Method for manufacturing hot-rolled H-shaped steel for V-containing low-temperature-resistant structure

In the manufacturing of hot-rolled H-shaped steel for low-temperature structures, converter smelting, LF refining and stylised continuous casting processes are used to reasonably design chemical components and process parameters, and the problem of insufficient low-temperature impact toughness in the existing technology is solved, achieving high The production of hot-rolled H-shaped steel of mass low-temperature structures has good mechanical properties and low-temperature impact toughness.

CN118957403AInactive Publication Date: 2024-11-15BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410872915.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to develop hot-rolled H-shaped steel for low-temperature structures with good low-temperature impact toughness in the prior art, and cannot meet the harsh environment needs in marine oil and gas resource development.

Method used

Converter smelting, LF refining and stylised continuous casting technology are adopted to reasonably design chemical components (C 0.07%-0.16%, Si 0.15%-0.50%, Mn 1.10%-1.60%, P ≤ 0.035%, S ≤ 0.035%, V 0.050%~0.10%), combined with weak-cold technology and protective casting, control the pulling speed, superheat and crystallizer water volume, avoid crack-sensitive areas, and improve the temperature uniformity of continuous casting billets.

Benefits of technology

The produced hot-rolled H-shaped steel for low-temperature resistant structures has good mechanical properties and low-temperature impact toughness, excellent surface and internal quality, and all performances after rolling meet the standard requirements, and the surface crack rate is less than 2%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004922147340000041
    Figure BDA0004922147340000041
  • Figure BDA0004922147340000051
    Figure BDA0004922147340000051
  • Figure BDA0004922147340000052
    Figure BDA0004922147340000052
Patent Text Reader

Abstract

The invention discloses a method for manufacturing hot-rolled H-shaped steel for a V-containing low-temperature-resistant structure. The hot-rolled H-shaped steel comprises the following chemical components in percentage by mass: 0.07%-0.16% of C, 0.15%-0.50% of Si, 1.10%-1.60% of Mn, less than or equal to 0.035% of P, less than or equal to 0.035% of S, 0.050%-0.10% of V and the balance of Fe and inevitable impurities, and the total mass fraction is 100%. The manufacturing process comprises the steps of converter smelting, LF refining, beam blank continuous casting and casting blank stacking and slow cooling, wherein the heating temperature of a steel blank is 1080-1120 DEG C; the initial rolling temperature is 1030-1050 DEG C, and the final rolling temperature is 940 DEG C. The invention aims to provide the method for manufacturing the hot-rolled H-shaped steel for the V-containing low-temperature-resistant structure, and the hot-rolled H-shaped steel has good mechanical properties, especially good low-temperature impact toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of smelting and continuous casting, and in particular relates to a method for manufacturing V-containing hot-rolled H-shaped steel for low-temperature resistant structures. Background Art

[0002] In recent years, with the continuous development of marine oil and gas resources, the market demand for hot-rolled H-shaped steel for low-temperature structures has been increasing. The research and development of high-strength and high-toughness H-shaped steel for low-temperature structures has far-reaching significance for making full use of my country's marine resources and realizing the country's energy strategy. Hot-rolled H-shaped steel for low-temperature structures is often used in working environments with very harsh environmental conditions. In addition to gravity loads, wind loads, wave loads, river loads, ice loads, earthquake loads, etc. must also be considered. Therefore, the development of hot-rolled H-shaped steel for low-temperature resistant structures has a very bright prospect. Summary of the invention

[0003] The object of the present invention is to provide a method for manufacturing hot-rolled H-shaped steel containing V for low-temperature resistant structure, which has good mechanical properties, especially good low-temperature impact toughness.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention discloses a method for manufacturing hot-rolled H-shaped steel containing V for low-temperature resistant structure. The mass percentage of chemical components of the hot-rolled H-shaped steel includes: C 0.07%-0.16%, Si 0.15%-0.50%, Mn 1.10%-1.60%, P≤0.035%, S≤0.035%, V 0.050%-0.10%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%. The manufacturing process includes: converter smelting, LF refining, special-shaped billet continuous casting, billet stacking slow cooling: wherein:

[0006] Combined blowing converter smelting, the final slag basicity is controlled at 3.0, the end point control target C ≥ 0.03%, T ≥ 1640℃, SiMn and MnFe deoxidation alloying is used, the final deoxidation is Al deoxidation, lime is added during the steel tapping process, and slag is blocked during steel tapping;

[0007] Refining white slag operation, after lifting the electrode each time, dip the slag sample, add silicon calcium barium according to the slag color, add white ash according to the slag viscosity, and the final slag requires white slag. Blow Ar throughout the process, desulfurization, composition fine-tuning and temperature increase operations are performed according to the composition and temperature of the converter molten steel; add ferrovanadium in the later stage of refining, and ensure that V is 0.050%~0.10% after adding, and ensure that the soft blowing time is more than 15min;

[0008] The whole process adopts protective pouring, the overheating degree is ≤30℃, and the weak cooling system is adopted. Before entering the straightening machine, the target temperature of the billet web is ≥900℃, and the target temperature of the billet flange is ≥800℃. The constant pulling speed operation is adopted, and the pulling speed is controlled at 0.9m / min-1.0m / min. After the continuous casting billet is cut, it is promptly stacked and slowly cooled, and the slow cooling time is more than 48 hours;

[0009] The heating temperature of the steel billet is 1080-1120℃, the allowable temperature difference is ≤50℃, the total heating time is controlled at 2h, overheating, overburning and decarburization are prevented, the temperature is increased slowly to ensure uniform heating temperature of the steel billet and reduce temperature difference; the starting rolling temperature is 1030-1050℃, and the final rolling temperature is 940℃.

[0010] Furthermore, the cross-sectional dimensions of the continuous casting billet are H350mm×290mm×100mm.

[0011] Furthermore, the mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.10%, Si 0.25%, Mn 1.45%, P 0.015%, S 0.010%, V 0.060%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

[0012] Furthermore, the mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.09%, Si 0.22%, Mn 1.47%, P 0.014%, S 0.009%, V 0.063%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

[0013] Furthermore, the mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.10%, Si 0.23%, Mn 1.43%, P 0.013%, S 0.007%, V 0.067%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

[0014] Furthermore, the mass percentage of the chemical composition of the hot-rolled H-beam includes: C0.09%, Si0.28%, Mn1.46%, P0.015%, S0.008%, V0.061%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

[0015] Compared with the prior art, the beneficial technical effects of the present invention are:

[0016] The present invention adopts a weak cooling process during the continuous casting process through reasonable chemical composition design. According to the molten steel composition characteristics of the hot-rolled H-beam, the pulling speed, superheat, water volume of the crystallizer and the water inlet temperature are reasonably matched to improve the uniformity of the temperature of the continuous casting billet, control the temperature of the continuous casting billet, and avoid the crack sensitive area as much as possible during the straightening process. The accuracy of the equipment is improved, and the arc and centering of the crystallizer are adjusted to be less than or equal to 0.1mm. The surface and internal quality of the hot-rolled H-beam billet containing V for low-temperature resistant structure produced by this process are good, and the surface crack rate is less than 2%. The various properties of the H-beam after rolling meet the standard requirements, and it has good mechanical properties, especially good low-temperature impact toughness. DETAILED DESCRIPTION

[0017] The present invention is further described in detail below

[0018] A method for manufacturing V-containing hot-rolled H-shaped steel for low-temperature resistant structure, wherein the mass percentage of chemical components includes: C 0.07%-0.16%, Si 0.15%-0.50%, Mn 1.10%-1.60%, P≤0.035%, S≤0.035%, V 0.050%-0.10%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

[0019] The invention discloses a manufacturing process for hot-rolled H-shaped steel containing V for low-temperature resistant structure, comprising converter smelting, LF refining, continuous casting of special-shaped billets, and slow cooling of billet stacking.

[0020] In combined blowing converter smelting, the final slag basicity is controlled at 3.0, the endpoint control target C≥0.03%, T≥1640℃, SiMn and MnFe are used for deoxidation and alloying, and Al is used for final deoxidation. Lime is added during the steelmaking process to prevent slag during steelmaking.

[0021] Refining white slag operation, dip the slag sample after lifting the electrode each time, add silicon calcium barium according to the color of the slag, add white ash according to the viscosity of the slag, and the final slag requires white slag. Blow Ar operation is carried out throughout the process, desulfurization, composition fine-tuning and heating operation are carried out according to the composition and temperature of the converter molten steel. After desulfurization, S≤0.010%, the composition content is C0.08%~0.10%, Si0.20%~0.30%, Mn1.30%~1.50%, P≤0.020%, S≤0.010%, and the temperature after heating is T≥1560℃. Ferrovanadium is added in the later stage of refining, and V0.050%~0.10% is guaranteed after addition, and the soft blowing time is guaranteed to be more than 15min.

[0022] Protected pouring is adopted throughout the whole process, the superheat is ≤30℃, and the weak cooling system is adopted. Before entering the straightening machine, the target temperature of the billet web is ≥900℃, and the target temperature of the billet flange is ≥800℃. The constant pulling speed operation is adopted, and the pulling speed is controlled at 0.9m / min-1.0m / min. After the continuous casting billet is cut, it is promptly taken offline and stacked for slow cooling, and the slow cooling time is greater than 48 hours.

[0023] The cross-sectional dimensions of the continuous casting billet are H350mm×290mm×100mm.

[0024] The heating temperature of the steel billet is 1080-1120℃, the allowable temperature difference is ≤50℃, the total heating time is controlled at 2h, overheating, overburning and decarburization are prevented, the temperature is increased slowly to ensure uniform heating temperature of the steel billet and reduce temperature difference; the starting rolling temperature is 1030-1050℃, and the final rolling temperature is 940℃.

[0025] The surface quality of hot-rolled H-beam special-shaped continuous casting billets containing V for low-temperature resistant structures is inspected, and the internal quality is tested by low-power hot acid test and the quality of H-beam is tracked.

[0026] No obvious surface and internal quality defects of the ingot were found during the inspection process. The quality of the ingot was good, the surface crack rate of the ingot was less than 2%, and the various properties of the H-beam after rolling met the standard requirements. Table 1 shows the chemical composition of each steel grade, and Tables 2, 3, and 4 further illustrate the present invention in combination with the embodiments.

[0027] Table 1 Chemical composition of each example (mass percentage / %)

[0028]

[0029]

[0030] Table 2 Casting speed and superheat control of each example

[0031] Examples Superheat(℃) Pulling speed(m / min) Example 1 27 0.95 Example 2 28 0.97 Example 3 30 0.96 Example 4 29 0.98

[0032] Table 3 Surface temperature of the billet entering the straightening machine for each example

[0033] Examples Flange plate end(℃) R angle(℃) Web(℃) Example 1 888 984 926 Example 2 885 996 927 Example 3 886 993 924 Example 4 883 996 923

[0034] Table 4 Mechanical properties of H-beam after rolling in each example

[0035]

[0036] It can be seen from Table 4 that the H-beam not only has good yield and tensile strength, but also has good low-temperature impact toughness.

[0037] The embodiments described above are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for manufacturing hot-rolled H-shaped steel containing V for low-temperature resistant structure, characterized in that: The mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.07%-0.16%, Si 0.15%-0.50%, Mn 1.10%-1.60%, P≤0.035%, S≤0.035%, V 0.050%-0.10%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%; its manufacturing process includes: converter smelting, LF refining, special-shaped billet continuous casting, billet stacking slow cooling: wherein: Combined blowing converter smelting, the final slag basicity is controlled at 3.0, the end point control target C ≥ 0.03%, T ≥ 1640℃, SiMn and MnFe deoxidation alloying is used, the final deoxidation is Al deoxidation, lime is added during the steel tapping process, and slag is blocked during steel tapping; Refining white slag operation, after lifting the electrode each time, dip the slag sample, add silicon calcium barium according to the slag color, add white ash according to the slag viscosity, and the final slag requires white slag. Blow Ar throughout the process, desulfurization, composition fine-tuning and temperature increase operations are performed according to the composition and temperature of the converter molten steel; add ferrovanadium in the later stage of refining, and ensure that V is 0.050%~0.10% after adding, and ensure that the soft blowing time is more than 15min; The whole process adopts protective pouring, the overheating degree is ≤30℃, and the weak cooling system is adopted. Before entering the straightening machine, the target temperature of the billet web is ≥900℃, and the target temperature of the billet flange is ≥800℃. The constant pulling speed operation is adopted, and the pulling speed is controlled at 0.9m / min-1.0m / min. After the continuous casting billet is cut, it is promptly stacked and slowly cooled, and the slow cooling time is more than 48 hours; The heating temperature of the steel billet is 1080-1120℃, the allowable temperature difference is ≤50℃, the total heating time is controlled at 2h, overheating, overburning and decarburization are prevented, the temperature is increased slowly to ensure uniform heating temperature of the steel billet and reduce temperature difference; the starting rolling temperature is 1030-1050℃, and the final rolling temperature is 940℃.

2. The method for manufacturing V-containing low-temperature resistant structural hot-rolled H-beam according to claim 1, characterized in that: The cross-sectional dimensions of the continuous casting billet are H350mm×290mm×100mm.

3. The method for manufacturing V-containing low-temperature resistant structural hot-rolled H-beam according to claim 1, characterized in that: The mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.10%, Si 0.25%, Mn 1.45%, P 0.015%, S 0.010%, V 0.060%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

4. The method for manufacturing V-containing low-temperature resistant structural hot-rolled H-beam according to claim 1, characterized in that: The mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.09%, Si 0.22%, Mn 1.47%, P 0.014%, S0.009%, V 0.063%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

5. The method for manufacturing V-containing low-temperature resistant structural hot-rolled H-beam according to claim 1, characterized in that: The mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.10%, Si 0.23%, Mn 1.43%, P 0.013%, S 0.007%, V 0.067%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

6. The method for manufacturing V-containing low-temperature resistant structural hot-rolled H-beam according to claim 1, characterized in that: The mass percentage of the chemical composition of the hot-rolled H-beam includes: C 0.09%, Si 0.28%, Mn 1.46%, P 0.015%, S 0.008%, V 0.061%, and the rest is Fe and unavoidable impurities, with a total mass fraction of 100%.

Citation Information

Patent Citations

  • Hot-rolled H-steel for low temperature-resistance structure and preparation method for hot-rolled H-steel

    CN102618781A

  • Low-temperature toughness resistant H-shaped steel and production process thereof

    CN104018073A

  • Process for producing low-cost 355MPa hot-rolled H-shaped steel

    CN112517634A

  • Production method of rare earth alloy structural steel

    CN116590601A

  • Production method of hot-rolled H-shaped steel special-shaped continuous casting billet for low-alloy high-strength engineering structure

    CN116900264A