Deformed steel bar with yield strength larger than or equal to 1200 MPa and production method

Through the combination of specific chemical components and processes, the problems of insufficient yield strength and low production efficiency in the prior art are solved, and the production of high-performance rebar is realized, which simplifies the process and reduces costs.

CN118957426AActive Publication Date: 2024-11-15武汉钢铁有限公司
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411366603.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-15
Estimated Expiration
2044-09-29

AI Technical Summary

Technical Problem

It is difficult to produce fine-rolled threaded steel bars with a yield strength of ≥1200MPa, and there are problems such as high steel alloy content, high energy consumption, poor cooling effect and low production efficiency.

Method used

The rolling temperature and speed are controlled through converter smelting, LF furnace refining, casting, rolling and cooling processes, such as C: 0.48-0.65%, Si: 0.80-1.55%, Mn: 1.00-1.65%, etc. , uniform martensite structure is formed to improve the strength and toughness of the steel bars.

Benefits of technology

High-performance rebar with yield strength ≥1200MPa, tensile strength ≥1330MPa and elongation ≥6% was achieved, which simplified the process flow, improved product performance stability and production efficiency, and reduced costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957426A_ABST
    Figure CN118957426A_ABST
Patent Text Reader

Abstract

The invention relates to engineering machinery steel with excellent plate shape and yield strength greater than or equal to 1200 MPa. The engineering machinery steel comprises the following components in percentage by weight: 0.48-0.65% of C, 0.80-1.55% of Si, 1.00-1.65% of Mn, less than or equal to 0.035% of P, less than or equal to 0.035% of S, 0.0006-0.0038% of B, 0.60-1.10% of Cr, 0.50-0.75% of Zr, 0.0045-0.0120% of N, less than or equal to 0.10% of V or less than or equal to 0.05% of Nb or a mixture of the two, and the mixture of the two meets the condition that (V + 1.6 Nb) is not less than 0.03%; pretreating molten iron; smelting in a converter; refining in an LF furnace; casting into a square billet; heating the casting blank; performing rough rolling and intermediate rolling; finish rolling is conducted according to two sections; and cooling. The hot rolling yield strength Rel is larger than or equal to 1200 MPa, Rm is larger than or equal to 1330 MPa, the elongation A is larger than or equal to 6%, and Agt is larger than or equal to 3.5%, the process is simple, the performance of a finished deformed steel bar product is stable, the load of a rolling mill can be reduced by increasing the heating temperature on the premise that the cost is greatly reduced, and the production efficiency can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a threaded steel and a production method, and specifically relates to a threaded steel with a yield strength of ≥1200MPa and a production method. The threaded steel is particularly suitable for producing threaded steel with a diameter of 34-75mm, and is used for hydropower dams, urban interchanges, highway bridges, port terminals, railway bridges, etc. 1200MPa fine-rolled threaded steel and a production method. Background Art

[0002] Finely rolled threaded steel bar, also known as prestressed concrete threaded steel bar, is a straight steel bar with discontinuous external threads and no longitudinal ribs on the entire surface of the steel bar. This steel bar is directly connected with nuts and spiral sleeves, without welding and machining screw buckles. It has the advantages of simple connection and anchoring, strong adhesion, safe and reliable tensioning and anchoring, convenient construction, fast speed, and material saving. Finely rolled threaded steel bar is widely used in large-scale water conservancy and hydropower projects, continuous beams and large frame structures in industrial and civil buildings, highways, high-speed railways, large bridge baskets, nuclear power plants, ground anchors, slope anchors, and other super-large buildings, frame structures, bridges and culverts and other projects.

[0003] Finished rolled steel bar products are high-tech steel products in China, and have extremely strict requirements on the grade and quality of the products. Since there is no need to consider the impact of welding performance, a variety of micro-alloying or heat treatment processes can be used to produce this steel. According to the characteristics of finished rolled threaded steel bars, the connection device and finished product pass of the finished rolling mill need to be redesigned, and high control accuracy is required during the rolling process.

[0004] Compared with the traditional general bar rolling production line, the high-speed bar production line adopts the roller ring rolling mill to obtain higher precision finished products. The single-bar torsion-free low-temperature controlled rolling technology is adopted in the finishing rolling area to achieve alloy reduction production. Placing a single bar for a single tooth groove on the cooling bed for cooling and single-bar alignment can obtain a higher yield rate. Based on these advantages, the high-speed bar production technology has developed rapidly in recent years.

[0005] There are currently two main types of high-speed bar production lines: one is a single-line high-speed bar production line, also referred to as a single-high bar production line, that is, the rough rolling, intermediate rolling, pre-finishing rolling, and finishing rolling units are all single-bar rolling, and after finishing rolling, they are sent to a cooling bed by a set of high-speed steel-loading system; the other is a double-line high-speed bar production line, also referred to as a double-high bar production line, that is, rough rolling and intermediate rolling are single-bar rolling, pre-finishing rolling is two-slice rolling, and after pre-finishing rolling, double lines enter two groups of finishing rolling units at the same time, each line rolls a single bar in each group of finishing rolling, and after finishing rolling, they are merged and sent to the cooling bed by a set of double high-speed steel-loading system that can meet the needs of double lines on the cooling bed at the same time.

[0006] In the national standard GB / T 20065-2016, the chemical composition (melting composition) of finished rolled threaded steel bars is not clearly specified except that the mass fraction of S and P is controlled to be ≤0.035%. The chemical composition and alloy elements are selected by the manufacturer to ensure that the finished steel bars processed by different methods meet the mechanical property requirements specified in the standard. Finished rolled threaded steel bars have added relaxation, fatigue, and non-metallic inclusion inspection items, and the quality requirements are significantly higher than those of ordinary threaded steel bars.

[0007] The fine-rolled threaded steel bars are classified according to the yield strength level, including five grades: PSB785, PSB830, PSB930, PSBl080, and PSB1200. Among them, PSB1200 is the grade with the highest strength level among the fine-rolled threaded steel bars, requiring yield strength ≥1200MPa, tensile strength ≥1330MPa, elongation after fracture ≥6%, and total elongation under maximum force ≥3.5%.

[0008] Since there is no unified chemical composition requirement in the product standard of finished rolled rebar, domestic steel mills use carbon steel microalloy strengthening technology for chemical composition design, generally using hypoeutectoid steel with medium and low carbon content. There are mainly two types of chemical composition design for finished rolled rebar, namely 40Si2MnV and Mn bainite steel. The 40Si2MnV component control process rolling process is produced by the post-rolling residual heat treatment process. The internal and external organizations of the steel bars are inconsistent, and the gradient of the organizational morphology from the surface to the core is large, resulting in large fluctuations in product performance; the internal and external organizations of the Mn bainite finished rolled rebar are both bainite / martensite composite phases, the microstructure is uniform, and the performance is relatively stable. However, due to the main hard phase organization after rolling, the internal stress and residual stress of the organization are large, and it is necessary to carry out pit slow cooling or annealing heat treatment to eliminate stress cracks and reduce cracking tendency. At present, these two types of steel only produce finished rolled rebars with a yield strength of 785MPa to 1080MPa, and there is no report on the industrial production of 1200MPa high-strength finished rolled rebar.

[0009] Therefore, the development and stable batch supply of 1200MPa grade high-strength fine-rolled threaded steel bars will meet the market demand for high-strength steel and the needs of major engineering construction. Replacing low-strength steel with high-strength steel can reduce the overall steel consumption and has good economic and social benefits.

[0010] After searching,

[0011] The document of Chinese patent application number CN202311374054.X (publication number CN 117230375A) discloses "A rare earth corrosion-resistant high-strength refined threaded steel bar and its processing method", whose chemical composition weight percentage is: C: 0.23-0.34%, Si: 0.7-1.2%, Mn: 1.4-1.8%, V: 0.01-0.05%, lanthanum La: 0.01-0.05%, cerium Se: 0.01-0.05%, Fe: balance, the steel billet containing rare earth on the surface is heated to the rolling temperature and then rolled into a steel bar with regular threads; and cooled to room temperature; the rolled steel bar with regular threads is heated to the rolling temperature and rolled into a steel bar with regular threads; and the rolled steel bar with regular threads is heated to the rolling temperature and rolled into a steel bar with regular threads; and the rolled steel bar with regular threads is cooled to room temperature; and the rolled steel bar with regular threads is heated to the rolling temperature and rolled into a steel bar with regular threads ... The regular threaded steel bar is sent into the induction heating furnace at a speed of 5-15m per minute and heated to 830-930℃; the steel bar after induction heating is directly quenched with high-pressure jet water or quenching liquid without insulation, the quenching cooling rate is 200-250℃ / s, the quenching pressure reaches above 16MPa, the quenching cooling time is 5-30 seconds, and the steel bar temperature is cooled to below Ms point; the quenched steel bar is heated to 350-500℃ in the tempering heating furnace; the tempered steel bar is water-cooled to 230 degrees and directly cooled to room temperature with water. The head of each steel bar is connected to the tail of another steel bar by carbon dioxide protective gas ring welding, and then heated, quenched, and tempered in turn under the traction of the front traction drive system, and then pulled out and cooled by the rear traction drive system. The frequency difference between the front and rear traction drive systems is 25%-40%. Since the head and tail of the steel bar are welded together, the steel bar runs forward in the speed difference state of the front and rear traction, which ensures that the steel bar is quenched and tempered under the condition of micro-tension, greatly reducing the relaxation rate of the steel bar. This document adopts the production process of online hot rolling + offline quenching and tempering heat treatment, which has the disadvantages of complex process, low production efficiency and difficult production organization. Summary of the invention

[0012] Aiming at the shortcomings of the prior art such as high steel bar alloy content, high energy consumption, poor cooling effect and low production efficiency, the present invention provides a 1200MPa fine-rolled threaded steel with a nominal diameter of 34-75mm and a production method, which has a hot-rolled yield strength Rel≥1200MPa, Rm≥1330MPa, an elongation A≥6% and Agt≥3.5%, and has a simple process and stable product performance.

[0013] Measures to achieve the above objectives:

[0014] A threaded steel with a yield strength of ≥1200MPa, wherein the components and weight percentage contents are: C: 0.48-0.65%, Si: 0.80-1.55%, Mn: 1.00-1.65%, P≦0.035%, S≦0.035%, B: 0.0006-0.0038%, Cr: 0.60-1.10%, Zr: 0.50-0.75%, N 0.0045-0.0120%, V: not higher than 0.10% or Nb not higher than 0.05% or a mixture of the two, and the mixture of the two satisfies: (V+1.6Nb) is not lower than 0.03%, and the rest is Fe and unavoidable impurities.

[0015] Preferably, the weight percentage of C is 0.49-0.60%.

[0016] Preferably, the weight percentage of Si is between 0.90 and 1.45%.

[0017] Preferably, the weight percentage of Mn is 1.10-1.50%.

[0018] Preferably, the weight percentage of B is 0.0006-0.0025%.

[0019] Preferably, the weight percentage of Cr is 0.65-0.95%.

[0020] Preferably, the weight percentage of Nb is 0.015-0.035%.

[0021] Preferably, the weight percentage of Zr is 0.55-0.70%.

[0022] A method for producing a threaded steel bar with a yield strength ≥ 1200 MPa, comprising the following steps:

[0023] 1) Pre-treat the molten iron. After desulfurization, the molten iron has P < 0.020%, S < 0.020%;

[0024] 2) Converter smelting, control the converter endpoint C at 0.1-0.36%, and the tapping temperature ≥1650℃; when the molten steel is 2 / 3 out, the alloy and carburizer should be added all at once;

[0025] 3) Carry out LF furnace refining, the refining time is not less than 25min, and argon is blown throughout the refining process; after the composition is adjusted, the molten steel is prohibited from being exposed;

[0026] 4) Casting into billets, during which a large tank long nozzle and a crystallizer immersion nozzle are used to protect the pouring, and the superheat of the molten steel in the middle package is controlled at 20-35°C; the cross-sectional size of the continuous casting billet is not less than 200mm, and the ratio of the billet cross-sectional area to the thread cross-sectional area is controlled to be not less than 9.0;

[0027] 5) When heating the ingot, the temperature of the soaking section is controlled at 1100-1220°C, and the total heating time is 60-90 minutes; and the temperature difference of the same ingot section is controlled to be ≤35°C;

[0028] 6) performing rough rolling and intermediate rolling, and controlling the starting rolling temperature to be between 1000°C and 1060°C, and controlling the cumulative deformation rate of rough rolling and intermediate rolling to be between 15% and 50%;

[0029] 7) Finish rolling is performed in two stages, during which: the temperature of the finishing rolling stage I is controlled at 880-950°C, the temperature of the finishing rolling stage II is controlled at 900-980°C, and the rolling speed of the final stand is controlled at 1.2-20.8 m / s;

[0030] 8) Cooling is performed, the temperature of the cooling bed is controlled at 320-380°C, and the cooling rate is 3-7°C / s to cool to room temperature.

[0031] Functions and mechanisms of the components and main processes in the present invention

[0032] C: C is the cheapest and most effective strengthening element in steel materials. It can play a role of solid solution strengthening when dissolved in the matrix. If the C content is lower than 0.65%, it is difficult to ensure the yield strength and tensile strength of the steel bar. If the C content is higher than 0.48%, the toughness of the steel will deteriorate. Therefore, the C content is controlled at 0.48-0.65%, preferably at 0.49-0.60%.

[0033] Si: It exists in the steel in a solid solution state to improve the strength and is also a deoxidizing element for steelmaking. Under the premise of ensuring that the strength and toughness of the steel bars meet the requirements, as much cheap Si element as possible is used, but the content should not be too high to avoid reducing the toughness and plasticity of the steel. Therefore, the Si content is controlled at 0.80-1.55%, and preferably the Si content is 0.90-1.45%.

[0034] Mn: Mn dissolves in ferrite to improve the strength of steel, reduce the supercooled austenite transformation temperature, refine ferrite grains, and is beneficial to improving the strength and toughness of finished rolled steel bars. However, Mn is also an element that is prone to segregation. The higher the content, the more likely it is to segregate. Therefore, the Mn content is controlled at 1.00-1.65%, and preferably the Mn content is 1.10-1.50%.

[0035] P, S: P and S are harmful elements in this steel. Generally, the lower their content, the better. Considering the actual control of steelmaking and production cost factors, P is controlled to be ≤ 0.035% and S ≤ 0.035%.

[0036] B: B in alloy steel mainly improves the hardenability of steel, but the inherent properties of steel bars do not involve hardenability. In the present invention, B is a strong nitride-forming element, and the formation of fine dispersed BN can produce precipitation strengthening effect, improve the strength of steel, and has a strong affinity with the O element, which can reduce free oxygen and nitrogen in steel, which is conducive to eliminating the aging phenomenon of steel bars. At the same time, adding trace hardenability elements can make up for the lack of online controlled cooling ability and accelerate the transformation of organization, but when the B content is too high, the strength and toughness of the steel will be deteriorated, so the content is controlled at 0.0006-0.0038%, preferably the B content is 0.0006-0.0025%.

[0037] Cr: can reduce the transformation temperature of supercooled austenite, refine ferrite grains, refine pearlite lamellae, and improve the strength of steel bars. However, too high a Cr content will deteriorate the toughness of the steel. Therefore, the Cr content is controlled at 0.60-1.10%, and preferably the Cr content is 0.65-0.95%.

[0038] Zr: Zirconium can degas and refine grains, but too high a zirconium content will increase smelting difficulty and production costs, and cause local segregation, deteriorating steel properties, so the content is controlled at 0.50-0.75%, preferably the Zr content is 0.55-0.70%.

[0039] N: N is a gas element, which combines with V and NbI microalloying elements in steel to form second phase particles such as VN and NbN, which enhances precipitation strengthening and fine grain strengthening, significantly improves the strength of steel and improves toughness. At the same time, N is a gas element and its control is relatively unstable. If it is added too little, it is difficult to ensure the above-mentioned strengthening effect. If it is added too much, the toughness of the steel bar will decrease and the difficulty of smelting operation will increase. Therefore, the content is controlled at 0.0045-0.0120%. The N content is preferably 0.0055-0.0095%.

[0040] V, Nb, Ti: the most common microalloying elements. These three elements are all strong nitride and carbide forming elements. During the coil rolling process, when small dispersed second phase particles are generated, a strong precipitation strengthening effect can be produced, and the grains can be refined, and the strength and toughness of the steel can be improved. When the content of V, Nb and Ti is too much, the size of the precipitates will increase, which may worsen the above effects, especially for large and hard TiN particles. It has been proved through multiple rounds of tests that good results can be achieved by considering the mutual influence between two or three elements at the same time, controlling V 0~0.10%, Nb 0~0.05%, and satisfying: 2.0≤(V+2Nb+2Ti) / N≤4.6.

[0041] High compression ratio rolling into products: The present invention adopts continuous casting billets with cross-sectional dimensions of 200mm×200mm, 220mm×220mm and above for rolling. Compared with the general rolling of 150mm×150mm, 160mm×160mm continuous casting billets, it has a larger compression ratio feature. The large deformation rolling can increase the compression rate of the billet, which is beneficial to improving the fineness and uniformity of the micro-grains of the steel bars, and is beneficial to improving the strength and toughness of the steel. In addition, it can increase the nucleation and growth of controlled cooling martensite.

[0042] The reason why the converter endpoint C is controlled at 0.1-0.36% and the tapping temperature is ≥1650°C and the alloy and the carburizer are all added at one time when 2 / 3 of the molten steel is tapped is that the contents of Si, Mn, Al, V, Zr alloy elements and C element can be accurately controlled. If the alloy elements are added in advance, the alloy elements will be oxidized too early, resulting in a low yield. If the alloy elements are added later, the alloy blocks will not have time to melt in the molten steel, resulting in uneven composition and even the presence of foreign metals.

[0043] The reason why the temperature of the soaking section is controlled at 1100-1220°C and the total heating time is 60-90 minutes, and the temperature difference of the cross section of the same billet is controlled to be ≤35°C, is that the use of soaking forging high temperature heating of 1100-1180°C and a long heating time is beneficial to the uniform diffusion of various components in the steel, reducing segregation, and being beneficial to uniform microstructure and stable performance.

[0044] The reason why the present invention controls the start rolling temperature at 1000-1060°C during rough and medium rolling, and controls the cumulative deformation rate of rough and medium rolling at 15-50% is that the use of this start rolling temperature can ensure that the steel billet is fully austenitized in the heating furnace and undergoes austenite zone rolling deformation in subsequent rolling, which is beneficial to uniform composition and organization, and controlling the cumulative deformation rate can ensure uniform and refined microstructure.

[0045] The reason why the temperature of entering the finishing rolling stage I is controlled at 880-950°C, the temperature of entering the finishing rolling stage II is controlled at 900-980°C, and the rolling speed of the final stand is controlled at 1.2-20.8 m / s is that the finishing rolling still adopts rolling deformation in the austenite zone, which is beneficial to ensure the appropriate strength and plasticity of the steel product; the speed of the final stand is controlled at 1.2-20.8 m / s because different rolling speeds are adopted for specifications of 34-75 mm, which, on the one hand, exerts the deformation-induced strengthening effect, and on the other hand, ensures smooth production and increases hourly output.

[0046] The reason why the present invention controls the temperature of entering the cooling bed at 320-380°C is to obtain a martensitic structure by strong cooling after rolling so as to have higher strength and suitable plasticity. If the temperature of entering the cooling bed is too low, the plasticity of the steel is insufficient, and vice versa, the strength of the steel is insufficient.

[0047] Compared with the prior art, the present invention has a hot-rolled yield strength of Rel≥1200MPa, Rm≥1330MPa, an elongation A≥6%, and Agt≥3.5%, a simple process, and stable performance of the finished rolled threaded steel product. Moreover, by increasing the heating temperature, the rolling mill load can be reduced while the cost is greatly reduced, which is beneficial to improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is a picture of the metallographic structure of the thread of the present invention being tempered troostite. DETAILED DESCRIPTION

[0049] The present invention is described in detail below:

[0050] Table 1 is a list of chemical composition values ​​of various embodiments and comparative examples of the present invention;

[0051] Table 2 is a list of process parameters of the smelting process of various embodiments and comparative examples of the present invention;

[0052] Table 3 is a list of rolling process parameters of various embodiments of the present invention and comparative examples;

[0053] Table 4 shows the test results of various embodiments of the present invention and comparative examples.

[0054] Each embodiment of the present invention is produced according to the following steps

[0055] 1) Pre-treat the molten iron. After desulfurization, the molten iron has P < 0.020%, S < 0.020%;

[0056] 2) Converter smelting, control the converter endpoint C at 0.1-0.36%, and the tapping temperature ≥1650℃; when the molten steel is 2 / 3 out, the alloy and carburizer should be added all at once;

[0057] 3) Carry out LF furnace refining, the refining time is not less than 25min, and argon is blown throughout the refining process; after the composition is adjusted, the molten steel is prohibited from being exposed;

[0058] 4) Casting into billets, during which a large tank long nozzle and a crystallizer immersion nozzle are used to protect the pouring, and the superheat of the molten steel in the middle package is controlled at 20-35°C; the cross-sectional size of the continuous casting billet is not less than 200mm, and the ratio of the billet cross-sectional area to the thread cross-sectional area is controlled to be not less than 9.0;

[0059] 5) When heating the ingot, the temperature of the soaking section is controlled at 1100-1220°C, and the total heating time is 60-90 minutes; and the temperature difference of the same ingot section is controlled to be ≤35°C;

[0060] 6) performing rough rolling and intermediate rolling, and controlling the starting rolling temperature to be between 1000°C and 1060°C, and controlling the cumulative deformation rate of rough rolling and intermediate rolling to be between 15% and 50%;

[0061] 7) Finish rolling is carried out in two stages, during which the temperature of the finishing rolling stage I is controlled at 880-950°C and the temperature of the finishing rolling stage II is controlled at

[0062] 900~980℃, the rolling speed of the final stand is 1.2~20.8m / s;

[0063] 8) Cooling is performed, the temperature of the cooling bed is controlled at 320-380°C, and the cooling rate is 3-7°C / s to cool to room temperature.

[0064] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)

[0065]

[0066]

[0067] Table 2 List of process parameters of the smelting process of each embodiment of the present invention and the comparative example

[0068]

[0069] Table 3 List of rolling process parameters of various embodiments of the present invention and comparative examples

[0070]

[0071]

[0072] Table 4 Performance test results of various embodiments of the present invention and comparative examples

[0073]

[0074] Note: The thread diameters of the above embodiments are all within the range of 34-75 mm.

[0075] It can be seen from Table 4 that compared with the comparative example, the steel of the embodiment of the present invention has higher yield strength, tensile strength and more suitable plastic properties such as elongation, and can reduce the total cost of use.

[0076] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.

Claims

1. A threaded steel bar with a yield strength of ≥1200 MPa, wherein the components and weight percentages thereof are: C: 0.48-0.65%, Si: 0.80~1.55%, Mn: 1.00~1.65%, P≦0.035%, S≦0.035%, B: 0.0006~0.0038%, Cr: 0.60~1.10%, Zr: 0.50~0.75%, N 0.0045~0.0120%, V: not higher than 0.10% or Nb not higher than 0.05% or a mixture of the two, and the mixture of the two satisfies: (V+1.6Nb) is not less than 0.03%, and the rest is Fe and unavoidable impurities.

2. The threaded steel bar with a yield strength of ≥1200 MPa according to claim 1, characterized in that: The weight percentage of C is 0.49-0.60%.

3. The threaded steel bar with a yield strength of ≥1200 MPa according to claim 1, characterized in that: The weight percentage of Si is 0.90-1.45%.

4. The threaded steel bar with a yield strength of ≥1200 MPa according to claim 1, characterized in that: The weight percentage of Mn is 1.10-1.50%.

5. The threaded steel bar with a yield strength ≥ 1200 MPa according to claim 1, characterized in that: The weight percentage of B is 0.0006-0.0025%.

6. The threaded steel bar with a yield strength of ≥1200 MPa according to claim 1, characterized in that: The weight percentage of Cr is 0.65-0.95%.

7. The threaded steel bar with a yield strength of ≥1200 MPa according to claim 1, characterized in that: The weight percentage of Nb is 0.015-0.035%.

8. The threaded steel bar with a yield strength of ≥1200 MPa according to claim 1, characterized in that: The weight percentage of Zr is 0.55-0.70%.

9. A method for producing a threaded steel bar with a yield strength of ≥1200 MPa as claimed in claim 1, comprising the steps of: 1) Pre-treat the molten iron. After desulfurization, the molten iron has P < 0.020%, S < 0.020%; 2) Converter smelting, control the converter endpoint C at 0.1-0.36%, and the tapping temperature ≥1650℃; when the molten steel is 2 / 3 out, All the alloy and carburizer should be added at once; 3) Carry out LF furnace refining, the refining time is not less than 25min, and argon is blown throughout the refining process; after the composition is adjusted, the molten steel is prohibited from being exposed; 4) Casting into billets, during which a large tank long nozzle and a crystallizer immersion nozzle are used to protect the pouring, and the superheat of the molten steel in the middle package is controlled at 20-35°C; the cross-sectional size of the continuous casting billet is not less than 200mm, and the ratio of the billet cross-sectional area to the thread cross-sectional area is controlled to be not less than 9.0; 5) When heating the ingot, the temperature of the soaking section is controlled at 1100-1220°C, and the total heating time is 60-90 minutes; and the temperature difference of the same ingot section is controlled to be ≤35°C; 6) performing rough rolling and intermediate rolling, and controlling the starting rolling temperature to be between 1000°C and 1060°C, and controlling the cumulative deformation rate of rough rolling and intermediate rolling to be between 15% and 50%; 7) Finish rolling is performed in two stages, during which: the temperature of the finishing rolling stage I is controlled at 880-950°C, the temperature of the finishing rolling stage II is controlled at 900-980°C, and the rolling speed of the final stand is controlled at 1.2-20.8 m / s; 8) Cooling is performed, the temperature of the cooling bed is controlled at 320-380°C, and the cooling rate is 3-7°C / s to cool to room temperature.

Citation Information

Patent Citations

  • Steel wire for bolt, bolt, and manufacturing processes therefor

    CN103842546A

  • Finish-rolled twisted steel with yield strength being more than or equal to 960MPa and production method thereof

    CN104046907A

  • Microalloying third-generation car spring flat steel and preparing method thereof

    CN106978571A

  • Steel for alloy structure and manufacturing method thereof

    CN112575242A

  • Low-relaxation ultrahigh-strength finish-rolled twisted steel and preparation method thereof

    CN114686764A