Medium-thickness low-cost low-yield-ratio ultrahigh-strength steel plate and preparation method thereof

By defining the alloy composition of Cr and Mn in medium-thick specification steel plates and conventional tempering and heat treatment processes, the problem of yield and strength ratio control is solved, and a low-cost production of 690MPa grade ultra-high strength steel plate has good performance stability and uniformity adapts to industrial production.

CN118957421APending Publication Date: 2024-11-15NORTH CHINA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411049621.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively produce medium-thickness 690MPa grade ultra-high strength steel plates that meet the requirements of low yield-strength ratio. Especially when the thickness of the steel plate increases, the yield-strength ratio is difficult to control, and the existing process costs are high or not suitable for industrial production.

Method used

By defining the alloy composition system of Cr and Mn, combined with conventional tempering and heat treatment, two-stage rolling and offline quenching and tempering treatment were used to prepare steel plates with a thickness of 60-200mm to form tempered sostenite structure to achieve yield strength ≥690MPa, tensile strength 770~910MPa, yield strength ratio ≤0.93.

Benefits of technology

It has achieved low-cost production of medium-thick specification steel plates, with good performance stability and full thickness performance uniformity, reduced production costs, and adapted to the existing steel plate industrial production route.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957421A_ABST
    Figure CN118957421A_ABST
Patent Text Reader

Abstract

The invention provides a medium-thickness-specification low-cost low-yield-ratio ultrahigh-strength steel plate and a preparation method thereof, and belongs to the technical field of low-alloy high-strength steel, the steel plate comprises the following chemical components in percentage by mass: 0.13%-0.18% of C, 0.10%-0.35% of Si, 1.20%-2.00% of Cr, 0.30%-0.60% of Mo, 0.02%-0.03% of Nb, 0.005%-0.02% of Ti, 0.02%-0.05% of V, 0.0005%-0.002% of B, less than or equal to 0.01% of P, less than or equal to 0.005% of S, and the balance of Fe and Mn. Wherein Cr and Mn conform to a certain relational expression, and a conventional quenching and tempering heat treatment process is matched, so that the ultrahigh-strength steel plate for the engineering structure, which has the thickness specification of 60-200mm, the yield strength of more than or equal to 690MPa, the tensile strength of 770-910MPa, the yield ratio of less than or equal to 0.93 and the transverse impact energy of more than or equal to 50J at the temperature of minus 40 DEG C, is produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of low-alloy high-strength steel, and in particular relates to a medium-thick specification, low-cost, low-yield ratio ultra-high-strength steel plate and a preparation method thereof. Background Art

[0002] In general, the higher the strength level of the steel plate, the higher the ratio of yield strength to tensile strength (yield ratio). The higher the yield ratio of the steel plate, the smaller the allowable margin of deformation and fracture of the manufactured structural parts, which will increase the safety risk of the engineering structure during service. Therefore, international classification societies such as Lloyd's Register of Shipping have put forward technical requirements that the yield ratio of steel plates with a yield strength of 690MPa cannot exceed 0.94. At the same time, industries such as construction engineering have also put forward yield ratio requirements for 690MPa steel plates. For steel plates with a yield strength of 690MPa, it is generally necessary to obtain a martensitic structure to ensure its high strength, so the yield ratio below 0.94 is a recognized technical problem for steel plates ≥690MPa. With the large-scale development of equipment such as marine engineering, the thickness of steel used has been further increased, and the demand for thick-gauge steel plates with low yield ratio performance has also increased.

[0003] Chinese patent CN116607076A discloses a thin-gauge low yield ratio 690MPa grade marine engineering steel and a manufacturing method. For steel plates with a thickness of ≤20mm, by controlling the lower rolling temperature and cooling temperature, the steel plate forms a matrix structure of not less than 60% martensite and not more than 40% bainite ferrite, and the yield ratio is reduced by the dual-phase matrix structure to obtain a high-strength steel plate with a yield strength of ≥690MPa and a yield ratio of ≤0.92. However, since the process uses online controlled rolling and sub-temperature online quenching, there is a large temperature gradient from the surface to the core of the steel plate during the rolling process, so it is easier to control for steel plates ≤20mm, but it is difficult to achieve when the thickness of the steel plate increases.

[0004] Chinese patent CN114231714A discloses a heat treatment method for 890MPa grade ultra-high strength and low yield ratio marine engineering steel. By controlling rolling and online cooling after rolling plus sub-temperature quenching plus tempering and water cooling, ultra-high strength and low yield ratio marine engineering steel plates with a thickness of 10-40mm and a yield ratio of ≤0.93 and a yield strength of ≥890MPa can be obtained. However, since this process is a sub-temperature quenching process and the temperature of the two-phase zone is limited to a narrow temperature range of 820-850℃, it has high requirements for the control of the chemical composition of the steel and requires water cooling after tempering, which is not suitable for existing industrial production equipment conditions.

[0005] Chinese patent CN114134414A discloses a low yield ratio high toughness steel and its preparation method. Through a two-stage rolling process, the obtained low yield ratio high toughness steel plate has a thickness of ≤80mm, a yield strength of ≥500MPa, a tensile strength of ≥640MPa, an elongation after fracture of ≥20.0%, a yield ratio of ≤0.80, and a -60℃ Charpy impact energy of >200J. This patent is aimed at steel for bridges and building structures with a strength level of 500MPa, and adopts a controlled rolling and controlled cooling process of low-temperature final rolling, which cannot meet the requirements of the ultra-high strength level of 690MPa.

[0006] Chinese patent CN114134416A discloses a medium-thick steel plate with low yield ratio and high strength and a short-process manufacturing method thereof. Through rolling and water cooling process development, a bainite structure with soft and hard substructure is formed, and no quenching and tempering heat treatment is required. After rolling, the steel plate is directly delivered by water cooling. The thickness of the steel plate is 15-60mm, the yield strength is 580-680MPa, the tensile strength is 700-820MPa, the elongation after fracture is 16-23%, the longitudinal Charpy impact absorption energy at a test temperature of -40℃ is 80-260J, and the yield ratio is ≤0.82. However, its manufacturing method is suitable for the production of steel with a yield strength of 580-680MPa.

[0007] Chinese patent CN114058793A discloses a heat treatment method for reducing the yield strength ratio of ultra-high strength marine steel eh890, which adopts the quenching + sub-temperature quenching + tempering quenching and tempering process, and can produce steel plates with thickness specifications of 15-50mm, yield strength ≥890MPa, tensile strength 940-1100MPa, yield strength ratio ≤0.94, V-shaped transverse -40℃ impact energy ≥50J. However, the patent adopts multiple heat treatment processes of quenching + sub-temperature quenching + tempering, which has a long production cycle and high process cost, and is also only suitable for the production of thin steel plates below 50mm.

[0008] Chinese patent CN114032459A discloses a method for preparing a medium-thick steel plate with a yield strength of 690MPa and high toughness and low yield strength ratio, which can be used to produce steel plates with a thickness of 10 to 50mm. However, the patent adopts a very complicated heat treatment process route, which requires the hot-rolled steel plate to be heated to 300 to 650℃ for pre-insulation, and then heated to the two-phase region for insulation before quenching, which cannot adapt to the industrial production equipment of medium-thick steel plates.

[0009] In summary, there is an urgent need to provide a medium-thick specification engineering structure steel suitable for producing low yield ratio requirements and a preparation method thereof. Summary of the invention

[0010] In order to solve the above technical problems, the present invention proposes a medium-thick specification, low-cost, low-yield-to-strength ratio ultra-high strength steel plate and a preparation method thereof. The prepared medium-thick specification steel plate for engineering structure has a thickness of 60 to 200 mm, a yield strength of not less than 690 MPa, and a ratio of yield strength to tensile strength of not higher than 0.93.

[0011] To achieve the above object, the present invention provides the following technical solutions:

[0012] One of the technical solutions of the present invention:

[0013] A medium-thick specification, low-cost, low-yield-to-strength ratio ultra-high strength steel plate, the thickness of the steel plate is X, 60mm≤X≤100mm, and the chemical composition of the steel plate, calculated by mass percentage, includes:

[0014] C 0.13%~0.18%, Si 0.10%~0.35%, Cr 1.20%~2.00%, Mo 0.30%~0.60%, Nb0.02%~0.03%, Ti 0.005%~0.02%, V 0.02%~0.05%, B 0.0005%~0.002%, P≤0.01%, S≤0.005%, the mass percentage of Mn conforms to the following relationship: Cr / Mn≥1.8, Cr%+Mn%≥1.8%; the balance is Fe.

[0015] The second technical solution of the present invention:

[0016] A medium-thick specification low-cost low-yield ratio ultra-high strength steel plate, the thickness of the steel plate is X, 100mm<X≤150mm, and the chemical composition of the steel plate includes, by mass percentage:

[0017] C 0.13%~0.18%, Si 0.10%~0.35%, Cr 1.20%~2.00%, Mo 0.30%~0.60%, Nb0.02%~0.03%, Ti 0.005%~0.02%, V 0.02%~0.05%, B 0.0005%~0.002%, P≤0.01%, S≤0.005%, the mass percentage of Mn conforms to the following relationship: Cr / Mn≥1.5, Cr%+Mn%≥2.2%; the balance is Fe.

[0018] The third technical solution of the present invention:

[0019] A medium-thick specification low-cost low-yield ratio ultra-high strength steel plate, the thickness of the steel plate is X, 150mm<X≤200mm, and the chemical composition of the steel plate includes, by mass percentage:

[0020] C 0.13%~0.18%, Si 0.10%~0.35%, Cr 1.20%~2.00%, Mo 0.30%~0.60%, Nb0.02%~0.03%, Ti 0.005%~0.02%, V 0.02%~0.05%, B 0.0005%~0.002%, P≤0.01%, S≤0.005%, the mass percentage of Mn conforms to the following relationship: Cr / Mn≥1.2, Cr%+Mn%≥2.4%; the balance is Fe.

[0021] The fourth technical solution of the present invention:

[0022] A method for preparing a medium-thickness, low-cost, low-yield ratio, ultra-high-strength steel plate comprises the following steps:

[0023] The chemical components of the steel plates in the above three technical solutions are smelted and cast to obtain steel billets;

[0024] The steel billet is sequentially heated, rolled, off-line quenched and tempered to obtain the steel plate.

[0025] Preferably, the parameters in the heating process are:

[0026] Heat the steel billet to 1150-1200℃, with the total heating time ≥1min / mm (i.e. the heating time is determined by the billet thickness. For example, if the billet thickness is 100mm, the total heating time is ≥100min, the same below);

[0027] Heating speed: when heating temperature is ≤600℃, heating speed is ≤90℃ / h;

[0028] When 600℃<heating temperature<900℃, 90℃ / h<heating speed≤100℃ / h;

[0029] When the heating temperature is 900℃≤ and the heating temperature is less than 1200℃, the heating rate is 100℃ / h<and less than 120℃ / h.

[0030] Preferably, the rolling process adopts two-stage rolling;

[0031] The first stage is the austenite recrystallization stage, with a rolling temperature of 980-1080°C;

[0032] The second stage is rolling in the non-crystallized zone, with a rolling temperature of 800-880°C;

[0033] The cumulative rolling reduction rate is ≥50%.

[0034] Preferably, the offline quenching process is specifically as follows: the quenching temperature is 900-940°C, and the holding time is 30-45min;

[0035] Quenching cooling rate ≥15℃ / s; Cool to room temperature;

[0036] The tempering temperature is 580~650℃, and the holding time is ≥2.5min / mm.

[0037] Furthermore, when 60mm≤X≤100mm, the quenching cooling rate is ≥20℃ / s.

[0038] Furthermore, when 100mm<X≤150mm, 17℃ / s≤quenching cooling rate<20℃ / s.

[0039] Furthermore, when 150 mm<X≤200 mm, 15°C / s≤quenching cooling rate<17°C / s.

[0040] Compared with the prior art, the present invention has the following advantages and technical effects:

[0041] (1) The present invention produces an ultra-high strength engineering structure steel plate with a thickness of 60 to 200 mm, a yield strength of ≥690 MPa, a tensile strength of 770 to 910 MPa, a yield strength ratio of ≤0.93, and a transverse impact energy of ≥50 J at -40°C by limiting the alloy component system in which Cr and Mn are added in proportion and cooperating with a conventional quenching and tempering heat treatment process.

[0042] (2) The present invention adopts a conventional quenching and tempering process that is more suitable for the existing industrial production route of steel plates. The metallographic structure is a tempered martensite structure, and there is no need to control the ferrite structure generated in the structure, which is different from the sub-temperature quenching process with greater difficulty in production process control. The steel plate produced by this process has good performance stability and full thickness performance uniformity, which is particularly prominent in the production process of medium and thick plates.

[0043] (3) The alloy composition system designed by the present invention does not require the addition of precious alloy Ni elements, which can greatly reduce the production cost. The engineering structure steel produced by the present invention has strong market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0045] Figure 1 The metallographic structure (tempered troostite structure) of the 110 mm thick steel plate prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0046] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0047] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0048] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0049] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0050] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0051] The invention discloses a medium-thickness steel plate with low yield ratio and ultra-high strength for engineering structure. The chemical composition of the steel plate is as follows by mass percentage: C 0.13%-0.18%, Si 0.10%-0.35%, Cr 1.20%-2.00%, Mo 0.30%-0.60%, Nb 0.02%-0.03%, Ti 0.005%-0.02%, V 0.02%-0.05%, B 0.0005%-0.002%, P≤0.01%, S≤0.005%, and the balance is Fe and Mn. The alloy Cr and Mn are preferably selected from the following schemes:

[0052] When the thickness of the steel plate is ≥60~100mm, Cr / Mn≥1.8, Cr%+Mn%≥1.8%;

[0053] When the thickness of the steel plate is >100-150mm, Cr / Mn≥1.5, Cr%+Mn%≥2.2%;

[0054] When the thickness of the steel plate is >150-200 mm, Cr / Mn≥1.2, Cr%+Mn%≥2.4%.

[0055] The present invention also discloses a method for preparing the medium-thickness, low-cost, low-yield-to-strength ratio, ultra-high-strength engineering structure steel plate, comprising the following steps:

[0056] 1) Smelting and casting: The production is carried out by converter or electric furnace smelting, refining outside the furnace, vacuum treatment and continuous casting or mold casting process. The thickness of the ingot is 200-1000mm. The ingot is stacked and slowly cooled after it comes off the line. The stacking time is ≥48h;

[0057] 2) Heating rolling process: heat the steel billet to 1150-1200°C, with a total heating time of ≥1min / mm; the heating rate is controlled as follows: in the range of ≤600°C, the heating rate is ≤90°C / h; in the range of >600-900°C, the heating rate is ≤100°C / h; in the range of ≥900-1200°C, the heating rate is ≤120°C / h;

[0058] A two-stage rolling process is adopted, the first stage is the austenite recrystallization stage, the rolling temperature is 980-1080℃; the second stage is the non-crystallization zone rolling, the rolling temperature is 800-880℃; the cumulative rolling reduction rate is ≥50%, after the rolling is completed, the water cooling is carried out, the water temperature is 800-840℃, and the final cooling temperature is ≤700℃;

[0059] 3) Finally, heat treatment is performed: offline quenching treatment is performed, the quenching temperature is 900-940°C, and the holding time is 30-45 minutes;

[0060] When the steel plate thickness is ≥60~100mm, the quenching cooling rate is ≥20℃ / s;

[0061] When the steel plate thickness is >100-150mm, the quenching cooling rate is ≥17℃ / s;

[0062] When the steel plate thickness is >150-200mm, the quenching cooling rate is ≥15℃ / s;

[0063] The tempering temperature is 580~650℃, and the holding time is ≥2.5min / mm.

[0064] In some preferred embodiments, the medium and thick low yield ratio ultra-high strength steel plate produced by the method has a yield strength ≥690MPa, a tensile strength of 770-910MPa, a yield ratio ≤0.93, an impact energy at -40°C ≥50J, and a metallographic structure of tempered bainite.

[0065] All raw materials used in the examples of the present invention are commercially available.

[0066] The technical solution of the present invention is further illustrated by the following embodiments.

[0067] Example 1

[0068] The steel plate of this embodiment has a thickness of 60 mm and is composed of the following chemical components in weight percentage: C 0.16%, Si 0.10%, Cr 1.80%, Mn 0.50%, Mo 0.30%, Nb 0.02%, Ti 0.005%, V 0.02%, B 0.0006%, P 0.008%, S 0.005%, and the balance is Fe and inevitable impurities.

[0069] 1) Smelting and continuous casting process: rough refining is carried out in a converter, followed by LF refining outside the furnace. After refining, vacuum degassing is carried out in a VD furnace, and the vacuum holding time is 15 minutes. Finally, continuous casting is carried out, and the thickness of the ingot is 300mm. After the ingot is off the line, it is stacked and slowly cooled, and the stacking time is 48 hours;

[0070] 2) Heating rolling process: heat the steel billet to 1150°C, with a total heating time of 710 min. In the range of ≤600°C, the heating rate is 90°C / h; in the range of >600-900°C, the heating rate is 98°C / h; in the range of ≥900-1150°C, the heating rate is 119°C / h;

[0071] The first stage is the austenite recrystallization stage, with a rolling temperature of 1050-1080°C;

[0072] The second stage is rolling in the non-crystallized zone, with a rolling temperature of 800-830°C; the cumulative reduction rate of the two rollings is 60%, the water entry temperature after rolling is 800°C, and the final cooling temperature is 650°C.

[0073] 3) Heat treatment process: offline quenching treatment, quenching temperature is 940℃, holding time is 30min, quenching cooling rate is 22℃ / s; tempering temperature is 650℃, holding time is 150min.

[0074] The mechanical properties of the steel plate prepared in this embodiment are as follows: yield strength 776 MPa, tensile strength 845 MPa, yield strength ratio 0.92, and average impact energy of 122 J at -40°C.

[0075] Example 2

[0076] The steel plate of this embodiment has a thickness of 110 mm and is composed of the following chemical components in weight percentage: C 0.18%, Si 0.35%, Cr 1.20%, Mn 0.80%, Mo 0.40%, Nb 0.03%, Ti 0.010%, V 0.03%, B 0.0009%, P 0.01%, S 0.003%, and the balance is Fe and inevitable impurities.

[0077] 1) Smelting and continuous casting process: rough refining is carried out in a converter, followed by LF refining outside the furnace. After refining, vacuum degassing is carried out in a VD furnace, and the vacuum holding time is 15 minutes. Finally, continuous casting is carried out, and the thickness of the ingot is 450mm. After the ingot is off the line, it is stacked and slowly cooled, and the stacking time is 50 hours;

[0078] 2) Heating rolling process: heat the steel billet to 1155°C, with a total heating time of 716 min; in the range of ≤600°C, the heating rate is 89°C / h; in the range of >600-900°C, the heating rate is 99°C / h; in the range of ≥900-1155°C, the heating rate is 118°C / h;

[0079] The first stage is the austenite recrystallization stage, with a rolling temperature of 980-1020°C; the second stage is the non-crystallization zone rolling, with a rolling temperature of 830-840°C; the cumulative rolling reduction rate is 77.8%, the water entry temperature after rolling is 820°C, and the final cooling temperature is 680°C.

[0080] 3) Heat treatment process: offline quenching treatment, quenching temperature is 930℃, holding time is 30min; quenching cooling rate is 20℃ / s; tempering temperature is 630℃, holding time is 250min.

[0081] The mechanical properties of the steel plate prepared in this embodiment are as follows: yield strength 746 MPa, tensile strength 823 MPa, yield strength ratio 0.91, and average impact energy value at -40°C 85 J.

[0082] Example 3

[0083] The steel plate of this embodiment has a thickness of 150 mm and is composed of the following chemical components in weight percentage: C 0.13%, Si 0.25%, Cr 2.00%, Mn 0.60%, Mo 0.60%, Nb 0.025%, Ti 0.017%, V 0.05%, B 0.0012%, P 0.005%, S 0.002%, and the balance is Fe and inevitable impurities.

[0084] 1) Smelting and continuous casting process: rough refining is carried out in a converter, followed by LF refining outside the furnace. After refining, vacuum degassing is carried out in a VD furnace, and the vacuum holding time is 15 minutes. Finally, die casting is carried out, and the thickness of the ingot is 800mm. After the ingot is off the line, it is stacked and slowly cooled, and the stacking time is 55 hours;

[0085] 2) Heating and rolling process: heat the steel billet to 1180°C, with a total heating time of 790 min; in the range of ≤600°C, the heating rate is 80°C / h; in the range of >600-900°C, the heating rate is 96°C / h; in the range of ≥900-1180°C, the heating rate is 110°C / h;

[0086] The first stage is the austenite recrystallization stage, with a rolling temperature of 1030-1060°C; the second stage is the non-crystallization zone rolling, with a rolling temperature of 850-880°C; the cumulative rolling reduction rate is 60%, the water entry temperature after rolling is 840°C, and the final cooling temperature is 700°C.

[0087] 3) Heat treatment process: offline quenching treatment, quenching temperature is 920℃, holding time is 45min; quenching cooling rate is 17℃ / s; tempering temperature is 610℃, holding time is 400min.

[0088] The mechanical properties of the steel plate prepared in this embodiment are as follows: yield strength 734 MPa, tensile strength 817 MPa, yield strength ratio 0.90, and average impact energy value of 77 J at -40°C.

[0089] Example 4

[0090] The steel plate of this embodiment has a thickness of 200 mm and is composed of the following chemical components in weight percentage: C 0.17%, Si 0.25%, Cr 1.60%, Mn 1.10%, Mo 0.60%, Nb 0.03%, Ti 0.011%, V 0.04%, B 0.0019%, P 0.006%, S 0.001%, and the balance is Fe and unavoidable impurities.

[0091] 1) Smelting and continuous casting process: rough refining is carried out in a converter, followed by LF refining outside the furnace. After refining, vacuum degassing is carried out in a VD furnace, and the vacuum holding time is 15 minutes. Finally, die casting is carried out, and the thickness of the ingot is 1000mm. After the ingot is off the line, it is stacked and slowly cooled, and the stacking time is 60 hours;

[0092] 2) Heating rolling process: heat the steel billet to 1170°C, with a total heating time of 1108 min; in the range of ≤600°C, the heating rate is 48°C / h; in the range of >600-900°C, the heating rate is 91°C / h; in the range of ≥900-1170°C, the heating rate is 101°C / h;

[0093] The first stage is the austenite recrystallization stage, with a rolling temperature of 1050-1070°C; the second stage is the non-crystallization zone rolling, with a rolling temperature of 840-860°C; the cumulative rolling reduction rate is 60%, the water entry temperature after rolling is 830°C, and the final cooling temperature is 690°C.

[0094] 3) Heat treatment process: offline quenching treatment, quenching temperature is 900℃, holding time is 45min; quenching cooling rate is 15℃ / s; tempering temperature is 580℃, holding time is 500min.

[0095] The mechanical properties of the steel plate prepared in this embodiment are as follows: yield strength 715 MPa, tensile strength 804 MPa, yield strength ratio 0.89, and average impact energy at -40°C 65 J.

[0096] Comparative Examples 1-3

[0097] Three comparative examples are now set up. The thickness and composition of the steel plate in each comparative example are shown in Table 1 (the balance is Fe). The relationship between Cr and Mn in the composition does not conform to the defined relationship between Cr and Mn defined in the present invention. This series of components is produced according to the production process flow of the above corresponding thickness (such as comparative example 1 corresponds to embodiment 1, comparative example 2 corresponds to embodiment 2, and comparative example 3 corresponds to embodiment 3), and performance tests are carried out. The test results are shown in Table 2.

[0098] Table 1 Composition of steel plates of different thicknesses in Comparative Examples 1-3 (mass fraction %)

[0099]

[0100] Table 2 Mechanical properties of steel plates of different thicknesses in comparative examples 1-3

[0101]

[0102] Conclusion: It can be seen from Table 2 that if the steel plate is not prepared within the limited relationship between Cr and Mn defined in the present invention, although the yield strength and tensile strength can meet the standard requirements, the yield strength ratio cannot meet the requirement of ≤0.93.

[0103] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A medium-thickness, low-cost, low-yield-to-strength ratio ultra-high strength steel plate, characterized in that: The thickness of the steel plate is X, 60 mm ≤ X ≤ 100 mm, and the chemical composition of the steel plate, measured by mass percentage, includes: C 0.13%~0.18%, Si 0.10%~0.35%, Cr 1.20%~2.00%, Mo 0.30%~0.60%, Nb0.02%~0.03%, Ti 0.005%~0.02%, V 0.02%~0.05%, B 0.0005%~0.002%, P≤0.01%, S≤0.005%, the mass percentage of Mn conforms to the following relationship: Cr / Mn≥1.8, Cr%+Mn%≥1.8%; the balance is Fe.

2. A medium-thickness, low-cost, low-yield-to-strength ratio ultra-high strength steel plate, characterized in that: The thickness of the steel plate is X, 100 mm < X ≤ 150 mm, and the chemical composition of the steel plate, measured by mass percentage, includes: C 0.13%~0.18%, Si 0.10%~0.35%, Cr 1.20%~2.00%, Mo 0.30%~0.60%, Nb0.02%~0.03%, Ti 0.005%~0.02%, V 0.02%~0.05%, B 0.0005%~0.002%, P≤0.01%, S≤0.005%, the mass percentage of Mn conforms to the following relationship: Cr / Mn≥1.5, Cr%+Mn%≥2.2%; the balance is Fe.

3. A medium-thickness, low-cost, low-yield-to-strength ratio ultra-high strength steel plate, characterized in that: The thickness of the steel plate is X, 150 mm < X ≤ 200 mm, and the chemical composition of the steel plate, measured by mass percentage, includes: C 0.13%~0.18%, Si 0.10%~0.35%, Cr 1.20%~2.00%, Mo 0.30%~0.60%, Nb0.02%~0.03%, Ti 0.005%~0.02%, V 0.02%~0.05%, B 0.0005%~0.002%, P≤0.01%, S≤0.005%, the mass percentage of Mn conforms to the following relationship: Cr / Mn≥1.2, Cr%+Mn%≥2.4%; the balance is Fe.

4. A method for preparing medium-thickness, low-cost, low-yield ratio ultra-high strength steel plate, characterized in that: The following steps are involved: Smelting and casting the chemical composition according to any one of claims 1 to 3 to obtain a steel billet; The steel billet is sequentially heated, rolled, off-line quenched and tempered to obtain the steel plate.

5. The method for preparing a medium-thickness, low-cost, low-yield ratio ultra-high strength steel plate according to claim 4, characterized in that: The parameters in the heating process are: Heat the steel billet to 1150-1200℃, with a total heating time of ≥1min / mm; Heating speed: when heating temperature is ≤600℃, heating speed is ≤90℃ / h; When 600℃<heating temperature<900℃, 90℃ / h<heating speed≤100℃ / h; When the heating temperature is 900℃≤ and the heating temperature is less than 1200℃, the heating rate is 100℃ / h<and less than 120℃ / h.

6. The method for preparing a medium-thickness, low-cost, low-yield ratio ultra-high strength steel plate according to claim 4, characterized in that: The rolling process adopts two-stage rolling; The first stage is the austenite recrystallization stage, with a rolling temperature of 980-1080°C; The second stage is rolling in the non-crystallized zone, with a rolling temperature of 800-880°C; The cumulative rolling reduction rate is ≥50%.

7. The method for preparing a medium-thickness, low-cost, low-yield ratio ultra-high strength steel plate according to claim 4, characterized in that: The offline quenching process is specifically as follows: the quenching temperature is 900-940°C, and the holding time is 30-45min; Quenching cooling rate ≥15℃ / s; The tempering temperature is 580~650℃, and the holding time is ≥2.5min / mm.

8. The method for preparing a medium-thickness, low-cost, low-yield ratio ultra-high strength steel plate according to claim 7, characterized in that: When 60mm≤X≤100mm, the quenching cooling rate is ≥20℃ / s.

9. The method for preparing a medium-thickness, low-cost, low-yield ratio ultra-high strength steel plate according to claim 7, characterized in that: When 100mm<X≤150mm, quenching cooling rate is 17℃ / s≤<20℃ / s.