information
- Application Number
- CN202411022144.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional tungsten steel materials are prone to oxidation at high temperatures, resulting in insufficient oxidation resistance, which affects mechanical strength and service life, limiting their application in harsh industrial environments.
It employs high-pressure pressing, complex heat treatment and surface treatment processes, combined with rare earth element oxides as antioxidants to form a dense structure and an antioxidant layer on the surface. Internal stress is eliminated through high-temperature sintering and forging, and argon or nitrogen protective atmosphere is used to prevent oxidation.
It significantly improves the oxidation resistance and mechanical strength of tungsten steel materials, extends their service life, and ensures high precision and surface quality, making them suitable for applications in harsh environments.
Smart Images

Figure CN118957377A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel material processing, in particular to a production process of splash-proof and oxidation-resistant tungsten steel material. Background Art
[0002] Tungsten steel materials are widely used in various industrial fields due to their excellent mechanical strength and hardness, especially in high temperature and high stress environments, where they have significant wear resistance and corrosion resistance. However, with the complexity of the application environment and the harshness of the use conditions, traditional tungsten steel materials are prone to oxidation at high temperatures, resulting in a decrease in material performance, affecting its service life and reliability. Therefore, the development of a tungsten steel material with anti-splash and anti-oxidation properties has become an important topic in the field of materials science and engineering technology.
[0003] At present, the production process of tungsten steel materials mainly includes raw material mixing, molding, sintering and subsequent heat treatment and mechanical processing. In order to improve the oxidation resistance of the material, antioxidants are usually added to the material, and the surface of the material is specially treated, such as electroplating and spraying. However, these processes have certain limitations in practical applications, such as uneven mixing, oxidation problems during sintering, and low machining accuracy, which affect the comprehensive performance of the final material.
[0004] In the prior art, tungsten steel materials are still prone to oxidation in high temperature environments, resulting in insufficient anti-oxidation performance, which affects the mechanical strength and service life of the material. This major technical problem limits the widespread application of tungsten steel materials in more demanding industrial application environments, and an improved production process is urgently needed to solve this problem. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a production process for anti-splash and anti-oxidation tungsten steel materials, which solves the problem that oxidation is still prone to occur in high-temperature environments, resulting in insufficient anti-oxidation performance and affecting the mechanical strength and service life of the material.
[0006] To achieve the above purpose, the present invention is implemented by the following technical scheme: a production process of anti-splash and anti-oxidation tungsten steel material, comprising the following steps:
[0007] S1. Raw material preparation: weigh 70%-90% tungsten powder, 10%-30% steel powder and 1%-5% rare earth element oxide antioxidant by weight percentage;
[0008] S2, pretreatment: heating the raw materials in an environment of 100°C-200°C for 2-4 hours, and continuously stirring to ensure uniform mixing;
[0009] S3, mixed molding: pressing and molding the pretreated raw materials to form a preliminary green body;
[0010] S4, sintering: placing the preliminary green body in a sintering furnace at 1200℃-1500℃ for 3-5 hours to form a dense tungsten steel material;
[0011] S5. Forging: The sintered tungsten steel material is forged at 50-100MPa at 800℃-1000℃ to improve its density and mechanical properties;
[0012] S6. Heat treatment: The forged material is quenched at 900℃-1100℃ and tempered at 500℃-700℃ to stabilize the internal structure of the material;
[0013] S7. Machining: Turning, milling and grinding the heat-treated materials to produce tungsten steel products of the required size and shape;
[0014] S8. Surface treatment: The manufactured tungsten steel products are electroplated and sprayed to form an anti-oxidation layer with a thickness of 5-20 microns.
[0015] Preferably, in the pretreatment step, a vacuum environment is used to reduce oxidation and mixing of impurities.
[0016] Preferably, in the pretreatment step, a vacuum environment is used to reduce oxidation and mixing of impurities.
[0017] Preferably, in the press-forming step, a hydraulic press with a pressure of 100-300 MPa is used for forming to ensure the density of the preliminary green body.
[0018] Preferably, in the sintering step, the atmosphere in the sintering furnace is an argon or nitrogen protective atmosphere to prevent the material from being oxidized at high temperature.
[0019] Preferably, in the forging step, the forged material undergoes multiple cooling and heating cycles to eliminate internal stress.
[0020] Preferably, in the heat treatment step, the quenching medium is oil or salt bath to ensure the quenching effect.
[0021] Preferably, in the mechanical processing step, a high-precision CNC machine tool is used for processing to achieve the required dimensional accuracy and surface finish.
[0022] Preferably, in the surface treatment step, the electroplating layer is a nickel-chromium alloy layer to provide excellent anti-oxidation performance.
[0023] Preferably, after the surface treatment, the tungsten steel product is ultrasonically cleaned to remove the treatment liquid and impurities remaining on the surface.
[0024] The present invention provides a production process for anti-splash and anti-oxidation tungsten steel materials. It has the following beneficial effects:
[0025] 1. The present invention uses compression molding and high-temperature sintering processes to form a dense structure of the preliminary green body under high pressure and high temperature, thereby enhancing the mechanical strength and hardness of the material, so that it can withstand higher mechanical stress and load.
[0026] 2. The present invention forms an antioxidant layer by adding rare earth element oxide antioxidants to the material and performing electroplating and spraying in the surface treatment step, thereby effectively improving the antioxidant performance of the material and extending its service life.
[0027] 3. The present invention effectively eliminates the internal stress of the material through multiple cooling and heating cycles in the forging and heat treatment steps, improves the stability and reliability of the material, and prevents deformation or cracking during use.
[0028] 4. The present invention adopts high-precision CNC machine tools for mechanical processing to ensure the dimensional accuracy and surface finish of tungsten steel products to meet high-demand application scenarios, and ensures the cleanliness and quality of the products through ultrasonic cleaning.
[0029] 5. The present invention adopts argon or nitrogen protective atmosphere in the sintering step to prevent the material from being oxidized at high temperature, maintain the purity and performance of the material, and further improve the material's antioxidant ability and service life.
[0030] In summary, this method significantly improves the density and strength of the material, enhances the oxidation resistance, reduces the internal stress, ensures high-precision processing and excellent surface quality, and effectively prevents high-temperature oxidation through a series of steps, including uniform mixing of raw materials, press molding, high-temperature sintering, forging treatment, heat treatment, precision machining and surface treatment. This process not only improves the overall performance and service life of the material, but also optimizes the manufacturing process and is suitable for large-scale industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Embodiment 1:
[0034] Please refer to the attached drawings *-attached drawings *, the embodiment of the present invention provides a production process of anti-splash and anti-oxidation tungsten steel material, including the following steps:
[0035] S1. Raw material preparation: weigh 70%-90% tungsten powder, 10%-30% steel powder and 1%-5% rare earth element oxide antioxidant by weight percentage. Tungsten powder provides high hardness and wear resistance, steel powder increases the toughness of the material, and rare earth element oxide acts as an antioxidant to prevent the material from oxidizing at high temperatures; ensuring the basic properties of the material while giving it antioxidant properties.
[0036] S2, pretreatment: heating the raw materials in an environment of 100°C-200°C for 2-4 hours, and continuously stirring to ensure uniform mixing. Preferably, a vacuum environment is used in the pretreatment step to reduce oxidation and the mixing of impurities;
[0037] S201, heating: placing the mixed raw materials in a heating furnace, and controlling the temperature between 100°C and 200°C.
[0038] S202, stirring: using a stirring device to continuously stir for 2-4 hours.
[0039] S203, vacuum treatment: heating and stirring in a vacuum environment to reduce oxidation and mixing of impurities.
[0040] Heating helps activate the raw materials, stirring ensures uniform mixing, and vacuum treatment reduces the risk of oxidation; the raw materials are fully mixed to reduce oxidation and ensure the smooth progress of subsequent steps.
[0041] S3, mixed molding: the pre-treated raw materials are pressed and molded to form a preliminary green body. Preferably, in the pressing and molding step, a hydraulic press with a pressure of 100-300 MPa is used for molding to ensure the density of the preliminary green body.
[0042] S301, feeding: feeding the pretreated raw materials into the mold.
[0043] S302, pressing: using a hydraulic press for pressing and forming, the pressure is controlled at 100-300 MPa.
[0044] High pressure pressing can make the powder particles tightly combined to form a dense preliminary green body, improve the density of the green body, and provide a good foundation for subsequent sintering.
[0045] S4, sintering: the preliminary green body is placed in a sintering furnace at 1200°C-1500°C for 3-5 hours to form a dense tungsten steel material. Preferably, the atmosphere in the sintering furnace during the sintering step is an argon or nitrogen protective atmosphere to prevent the material from oxidizing at high temperature.
[0046] S401, preheating: placing the preliminary green body in a sintering furnace and gradually preheating it.
[0047] S402, sintering: sintering at a temperature of 1200°C-1500°C for 3-5 hours.
[0048] S403, Protective atmosphere: During the sintering process, argon or nitrogen is introduced to prevent oxidation.
[0049] High temperature sintering causes diffusion and bonding between green body particles, forming a dense material, and protecting the atmosphere from oxidation. The material is densified, the internal structure is uniform, and the anti-oxidation performance is enhanced.
[0050] S5, forging: the sintered tungsten steel material is forged at 50-100 MPa in an environment of 800°C-1000°C to improve its density and mechanical properties. Preferably, in the forging step, the forged material undergoes multiple cooling and heating cycles to eliminate internal stress.
[0051] S501, heating: heating the sintered material to 800°C-1000°C.
[0052] S502, forging: applying a forging pressure of 50-100 MPa in a heated state.
[0053] S503, cooling cycle: the forged material undergoes multiple cooling and heating cycles.
[0054] The forging process improves the density and mechanical properties of the material through plastic deformation, and the cooling cycle eliminates internal stress. It improves the strength and toughness of the material, eliminates internal stress, and improves stability.
[0055] S6. Heat treatment: The forged material is quenched at 900°C-1100°C and tempered at 500°C-700°C to stabilize the internal structure of the material. Preferably, the quenching medium is oil or salt bath to ensure the quenching effect.
[0056] S601, Quenching: Heat the forged material to 900℃-1100℃, then cool it rapidly. The quenching medium is oil or salt bath.
[0057] S602, tempering: the quenched material is heated to 500℃-700℃, kept for a certain period of time and then slowly cooled.
[0058] Quenching causes a sharp change in the molecular structure of the material, improving hardness and strength, while tempering eliminates quenching stress and improves toughness. The material has stable properties and has both high hardness and toughness.
[0059] S7, machining: turning, milling and grinding the heat-treated material to produce a tungsten steel product of the required size and shape. Preferably, the machining step uses a high-precision CNC machine tool to achieve the required dimensional accuracy and surface finish.
[0060] S701, Turning: Preliminary cutting of material to near required size.
[0061] S702, Milling: Fine processing of material surface to achieve precise dimensions.
[0062] S703, Grinding: Final polishing and finishing of the material surface.
[0063] Multi-step machining ensures precise control of material shape and size with high surface finish. Products have high dimensional accuracy and excellent surface quality to meet demanding applications.
[0064] S8, surface treatment: electroplating and spraying treatment are performed on the manufactured tungsten steel products to form an anti-oxidation layer with a thickness of 5-20 microns. Preferably, the electroplating layer is a nickel-chromium alloy layer to provide excellent anti-oxidation performance. After the surface treatment, the tungsten steel products are ultrasonically cleaned to remove the residual treatment liquid and impurities on the surface.
[0065] S801, electroplating: nickel-chromium alloy electroplating is performed on the surface of tungsten steel products, and the thickness is controlled at 5-20 microns.
[0066] S802, Spraying: Perform protective spraying on the electroplating layer to increase surface protection.
[0067] S803, Ultrasonic cleaning: clean the residual treatment liquid and impurities on the surface.
[0068] Electroplating and spraying form multiple layers of protection, and ultrasonic cleaning ensures a clean surface. The material surface has excellent anti-oxidation properties, the surface is clean and free of impurities, and the service life is extended.
[0069] Embodiment 2:
[0070] The second embodiment discloses a production process of a splash-proof and oxidation-resistant tungsten steel material, which specifically includes the following steps:
[0071] S1. Raw material preparation: weigh 70%-90% tungsten powder, 10%-30% steel powder and 1%-5% rare earth element oxide antioxidant by weight percentage. Tungsten powder provides high hardness and wear resistance, steel powder increases the toughness of the material, and rare earth element oxide acts as an antioxidant to prevent the material from oxidizing at high temperatures; ensuring the basic properties of the material while giving it antioxidant properties.
[0072] S2, pretreatment: heating the raw materials in an environment of 100°C-200°C for 2-4 hours, and continuously stirring to ensure uniform mixing. Preferably, a vacuum environment is used in the pretreatment step to reduce oxidation and the mixing of impurities;
[0073] S201, heating: placing the mixed raw materials in a heating furnace, and controlling the temperature between 100°C and 200°C.
[0074] S202, stirring: using a stirring device to continuously stir for 2-4 hours.
[0075] S203, vacuum treatment: heating and stirring in a vacuum environment to reduce oxidation and mixing of impurities.
[0076] Heating helps activate the raw materials, stirring ensures uniform mixing, and vacuum treatment reduces the risk of oxidation; the raw materials are fully mixed to reduce oxidation and ensure the smooth progress of subsequent steps.
[0077] S3, mixed molding: the pre-treated raw materials are pressed and molded to form a preliminary green body. In this embodiment, a hydraulic press with a pressure of 50-100 MPa is used in the pressing and molding step to ensure the density of the preliminary green body.
[0078] S301, feeding: feeding the pretreated raw materials into the mold.
[0079] S302, pressing: using a hydraulic press for pressing and forming, the pressure is controlled at 50-100 MPa.
[0080] High pressure pressing can make the powder particles tightly combined to form a dense preliminary green body, improve the density of the green body, and provide a good foundation for subsequent sintering.
[0081] S4, sintering: the preliminary green body is placed in a sintering furnace at 1200°C-1500°C for 3-5 hours to form a dense tungsten steel material. Preferably, the atmosphere in the sintering furnace during the sintering step is an argon or nitrogen protective atmosphere to prevent the material from oxidizing at high temperature.
[0082] S401, preheating: placing the preliminary green body in a sintering furnace and gradually preheating it.
[0083] S402, sintering: sintering at a temperature of 1200°C-1500°C for 3-5 hours.
[0084] S403, Protective atmosphere: During the sintering process, argon or nitrogen is introduced to prevent oxidation.
[0085] High temperature sintering causes diffusion and bonding between green body particles, forming a dense material, and protecting the atmosphere from oxidation. The material is densified, the internal structure is uniform, and the anti-oxidation performance is enhanced.
[0086] S5, forging: the sintered tungsten steel material is forged at 50-100 MPa in an environment of 800°C-1000°C to improve its density and mechanical properties. Preferably, in the forging step, the forged material undergoes multiple cooling and heating cycles to eliminate internal stress.
[0087] S501, heating: heating the sintered material to 800°C-1000°C.
[0088] S502, forging: applying a forging pressure of 50-100 MPa in a heated state.
[0089] S503, cooling cycle: the forged material undergoes multiple cooling and heating cycles.
[0090] The forging process improves the density and mechanical properties of the material through plastic deformation, and the cooling cycle eliminates internal stress. It improves the strength and toughness of the material, eliminates internal stress, and improves stability.
[0091] S6. Heat treatment: The forged material is quenched at 900°C-1100°C and tempered at 500°C-700°C to stabilize the internal structure of the material. Preferably, the quenching medium is oil or salt bath to ensure the quenching effect.
[0092] S601, Quenching: Heat the forged material to 900℃-1100℃, then cool it rapidly. The quenching medium is oil or salt bath.
[0093] S602, tempering: the quenched material is heated to 500℃-700℃, kept for a certain period of time and then slowly cooled.
[0094] Quenching causes a sharp change in the molecular structure of the material, improving hardness and strength, while tempering eliminates quenching stress and improves toughness. The material has stable properties and has both high hardness and toughness.
[0095] S7, machining: turning, milling and grinding the heat-treated material to produce a tungsten steel product of the required size and shape. Preferably, the machining step uses a high-precision CNC machine tool to achieve the required dimensional accuracy and surface finish.
[0096] S701, Turning: Preliminary cutting of material to near required size.
[0097] S702, Milling: Fine processing of material surface to achieve precise dimensions.
[0098] S703, Grinding: Final polishing and finishing of the material surface.
[0099] Multi-step machining ensures precise control of material shape and size with high surface finish. Products have high dimensional accuracy and excellent surface quality to meet demanding applications.
[0100] S8, surface treatment: electroplating and spraying treatment are performed on the manufactured tungsten steel products to form an anti-oxidation layer with a thickness of 5-20 microns. Preferably, the electroplating layer is a nickel-chromium alloy layer to provide excellent anti-oxidation performance. After the surface treatment, the tungsten steel products are ultrasonically cleaned to remove the residual treatment liquid and impurities on the surface.
[0101] S801, electroplating: nickel-chromium alloy electroplating is performed on the surface of tungsten steel products, and the thickness is controlled at 5-20 microns.
[0102] S802, Spraying: Perform protective spraying on the electroplating layer to increase surface protection.
[0103] S803, Ultrasonic cleaning: clean the residual treatment liquid and impurities on the surface.
[0104] Electroplating and spraying form multiple layers of protection, and ultrasonic cleaning ensures a clean surface. The material surface has excellent anti-oxidation properties, the surface is clean and free of impurities, and the service life is extended.
[0105] Compared with Example 1, the only variable is the pressure used in the compression molding step. In this embodiment, a hydraulic press with a pressure of 50-100 MPa is used for molding, and the remaining steps and parameters are the same as in Example 1.
[0106] Embodiment three:
[0107] The third embodiment discloses a production process of a splash-proof and oxidation-resistant tungsten steel material, which specifically includes the following steps:
[0108] S1. Raw material preparation: weigh 70%-90% tungsten powder, 10%-30% steel powder and 1%-5% rare earth element oxide antioxidant by weight percentage. Tungsten powder provides high hardness and wear resistance, steel powder increases the toughness of the material, and rare earth element oxide acts as an antioxidant to prevent the material from oxidizing at high temperatures; ensuring the basic properties of the material while giving it antioxidant properties.
[0109] S2, pretreatment: heating the raw materials in an environment of 100°C-200°C for 2-4 hours, and continuously stirring to ensure uniform mixing. Preferably, a vacuum environment is used in the pretreatment step to reduce oxidation and the mixing of impurities;
[0110] S201, heating: placing the mixed raw materials in a heating furnace, and controlling the temperature between 100°C and 200°C.
[0111] S202, stirring: using a stirring device to continuously stir for 2-4 hours.
[0112] S203, vacuum treatment: heating and stirring in a vacuum environment to reduce oxidation and mixing of impurities.
[0113] Heating helps activate the raw materials, stirring ensures uniform mixing, and vacuum treatment reduces the risk of oxidation; the raw materials are fully mixed to reduce oxidation and ensure the smooth progress of subsequent steps.
[0114] S3, mixed molding: the pre-treated raw materials are pressed and molded to form a preliminary green body. Preferably, in the pressing and molding step, a hydraulic press with a pressure of 100-300 MPa is used for molding to ensure the density of the preliminary green body.
[0115] S301, feeding: feeding the pretreated raw materials into the mold.
[0116] S302, pressing: using a hydraulic press for pressing and forming, the pressure is controlled at 100-300 MPa.
[0117] High pressure pressing can make the powder particles tightly combined to form a dense preliminary green body, improve the density of the green body, and provide a good foundation for subsequent sintering.
[0118] S4, sintering: the preliminary green body is placed in a sintering furnace at 1100°C-1300°C for 3-5 hours to form a dense tungsten steel material. Preferably, the atmosphere in the sintering furnace during the sintering step is an argon or nitrogen protective atmosphere to prevent the material from oxidizing at high temperature.
[0119] S401, preheating: placing the preliminary green body in a sintering furnace and gradually preheating it.
[0120] S402, sintering: sintering at a temperature of 1100°C-1300°C for 3-5 hours.
[0121] S403, Protective atmosphere: During the sintering process, argon or nitrogen is introduced to prevent oxidation.
[0122] High temperature sintering causes diffusion and bonding between green body particles, forming a dense material, and protecting the atmosphere from oxidation. The material is densified, the internal structure is uniform, and the anti-oxidation performance is enhanced.
[0123] S5, forging: the sintered tungsten steel material is forged at 50-100 MPa in an environment of 800°C-1000°C to improve its density and mechanical properties. Preferably, in the forging step, the forged material undergoes multiple cooling and heating cycles to eliminate internal stress.
[0124] S501, heating: heating the sintered material to 800°C-1000°C.
[0125] S502, forging: applying a forging pressure of 50-100 MPa in a heated state.
[0126] S503, cooling cycle: the forged material undergoes multiple cooling and heating cycles.
[0127] The forging process improves the density and mechanical properties of the material through plastic deformation, and the cooling cycle eliminates internal stress. It improves the strength and toughness of the material, eliminates internal stress, and improves stability.
[0128] S6. Heat treatment: The forged material is quenched at 900°C-1100°C and tempered at 500°C-700°C to stabilize the internal structure of the material. Preferably, the quenching medium is oil or salt bath to ensure the quenching effect.
[0129] S601, Quenching: Heat the forged material to 900℃-1100℃, then cool it rapidly. The quenching medium is oil or salt bath.
[0130] S602, tempering: the quenched material is heated to 500℃-700℃, kept for a certain period of time and then slowly cooled.
[0131] Quenching causes a sharp change in the molecular structure of the material, improving hardness and strength, while tempering eliminates quenching stress and improves toughness. The material has stable properties and has both high hardness and toughness.
[0132] S7, machining: turning, milling and grinding the heat-treated material to produce a tungsten steel product of the required size and shape. Preferably, the machining step uses a high-precision CNC machine tool to achieve the required dimensional accuracy and surface finish.
[0133] S701, Turning: Preliminary cutting of material to near required size.
[0134] S702, Milling: Fine processing of material surface to achieve precise dimensions.
[0135] S703, Grinding: Final polishing and finishing of the material surface.
[0136] Multi-step machining ensures precise control of material shape and size with high surface finish. Products have high dimensional accuracy and excellent surface quality to meet demanding applications.
[0137] S8, surface treatment: electroplating and spraying treatment are performed on the manufactured tungsten steel products to form an anti-oxidation layer with a thickness of 5-20 microns. Preferably, the electroplating layer is a nickel-chromium alloy layer to provide excellent anti-oxidation performance. After the surface treatment, the tungsten steel products are ultrasonically cleaned to remove the residual treatment liquid and impurities on the surface.
[0138] S801, electroplating: nickel-chromium alloy electroplating is performed on the surface of tungsten steel products, and the thickness is controlled at 5-20 microns.
[0139] S802, Spraying: Perform protective spraying on the electroplating layer to increase surface protection.
[0140] S803, Ultrasonic cleaning: clean the residual treatment liquid and impurities on the surface.
[0141] Electroplating and spraying form multiple layers of protection, and ultrasonic cleaning ensures a clean surface. The material surface has excellent anti-oxidation properties, the surface is clean and free of impurities, and the service life is extended.
[0142] Compared with Example 1, the only variable is the sintering temperature in the sintering step. In this example, the preliminary green body is placed in a sintering furnace at 1100° C.-1300° C. for sintering, and the remaining steps and parameters are the same as in Example 1.
[0143] Table 1 Comparison table of experimental data of embodiment
[0144]
[0145] In summary, Example 1 has the best performance in terms of density, hardness, oxidation resistance, tensile strength, fracture toughness and wear resistance due to the use of a higher pressing pressure (100-300 MPa) and a higher sintering temperature (1200-1500° C.).
[0146] Since Example 2 uses a lower pressing pressure (50-100 MPa), all performance indicators are lower than those of Example 1, indicating that the lower pressing pressure leads to insufficient densification of the material, affecting the final performance.
[0147] The pressing pressure of Example 3 is the same as that of Example 1, but the sintering temperature is lower (1100-1300° C.), so the performance is between Example 1 and Example 2, which shows that appropriately increasing the sintering temperature is helpful to improve the material performance.
[0148] Comparative Example 1:
[0149] This comparative example discloses a traditional production process of anti-splash and anti-oxidation tungsten steel material, comprising the following steps:
[0150] S1. Raw material preparation: weigh 80% tungsten powder and 20% steel powder by weight without adding antioxidant.
[0151] Tungsten powder provides high hardness and wear resistance, and steel powder increases the toughness of the material. They ensure the basic properties of the material, but lack anti-oxidation properties.
[0152] S2, pretreatment: placing the raw materials in a room temperature environment for dry mixing without heating and vacuum treatment.
[0153] S201, dry mixing: mechanically stir the raw materials at room temperature for 1-2 hours.
[0154] The raw materials are mixed by mechanical stirring, but no heating and vacuum treatment is applied. The mixing uniformity is poor and it is easy to oxidize.
[0155] S3, mixed molding: the pre-treated raw materials are pressed and molded to form a preliminary green body. In the pressing and molding step, a hydraulic press with a pressure of 50 MPa is used for molding.
[0156] S301, feeding: feeding the pretreated raw materials into the mold.
[0157] S302, pressing: using a hydraulic press for pressing and forming, the pressure is 50MPa.
[0158] Low-pressure pressing makes the powder particles not tightly combined. The green body has low density, providing a poor foundation for subsequent sintering.
[0159] S4. Sintering: Place the preliminary green body in a sintering furnace at 1000° C. and sinter for 2 hours without a protective atmosphere.
[0160] S401, preheating: placing the preliminary green body in a sintering furnace and gradually preheating it.
[0161] S402, sintering: sintering at a temperature of 1000°C for 2 hours.
[0162] Low temperature sintering results in insufficient bonding between green body particles, and the lack of protective atmosphere leads to oxidation. The material has a low degree of densification and poor oxidation resistance.
[0163] S5. Forging: The sintered tungsten steel material is forged at 50MPa at 800°C.
[0164] S501, heating: heating the sintered material to 800°C.
[0165] S502, forging: applying a forging pressure of 50 MPa in a heated state.
[0166] The forging process improves the mechanical properties of the material through plastic deformation. The density and mechanical properties are improved, but not as good as high-pressure forging.
[0167] S6. Heat treatment: The forged material is quenched at 800°C and tempered at 400°C.
[0168] S601, quenching: heat the forged material to 800℃ and then cool it rapidly.
[0169] S602, tempering: the quenched material is heated to 400°C, kept for a certain period of time and then slowly cooled.
[0170] Quenching and tempering improves material properties, but at lower temperatures. Material properties are improved, but hardness and toughness are lower.
[0171] S7. Machining: Perform simple turning and grinding on the heat-treated materials.
[0172] S701, Turning: Preliminary cutting of material to near required size.
[0173] S702, Grinding: Simple polishing of the material surface.
[0174] Simplified machining, low precision. Product dimensional accuracy and surface quality are poor.
[0175] S8. Surface treatment: The manufactured tungsten steel products are simply sprayed without electroplating and ultrasonic cleaning.
[0176] S801, Spraying: Simply spray on the surface of tungsten steel products.
[0177] Simple spraying increases surface protection, but no electroplating layer. Poor anti-oxidation performance and low surface cleanliness.
[0178] Comparative Example 1 Embodiment 1 Pressing pressure (MPa) 50 100-300 Sintering temperature(℃) 1000 1200-1500 <![CDATA[Material density (g / cm 3 )]]> 15.5 17.5 Hardness (HRC) 80 92 Antioxidant performance (%) 70 95 Tensile strength(MPa) 1400 1800 Fracture toughness (MPa·m^0.5) 9.0 12.5 Wear resistance (mg / 1000 revolutions) 15.0 10.5
[0179] Example 1 uses high-pressure pressing, high-temperature sintering and complex heat treatment and surface treatment processes, so that the tungsten steel material is significantly superior to the materials prepared by traditional processes in terms of density, hardness, oxidation resistance, tensile strength, fracture toughness and wear resistance.
[0180] The traditional process lacks antioxidant addition, has simple pretreatment steps, low pressing pressure, low sintering temperature, and simple heat treatment and machining processes, resulting in the final material performance being far inferior to that of Example 1.
[0181] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for anti-splash and anti-oxidation tungsten steel material, characterized in that: The following steps are involved: S1. Raw material preparation: weigh 70%-90% tungsten powder, 10%-30% steel powder and 1%-5% rare earth element oxide antioxidant by weight percentage; S2, pretreatment: heating the raw materials in an environment of 100°C-200°C for 2-4 hours, and continuously stirring to ensure uniform mixing; S3, mixed molding: pressing and molding the pretreated raw materials to form a preliminary green body; S4, sintering: placing the preliminary green body in a sintering furnace at 1200℃-1500℃ for 3-5 hours to form a dense tungsten steel material; S5. Forging: The sintered tungsten steel material is forged at 50-100MPa at 800℃-1000℃ to improve its density and mechanical properties; S6. Heat treatment: The forged material is quenched at 900℃-1100℃ and tempered at 500℃-700℃ to stabilize the internal structure of the material; S7. Machining: Turning, milling and grinding the heat-treated materials to produce tungsten steel products of the required size and shape; S8. Surface treatment: The manufactured tungsten steel products are electroplated and sprayed to form an anti-oxidation layer with a thickness of 5-20 microns.
2. The production process of anti-splash and anti-oxidation tungsten steel material according to claim 1 is characterized in that: In the pretreatment step, a vacuum environment is used to reduce oxidation and the mixing of impurities.
3. The production process of a splash-proof and oxidation-resistant tungsten steel material according to claim 1 is characterized in that: In the pretreatment step, a vacuum environment is used to reduce oxidation and the mixing of impurities.
4. The production process of anti-splash and anti-oxidation tungsten steel material according to claim 1 is characterized in that: In the compression molding step, a hydraulic press with a pressure of 100-300 MPa is used for molding to ensure the density of the preliminary green body.
5. The production process of anti-splash and anti-oxidation tungsten steel material according to claim 1 is characterized in that: In the sintering step, the atmosphere in the sintering furnace is an argon or nitrogen protective atmosphere to prevent the material from being oxidized at high temperature.
6. The production process of a splash-proof and oxidation-resistant tungsten steel material according to claim 1 is characterized in that: In the forging step, the forged material undergoes multiple cooling and heating cycles to eliminate internal stress.
7. The production process of anti-splash and anti-oxidation tungsten steel material according to claim 1 is characterized in that: In the heat treatment step, the quenching medium is oil or salt bath to ensure the quenching effect.
8. The production process of anti-splash and anti-oxidation tungsten steel material according to claim 1 is characterized in that: In the mechanical processing step, a high-precision CNC machine tool is used for processing to achieve the required dimensional accuracy and surface finish.
9. The production process of anti-splash and anti-oxidation tungsten steel material according to claim 1 is characterized in that: In the surface treatment step, the electroplating layer is a nickel-chromium alloy layer to provide excellent anti-oxidation performance.
10. The production process of anti-splash and anti-oxidation tungsten steel material according to claim 1 is characterized in that: After surface treatment, the tungsten steel products are ultrasonically cleaned to remove residual treatment liquid and impurities on the surface.