Production method of rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar
Through the reblowing converter smelting and LF refining technology, the addition of rare earth cerium alloys has solved the problem of high cost of atmospheric corrosion resistance, and the production of low-cost 400MPa corrosion-resistant steel bars has been realized, thus improving the corrosion resistance of the steel bars and Strength extends service life.
Patent Information
- Application Number
- CN202410935617.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The production cost of existing atmospheric corrosion-resistant steel bars is relatively high, making it difficult to achieve economical, low-cost corrosion-resistant steel bars, and the strength and service life of the steel bars are insufficient.
The rare earth cerium microalloy steel bars are produced by duplex converter smelting and low-pull carbon pulling process. The rare earth cerium alloy is added through LF refining to reduce the influence of non-metallic inclusions, and the pulling speed and rolling temperature are controlled to ensure the corrosion resistance and mechanics of the steel bars. performance.
It realizes a low-cost 400MPa corrosion-resistant steel bar, which has good corrosion resistance and mechanical properties, extends the service life of the steel bar and reduces production costs.
Smart Images

Figure BDA0004941234960000031 
Figure BDA0004941234960000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of smelting and rolling processes, and in particular relates to a production method of a rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar. Background Art
[0002] Atmospheric corrosion resistant steel is generally a low alloy steel with good atmospheric corrosion resistance, which is made by adding a certain amount of Cu, P or Ni, Mo, Nb, Ti, Cr and other alloying elements to steel. The mechanism of atmospheric corrosion resistant steel is mainly the process in which oxygen in the air undergoes an electrochemical reaction through the rust layer in the presence of a water film. The rust layer is composed of a loose outer rust layer and a dense inner rust layer. The alloying elements in the steel act mainly through the influence of the inner rust layer. Generally, a dense inner rust layer of Cu, P, and Cr can be observed in the corrosion products of atmospheric corrosion resistant steel.
[0003] The corrosion resistance of steel bars has become a major research topic in industrialized countries. The use scope of various corrosion-resistant steel bars and weather-resistant steel bars with long service life is expanding. However, for steel bars with ordinary corrosion resistance requirements, they require certain corrosion resistance, but are more concerned about whether their production costs are economical enough. In order to solve this problem, the present invention provides a low-cost and economical corrosion-resistant steel bar that is not suitable for expensive alloys such as V and Nb. Summary of the invention
[0004] The purpose of the present invention is to provide a method for producing a rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar, solve the corrosion problem of steel bars, achieve the upgrading of steel bars for concrete, and improve the strength and service life of steel bars.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] The present invention discloses a method for producing a rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar, and the production steps thereof mainly include:
[0007] The converter adopts double-blowing converter smelting, single slag operation, final slag basicity is controlled at 2.0, the converter adopts low carbon drawing process, converter endpoint control target C is not more than 0.06%, and the tapping temperature is controlled to be not less than 1630℃; ferromanganese and silicon manganese are used for refining, and aluminum deoxidation is used for final deoxidation; non-metallic inclusions in steel have a relatively large impact on the corrosion resistance of steel, and LF refining requires the addition of denaturants to the molten steel. In the production of this atmospheric corrosion-resistant steel bar, rare earth cerium alloy is added to denature and spheroidize non-metallic inclusions, eliminating or reducing their adverse effects on steel properties, thereby purifying steel quality, reducing the total amount of inclusions, and reducing corrosion between the contact surface of inclusions and steel matrix;
[0008] The drawing speed is controlled at 2.1-2.3 m / min. Due to the addition of alloy, the secondary cooling water of continuous casting adopts weak cooling to prevent surface cracks and internal defects of the casting billet, while ensuring constant drawing speed to obtain continuous casting billet.
[0009] The heating temperature of the casting billet is controlled at 1100-1200℃, the billet out-of-furnace temperature is 1050-1150℃, the starting rolling temperature is 950-1050℃, and the final rolling temperature is 850-900℃;
[0010] The chemical composition of the steel bar by mass percentage is: C: 0.20-0.25%, Si: 0.50-0.60%, Mn: 1.35-1.45%, Cr: 0.10-0.15%, the rare earth Ce is added in an amount of 30ppm, and the balance is Fe and inevitable impurity elements.
[0011] Furthermore, the chemical composition of the steel bar by mass percentage is: C: 0.24%, Si: 0.52%, Mn: 1.38%, Cr: 0.12%, rare earth Ce 15ppm, P 0.025%, S 0.034%, and the remainder is Fe and inevitable impurity elements.
[0012] Furthermore, the pulling speed is controlled at 2.2 m / min.
[0013] Furthermore, the cross-section of the ingot is 150 mm×150 mm, and the length of the ingot is 11.5 m.
[0014] Furthermore, the rolling temperature is 1050±20°C.
[0015] Compared with the prior art, the beneficial technical effects of the present invention are:
[0016] The rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar prepared by the present invention not only has good corrosion resistance, but also has good mechanical properties. DETAILED DESCRIPTION
[0017] The present invention will be further described below in conjunction with the embodiments.
[0018] The chemical composition of the rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar in this example is shown in Table 1. The main preparation process of the steel bar is: converter - LF refining - continuous casting - rolling.
[0019] Converter: top and bottom combined blowing is used for decarburization and dephosphorization. Steel is smelted at 1650°C until the carbon content in the molten steel is less than 0.05% and the phosphorus content is less than 0.01%, and then steel is tapped. During the tapping process, protective gas is used to stir the molten steel at a pressure of 0.5MPa. When the tapping is 1 / 4, ferrosilicon and silicon-manganese alloy are added for deoxidation, and carbon powder and slag-making materials are added to prevent large amounts of slag from falling during tapping. At the same time, the protective gas pressure gradually decreases with the amount of steel tapped.
[0020] Refining: LF refining is adopted, deoxidation is carried out until the oxygen content in the molten steel is 0.002%, and ferromanganese and silicon-manganese alloy are added. After the refining, calcium-iron alloy wire and rare earth-cerium alloy are fed, and the soft blowing time is ensured to be not less than 10 minutes.
[0021] Continuous casting: Try to ensure constant drawing speed for steel drawing, the drawing speed is controlled at 2.2m / min, the cross-section of the ingot is 150mm×150mm, and the ingot length is 11.5m.
[0022] Rolling: The specific rolling process is shown in Table 2. The continuous casting billet is heated to 1200℃, and the temperature is measured at about 1200℃ after being taken out of the furnace. After descaling with high-pressure water, rolling is carried out. The rolling temperature is 1050±20℃. After rough rolling and intermediate rolling, the final rolling temperature is controlled at 850~900℃, and then it is put on the cooling bed and enters the finishing and bundling process.
[0023] Table 1 Chemical composition of rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bars
[0024]
[0025]
[0026] Table 2 Rolling process of low-cost 400MPa corrosion-resistant steel bars made of rare earth cerium microalloy
[0027] Process solution Oven temperature / ℃ Rolling temperature / ℃ Finishing rolling temperature / ℃ Final rolling temperature / ℃ 1200±20 1050±20 1050±20 850~900
[0028] Table 3 Mechanical properties of rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bars
[0029] serial number <![CDATA[R p0.2 / MPa]]> <![CDATA[R m / MPa]]> A% Example 1 442 643 24.0 Example 2 445 646 28.0 Example 3 450 640 26.0 Example 4 448 647 25.0
[0030] It can be seen that the tensile strength of each embodiment of the present application is excellent, with an elongation of 24-28%, and a yield strength ratio of less than 0.72.
[0031] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for producing low-cost 400MPa corrosion-resistant steel bars made of rare earth cerium microalloy, characterized in that: The production steps mainly include: The converter adopts double-blowing converter smelting, single slag operation, final slag basicity is controlled at 2.0, the converter adopts low carbon drawing process, converter endpoint control target C is not more than 0.06%, and the tapping temperature is controlled to be not less than 1630℃; ferromanganese and silicon manganese are used for refining, and aluminum deoxidation is used for final deoxidation; non-metallic inclusions in steel have a relatively large impact on the corrosion resistance of steel, and LF refining requires the addition of denaturants to the molten steel. In the production of this atmospheric corrosion-resistant steel bar, rare earth cerium alloy is added to denature and spheroidize non-metallic inclusions, eliminating or reducing their adverse effects on steel properties, thereby purifying steel quality, reducing the total amount of inclusions, and reducing corrosion between the contact surface of inclusions and steel matrix; The drawing speed is controlled at 2.1-2.3 m / min. Due to the addition of alloy, the secondary cooling water of continuous casting adopts weak cooling to prevent surface cracks and internal defects of the casting billet, while ensuring constant drawing speed to obtain continuous casting billet. The heating temperature of the casting billet is controlled at 1100-1200℃, the billet out-of-furnace temperature is 1050-1150℃, the starting rolling temperature is 950-1050℃, and the final rolling temperature is 850-900℃; The chemical composition of the steel bar by mass percentage is: C: 0.20-0.25%, Si: 0.50-0.60%, Mn: 1.35-1.45%, Cr: 0.10-0.15%, the rare earth Ce is added in an amount of 30ppm, and the balance is Fe and inevitable impurity elements.
2. The method for producing a rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar according to claim 1, characterized in that: The chemical composition of the steel bar by mass percentage is: C: 0.24%, Si: 0.52%, Mn: 1.38%, Cr: 0.12%, rare earth Ce 15ppm, P 0.025%, S 0.034%, and the balance is Fe and inevitable impurity elements.
3. The method for producing a rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar according to claim 2, characterized in that: The pulling speed is controlled at 2.2m / min.
4. The method for producing a rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar according to claim 2, characterized in that: The cross section of the ingot is 150mm×150mm and the length of the ingot is 11.5m.
5. The method for producing a rare earth cerium microalloyed low-cost 400MPa corrosion-resistant steel bar according to claim 2, characterized in that: Rolling temperature 1050±20℃.
Citation Information
Patent Citations
Production method for fine grain steel bar
CN104831193A
500MPa-grade steel for engineering machinery, and manufacturing method thereof
CN108531816A
400 MPa-grade anti-seismic atmosphere-corrosion-resisting reinforcing steel bar and manufacturing method thereof
CN109023040A
High-strength threaded steel bar with good weldability and manufacturing method thereof
CN110079728A
HRB400E coiled steel bar subjected to rare earth and nitrogen microalloying treatment and production method of HRB400E coiled steel bar
CN114657460A