Steel containing B for straight seam welding hollow anchor rod body for railway tunnel and preparation method of straight seam welding hollow anchor rod body
By adjusting chemical composition and preparation process, the problem of the mechanical properties of hollow anchor rods for railway tunnels does not meet the requirements and high costs. The steel for hollow anchor rod body with B is used to weld the steel for hollow anchor rod body with B to achieve performance improvement and cost reduction, meeting the Technical requirements for railway tunnel anchors.
Patent Information
- Application Number
- CN202411069229.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the mechanical properties of the hollow anchor rod body for railway tunnels do not meet the technical requirements, and the cost is too high and the cost of alloy is too high.
The steel for hollow anchor rod body with B-containing straight seam welding is used, and the chemical composition and preparation process are adjusted, including smelting, converter, LF refining, continuous casting, heating, rough rolling, hot rolling, finish rolling, laminar cooling, Welding, high-frequency heating and online heat treatment, a straight-sea welded hollow anchor rod body that meets performance requirements was prepared.
The mechanical properties of the straight-seater welded hollow anchor rod body have been improved, meeting the technical requirements of "Railway Tunnel Anchor Bolt" (TB/T 3356-2021), reducing production costs, and improving the hardenability and production efficiency of materials.
Smart Images

Figure CN118957437A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hollow anchor steel, in particular to a Disclosed is a steel containing B for a straight seam welded hollow anchor rod body for railway tunnels and a method for preparing the straight seam welded hollow anchor rod body. Background Art
[0002] By the end of 2022, China's railway operating mileage will reach 155,000 km; among them, 17,873 railway tunnels will be put into operation with a total length of 21,978 km. In 2022, 341 new railway tunnels will be put into operation with a total length of 923 km, including 25 special-length tunnels over 10 km with a total length of about 362 km. There are 3,025 railway tunnels under construction with a total length of 7,704 km; 5,376 railway tunnels are planned with a total length of 13,221 km. Judging from the distribution of railways under construction and planning, most of them are distributed in areas with complex geological structures, and the design and construction are becoming more and more difficult, especially in tunnel construction. The technical requirements for the required materials are getting higher and higher. As for the steel used for tunnel and bridge support, in order to reduce the difficulty of construction, save construction costs and shorten the construction period, the overall technical goal of high performance and lightweight is proposed.
[0003] Anchor rods are the main supporting structures for roads, slopes, dams, tunnels, bridges and mine tunnels, playing a supporting and reinforcing role. With the promotion and development of technology, their application is becoming more and more extensive, and the demand is increasing. The working principle of anchor rods is to overcome the shortcoming that the tensile capacity of rock and soil is far lower than its compressive capacity through the longitudinal tension of the anchor rod body. On the surface, it limits the rock and soil from separating from the original body, and on a macroscopic level, it increases the cohesiveness of the rock and soil. It is a rod system structure for reinforcing rock and soil.
[0004] The Chinese invention patent with publication number CN 116024493 A discloses a hot-rolled steel strip for high-strength, corrosion-resistant hollow anchor welded pipe and its preparation method, which is composed of the following components in weight percentage: 0.18%≤C≤0.23%, 0.15%≤Si≤0.30%, 0.90%≤Mn≤1.10%, P≤0.020%, S≤0.007%, 0.02%≤Nb≤0.04%, 0.70%≤Cr≤0.90%, 0.20%≤Cu≤0.50%, 0.01%≤Ti≤0.03%, 0.04%≤Sb≤0.08%, and the rest is Fe and unavoidable impurities. The invention adds a relatively high content of Cr, Cu, Sb corrosion-resistant elements and precious metal Nb, and its yield strength is ≥600MPa and tensile strength is ≥700MPa, which is suitable for the production of As for the hollow anchor rod body, the strength after the processing of "welding → reheating → three-roller spinning rolling → online heat treatment → slow cooling on a cooling bed" is too high, and there are problems of high alloy cost and excess quality. Therefore, the product involved in this invention does not meet the technical requirements for the production of hollow anchor rod bodies for railway tunnels.
[0005] The Chinese invention patent with publication number CN 116024494 A discloses a corrosion-resistant hollow anchor welded pipe, a hot-rolled steel strip and a preparation method, which are composed of the following components in weight percentage: 0.18%≤C≤0.23%, 0.15%≤Si≤0.30%, 0.70%≤Mn≤0.90%, 0.070%≤P≤0.090%, S≤0.010%, 0.03%≤Nb≤0.04%, 0.30%≤Cr≤0.40%, 0.30%≤Cu≤0.50%, 0.01%≤Ti≤0.03%, and the rest are Fe and unavoidable impurities. This invention adds higher contents of corrosion-resistant elements such as Cr, Cu and P, and the contents of Cr, Cu and P do not meet the standard requirements of TB / T 3356-2021. The addition of the precious element Nb leads to excessively high alloy costs. Therefore, the products involved in this invention do not meet the technical requirements for the production of hollow anchor rods for railway tunnels.
[0006] The Chinese invention patent with publication number CN 115976409 A discloses a low-cost hollow anchor welded pipe, hot-rolled steel strip and preparation method, which is composed of the following components in weight percentage: 0.18% ≤ C ≤ 0.25%, 0.10% ≤ Si ≤ 0.20%, 1.00% ≤ Mn ≤ 1.50%, P ≤ 0.020%, S ≤ 0.008%, 0.10% ≤ Cr ≤ 0.30%, and the rest is Fe and unavoidable impurities. The C, Si and Mn contents of this invention do not meet the standard requirements of TB / T 3356-2021, so the products involved in this invention do not meet the technical requirements for the production of hollow anchor rods for railway tunnels, and the wall thickness of the anchor rod body involved is specified.
[0007] In order to meet the technical requirements of the hollow anchor rod body in railway tunnels, a The straight seam welded hollow anchor rod body for railway tunnels is of great significance. Summary of the invention
[0008] The technical problem solved by the present invention is to provide a The steel for the rod body of the straight seam welded hollow anchor containing B for railway tunnels makes the rod body of the straight seam welded hollow anchor have better mechanical properties and meets the technical requirements of the rod body of the hollow anchor.
[0009] In view of this, the present application provides a Steel for the rod body of B-containing straight seam welded hollow anchor for railway tunnels, in percentage by mass, includes:
[0010]
[0011] P≤0.015%;
[0012] S≤0.005%;
[0013] N≤0.0040%;
[0014] Fe balance.
[0015] Preferably, the C content is 0.21-0.23%, and the Si content is 0.12-0.29%.
[0016] Preferably, the content of Mn is 0.77% to 0.93%, and the content of Ti is 0.033% to 0.049%.
[0017] Preferably, the content of B is 0.0026-0.0047%.
[0018] The present application also provides a method for preparing the straight seam welded hollow anchor rod body, comprising the following steps:
[0019] The mixture is prepared according to the mass ratio of the steel for the hollow anchor rod body for straight seam welding, and the mixture is smelted, subjected to a converter, LF refining, continuous casting, heated, roughly rolled, coiled in a hot coil box, finished rolled, laminar cooled and coiled in sequence to obtain a hot rolled coil;
[0020] The hot-rolled coil is sequentially striped, roll-formed and welded to obtain a straight seam welded pipe;
[0021] The straight seam steel pipe is subjected to high frequency heating, three-roll rolling, online heat treatment and slow cooling in sequence to obtain a straight seam welded hollow anchor rod body.
[0022] Preferably, the S of the molten iron obtained by the smelting is ≤0.003% when it enters the converter, and the argon blowing time of the small platform process is ≥8min; argon is blown throughout the LF refining process, and 70TiFe alloy is used for micro-titanium treatment before leaving the station; the heating temperature after continuous casting is 1200-1300°C, the time is 150-250min, and the soaking time is ≥30min.
[0023] Preferably, the rough rolling is performed in 5 or 7 passes; the finish rolling is performed in 7 passes, the start rolling temperature of the finish rolling is 1000-1100°C, the reduction rates of the last three stands are ≥17%, ≥15% and ≥12% respectively, and the final rolling temperature is 850-900°C.
[0024] Preferably, the laminar cooling adopts a front-stage cooling mode, the cooling rate is 50-70°C / s, and the coiling temperature is 550-650°C.
[0025] Preferably, the welding power is 80-90 kW, the frequency is 280-290 kHz, the metal flow line angle of the welded joint is 55-65°; the high-frequency heating temperature is 920-930°C, and the quenching end temperature of the online heat treatment is 350-360°C.
[0026] This application also provides a The B-containing straight seam welded hollow anchor rod body for railway tunnels is prepared from the B-containing straight seam welded hollow anchor rod body steel.
[0027] This application provides a The steel for the rod body of a straight seam welded hollow anchor rod containing B for railway tunnels comprises: C 0.20-0.24%; Si 0.10-0.30%; Mn 0.75-0.95%; Ti0.030-0.050%; B 0.0020-0.0050%; Als 0.010-0.050%; P≤0.015%; S≤0.005%; N≤0.0040%; Fe balance. The steel for the rod body of a straight seam welded hollow anchor rod provided by the present application achieves the performance requirements of the rod body of a straight seam welded hollow anchor rod by increasing the C content, reducing the Mn content, and adding a small amount of B element, thereby improving the hardenability of the material and reducing the cost.
[0028] Furthermore, the present application also provides a method for preparing a straight-seam welded hollow anchor rod body, which achieves precise organization and performance control by regulating some parameters in the preparation steps, obtains qualified products that meet performance standards, and has the characteristics of high production efficiency, small mass, and low energy consumption and cost in the entire production process.
[0029] The experimental results show that the straight-seam welded hollow anchor rod for railway tunnels prepared by the composition and preparation method of the present invention has a yield force ≥135kN, a tensile strength ≥185kN, and a maximum force total elongation ≥5%, which meets the technical requirements for hollow anchor rods in "Railway Tunnel Anchor Rods" (TB / T 3356-2021), and is suitable for the production of steel anchor rods for supporting Railway 1 tunnels. It can also be expanded to roads, tunnels, bridges and mines, and has broad market application prospects. It is estimated that the economic benefit per ton of steel is 800 yuan. Calculated based on an annual output of 10,000 tons, the economic benefit is expected to be 8 million yuan. DETAILED DESCRIPTION
[0030] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0031] In view of the problem that the performance index of the straight seam welded hollow anchor rod body in the prior art does not meet the technical requirements, the present application provides a The invention discloses a steel for a straight seam welded hollow anchor rod body containing B for railway tunnels. The steel improves the performance of the straight seam welded hollow anchor rod body by selecting the components and further combining the preparation method with the precise control of the organization, and meets the technical requirements. Specifically, the embodiment of the invention discloses a Steel for the rod body of B-containing straight seam welded hollow anchor for railway tunnels, in percentage by mass, includes:
[0032]
[0033] S≤0.005%;
[0034] N≤0.0040%;
[0035] Fe balance.
[0036] The present invention controls the content of Si and Mn elements while ensuring material strength and reducing the carbon equivalent by adding a relatively high C element, adds a trace amount of Ti element to form precipitates during welding to inhibit the coarsening of the heat-affected zone structure to improve the welding performance, and adds a certain amount of B element to ensure the hardenability of the anchor rod body obtained after rolling, thereby obtaining good online heat treatment performance.
[0037] Specifically, for the B-containing straight seam welded hollow anchor rod steel described in this application, the carbon element (C) therein: carbon is an effective strengthening element in steel, which can be dissolved into the matrix to play a role in solid solution strengthening, and can be combined with titanium to form carbide precipitation particles, which play a role in fine grain strengthening and precipitation strengthening. Increasing the carbon content is beneficial to improving strength; however, too high a carbon content will form more coarse and brittle carbide particles in the steel, which is not good for plasticity and toughness, and will form a segregation band in the center of the steel plate, which is not good for bending performance, forming performance, etc. Therefore, the value range of C in the present invention is set to 0.20% to 0.24%, specifically, the content of C is 0.21 to 0.23wt%; for example, the C content in this application is 0.20%, 0.21%, 0.22%, 0.23%, and 0.24%.
[0038] Silicon: Silicon can be dissolved in ferrite and austenite to increase the hardness and strength of steel, which is beneficial to refine the rust layer structure and reduce the overall corrosion rate of steel. However, too high a content will reduce the plasticity and toughness of the steel, making it difficult to remove scale during rolling. Therefore, the value range of Si in the present invention is set to 0.10% to 0.30%, specifically, the content of Si is 0.12 to 0.29%; for example, the content of Si in the present application is 0.10%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, 0.20%, 0.21%, 0.22%, 0.23%, 0.24%, 0.25%, 0.26%, 0.27%, 0.28%, 0.29%, 0.30%.
[0039] Manganese: Manganese has a strong solid solution strengthening effect, can significantly reduce the phase transition temperature of steel, refine the microstructure of steel, and is an important strengthening element. However, when the Mn content is too much, the continuous casting process is prone to produce cracks in the ingot, and may cause component segregation in the core of the steel plate. Therefore, the value range of Mn in the present invention is set to 0.75% to 0.95%, specifically, the content of Mn is 0.77% to 0.93%; for example, the content of Mn in this application is 0.75%, 0.76%, 0.77%, 0.78%, 0.79%, 0.80%, 0.81%, 0.82%, 0.83%, 0.84%, 0.85%, 0.86%, 0.87%, 0.88%, 0.89%, 0.90%, 0.91%, 0.92%, 0.93%, 0.94%, 0.95%.
[0040] Phosphorus: Too high a phosphorus content will significantly reduce the plasticity and low-temperature toughness of the steel. Therefore, the value range of P in the present invention is set to ≤0.015%. Specifically, the content of P is 0.006%, 0.001%, and 0.014%. Sulfur: The sulfur element will have an adverse effect on the microstructure and properties of the steel plate. Too high a sulfur content will increase the hot brittleness tendency of the steel. At the same time, sulfur will form sulfide inclusions to deteriorate the performance of the steel. Therefore, the value range of S in the present invention is set to S≤0.005%. Specifically, the content of S is 0.001%, 0.002%, and 0.003%.
[0041] Boron: Boron can form strong compounds with carbon and nitrogen in steel, thereby improving the hardness and strength of the steel; it can improve the hardenability of steel, achieve martensitic structure under relatively stable conditions, and obtain higher plasticity; it also helps to improve the welding performance of steel, improve the strength and toughness of welds, and avoid weld cracking and porosity problems; it promotes grain refinement in steel, thereby improving the toughness and impact toughness of steel, and can prevent the production of excessively large grains in steel during high-temperature heat treatment. Therefore, the value range of B in the present invention is set to 0.0020% to 0.0050%, specifically, the content of B is 0.0026% to 0.0047%; for example, the content of B in the present application is 0.0021%, 0.0022%, 0.0023%, 0.0024%, 0.0025%, 0.0026%, 0.0027%, 0.0028%, 0.0029%, 0.0030%, 0.003 1%, 0.0032%, 0.0033%, 0.0034%, 0.0035%, 0.0036%, 0.0037%, 0.0038%, 0.0039%, 0.0040%, 0.0041%, 0.0042%, 0.0043%, 0.0044%, 0.0045%, 0.0046%, 0.0047%, 0.0048%, 0.0049%, 0.0050%.
[0042] Titanium and nitrogen: Ti(C, N) precipitates formed by titanium, carbon and nitrogen can effectively refine austenite grains and produce precipitation strengthening effects. Increasing the content of titanium and nitrogen elements can increase the volume fraction of Ti(C, N) precipitates and enhance the effects of grain refinement and precipitation strengthening. However, excessive content of titanium and nitrogen elements can easily form micron-sized TiN, resulting in decreased formability. Excessive nitrogen content will increase the aging tendency, cold brittleness and hot brittleness of steel, and damage the cold bending performance of steel. Therefore, the value range of Ti in the present invention is set to 0.030-0.050%, and the value range of N is set to ≤0.0040%; specifically, the content of Ti is 0.033%-0.049%, and the content of N is 0.0020-0.0039%; for example, the content of Ti in the present application is 0.031%, 0.032%, 0.033%, 0.034%, 0.035%, 0.036%, 0.037%, 0.038%, 0.039%, 0.040%, 0.041%, 0.042%, 0.043%, 0.044%, 0.045%, 0.046%, 0.047%, 0.048%, 0.049%, 0.050%, and the N content in this application is 0.0021%, 0.0022%, 0.0023%, 0.0024%, 0.0025%, 0.0026%, 0.0027%, 0.0028%, 0.0029%, 0.0030%, 0.0031%, 0.0032%, 0.0033%, 0.0034%, 0.0035%, 0.0036%, 0.0037%, 0.0038%, 0.0039%.
[0043] Aluminum: Aluminum is added to steel to play a deoxidizing role and improve the steel quality. However, if the aluminum content is too high, its nitrogen oxides are easily precipitated at the austenite grain boundary, resulting in cracks in the casting. Therefore, the value range of Als in the present invention is set to 0.010-0.050%, specifically, the Als content is 0.015-0.048%, more specifically, the Als content is 0.023-0.047%, and more specifically, the Als content is 0.030-0.040%.
[0044] Furthermore, the present application also provides a method for preparing steel for a straight seam welded hollow anchor rod body, comprising the following steps:
[0045] The mixture is prepared according to the mass ratio of the steel for the hollow anchor rod body for straight seam welding, and the mixture is smelted, subjected to a converter, LF refining, continuous casting, heated, roughly rolled, coiled in a hot coil box, finished rolled, laminar cooled and coiled in sequence to obtain a hot rolled coil;
[0046] The hot-rolled coil is sequentially striped, roll-formed and welded to obtain a straight seam welded pipe;
[0047] The straight seam steel pipe is subjected to high frequency heating, three-roll rolling, online heat treatment and slow cooling in sequence to obtain steel for the straight seam welded hollow anchor rod body.
[0048] During the preparation process, slabs are first smelted and continuously cast according to the components. When the molten iron enters the converter, S≤0.003%. The converter needs to be "washed" before smelting. The argon blowing time of the small platform process must be ≥8min to ensure low content of nitrogen, oxygen, and hydrogen in the molten steel and remove residual non-metallic inclusions in the molten steel. The LF refining process must be argon blown throughout the process, and the molten steel must not be exposed. 70TiFe alloy is used for micro-titanium treatment before leaving the station. The continuous casting process is protected throughout the casting, and low-alloy protective slag is used. "Open casting" is not allowed to obtain continuously cast steel billets whose chemical composition meets the design requirements. The thickness of the billet is 200mm.
[0049] Further, in the step of heating the steel billet obtained after continuous casting, the heating temperature is 1200-1300°C, specifically, the heating temperature is 1240-1260°C, more specifically, the heating temperature is 1241-1258°C; the heating time is 150-250min, specifically, the heating time is 170min-245min, more specifically, the heating time is 179-220min, wherein the soaking time is ≥30min, specifically, the soaking time is 30-45min. The heating after continuous casting is to homogenize the as-cast structure and component segregation, and to dissolve the alloy elements at the same time. The C content of the steel for the hollow anchor rod body of the present invention is relatively high, so the heating process requires sufficient temperature and time; in addition, a higher heating temperature helps to promote the dissolution of alloy elements, but too high a heating temperature and too long a heating time will cause problems such as burning, overheating, and overburning. Therefore, in the present invention, the continuous casting steel billet is required to be hot-sent and hot-loaded in the heating step.
[0050] Furthermore, in the rough rolling and hot coil box coiling steps described in the above technical solution, the rough rolling needs to achieve sufficient deformation to ensure austenite recrystallization, refine austenite grains, and prevent the appearance of mixed crystal structure; if the thickness of the intermediate billet is too large, the rough rolling deformation may be insufficient, and when the finished product thickness is thin, it will cause excessive finishing rolling load; if the thickness of the intermediate billet is too small, the finishing rolling deformation may be insufficient. Therefore, the rough rolling in the present invention is preferably carried out through 6 rough rolling passes, the deformation of 1 to 3 passes should be ≥18%, the deformation of 4 to 6 passes should be ≥20%, and the thickness of the intermediate billet is 42±1mm, wherein the odd number of passes are descaled throughout the process, and then the hot coil box is coiled for insulation.
[0051] Furthermore, rolling is performed afterwards. In the finishing rolling step, the three stands after finishing rolling are basically rolled in the austenite non-recrystallization zone. By adopting a large deformation rate, the austenite grains that have been rolled in the recrystallization zone and refined to a certain extent can be flattened and elongated, and the grain boundary area of austenite per unit volume can be increased. At the same time, a large number of deformation bands and high-density dislocations will be generated in the grains, thereby increasing the ferrite nucleation rate and obtaining a fine structure after phase transformation. If the finishing rolling start temperature is too high, the deformation amount in the austenite non-recrystallization zone during the finishing rolling process is insufficient, which is not conducive to structure refinement. If the final rolling temperature is too low, the difference with the start rolling temperature is too large, so that the cooling rate of the finishing rolling process is too fast, and there is a risk that the two stands after finishing rolling are rolled in the two-phase zone, and the comprehensive performance of the product is poor. If the final rolling temperature is too high, the deformation amount in the non-recrystallization zone is insufficient, which is not conducive to final structure refinement. Therefore, the present invention sets the finishing rolling step to be 7 passes of finishing rolling, the reduction rates of the last three stands are ≥17%, ≥15% and ≥12% respectively, the finishing rolling start temperature is 1000-1100°C, and the final rolling temperature is 850-900°C. Specifically, the finishing rolling start temperature is 1025-1080°C, and the final rolling temperature is 860-885°C. The finished product thickness is 3.0 mm.
[0052] Furthermore, after the finish rolling, laminar cooling and coiling are carried out in sequence to obtain a hot-rolled coil; specifically in the laminar cooling step, the front-stage cooling mode can achieve a larger degree of supercooling so as to refine the final structure, and the use of a larger cooling rate can have a certain improvement effect on the core band structure. Therefore, the front-stage cooling mode is adopted in the present invention, and the cooling rate is 60±10℃ / s, specifically, the cooling rate is 54-68℃ / s, and more specifically, the cooling rate is 56-61℃ / s. Specifically in the coiling step, if the coiling temperature is too low, the cooling rate in the laminar cooling stage will be too large, resulting in the formation of low-temperature structures such as martensite, resulting in reduced plasticity; if the coiling temperature is too high, the grains are coarse and the pearlite lamellar spacing increases, resulting in reduced strength and toughness. Therefore, the coiling temperature in the present invention is set to 550-650℃, specifically, the coiling temperature is 565-625℃, and more specifically, the coiling temperature is 597-615℃. The finished coil thickness is 3.0mm.
[0053] The present application then sequentially strips, rolls and welds the hot-rolled coils to obtain straight seam welded pipes; the welding is specifically high-frequency resistance welding. If the welding power and frequency are too large, the metal of the welded joint will be severely burned, and the risk of welding quality defects will increase; if the welding power and frequency are too small, the weld will be poorly welded; whether the metal streamline angle is too large or too small, it is not good for the performance of the welded joint, and will cause the welded pipe to be flattened and cracked and fail. Therefore, in the present invention, the welding power is 80-90kW, the frequency is 280-290kHz, and the metal streamline angle of the welded joint is controlled to be 55-65°. Specifically, the welding power is 82-89kW, the frequency is 283-288kHz, and the metal streamline angle of the welded joint is controlled to be 56-64°. More specifically, the welding power is 85-87kW, the frequency is 285-287kHz, and the metal streamline angle of the welded joint is controlled to be 58-62°. After the above steps, a straight seam welded pipe is obtained, and the cross-sectional dimensions of the finished straight seam welded pipe are
[0054] Finally, the straight seam steel pipe is subjected to high-frequency heating, three-roll rolling, online heat treatment and slow cooling in sequence to obtain a straight seam welded hollow anchor rod body. In the high-frequency heating step, if the heating temperature is too high, the austenite grain size will be coarse, thereby causing the strength after quenching to decrease; if the heating temperature is too low, it will lead to insufficient austenitization, thereby causing the plasticity after quenching to decrease. Therefore, the high-frequency heating of the straight seam welded pipe in the present invention is set to 920-930°C, specifically, the high-frequency heating temperature is 922-929°C, and more specifically, the high-frequency heating temperature is 923-925°C.
[0055] Specifically, in the online heat treatment step of the anchor rod body obtained by three-roll spinning, the three-roll rolling is specifically three-roll spinning rolling, rolling into a spiral shape. Hollow anchor rod body; the online heat treatment is specifically an online quenching heat treatment. If the quenching temperature is too high, the martensite content will be reduced, thereby causing a decrease in strength; if the quenching temperature is too low, the bainite content will be reduced and the martensite content will be too high, thereby causing plasticity deterioration. Therefore, the quenching temperature in the present invention is set to 350-360°C, specifically, the quenching temperature is 352-358°C, and more specifically, the quenching temperature is 353-356°C. The quenching adopts annular constant temperature cooling water for online quenching heat treatment.
[0056] Furthermore, in the cooling bed slow cooling step, the residual heat of the anchor rod body is used to perform self-tempering treatment and gradually cool to room temperature.
[0057] Furthermore, in the above technical solution, the raw material hot-rolled coil for making the hollow anchor rod body has a thickness of 3.0 mm, and the preparation steps are: hot metal desulfurization, converter, LF refining, continuous casting, heating furnace heating, rough rolling, hot coil box coiling, finishing rolling, laminar cooling, coiling, and the yield strength of the hot-rolled coil obtained is ≥420MPa, the tensile strength is ≥520MPa, the elongation after fracture is ≥26%, the maximum force elongation is ≥14%, and the impact energy of the 1 / 4 size V-type specimen under the conditions of D=0a and -40℃ in the 180° bending test is ≥17J. The microstructure of the hot-rolled coil is quasi-polygonal ferrite + pearlite, and the volume fraction is ferrite (F) 80% to 90%, and pearlite (P) 10% to 20%.
[0058] Furthermore, in the above technical solution, the raw material hot-rolled coil is processed by stripping, rounding and high-frequency resistance welding to obtain The specifications of straight seam welded pipes have a yield strength of ≥550MPa, a tensile strength of ≥670MPa, an elongation after fracture of ≥16%, and an elongation at maximum force of ≥8%.
[0059] Furthermore, in the above technical solution, The straight seam welded pipes of the specifications are heated by high-frequency electric heating device, three-roller spinning, equal diameter rolling, online heat treatment, sawing, cooling bed slow cooling and other processing procedures to obtain The standard straight seam welded hollow anchor rod body has a yield strength ≥135kN, a tensile strength ≥185kN, and a maximum force elongation ≥5%.
[0060] In order to further understand the present invention, the following embodiments are provided by the present invention. The steel for the rod body of a B-containing straight seam welded hollow anchor for railway tunnels and its preparation method are described in detail, and the protection scope of the present invention is not limited by the following embodiments.
[0061] Example
[0062] This embodiment provides three groups of key process parameters in the chemical composition of the straight seam welded hollow anchor rod body for railway tunnel and its preparation method;
[0063] A sort of The chemical composition of the steel for the rod body of the straight seam welded hollow anchor for railway tunnels is shown in Table 1, and the remainder is Fe and unavoidable impurities;
[0064] The materials are prepared according to the mass ratio of the steel for the rod body of the hollow anchor for straight seam welding as shown in Table 1 to obtain a mixture, and the mixture is sequentially subjected to smelting, converter, LF refining, continuous casting, billet heating, rough rolling, hot coil box coiling, finish rolling, laminar cooling and coiling to obtain a hot rolled coil;
[0065] The hot-rolled coil is sequentially subjected to striping, roll forming and high-frequency resistance welding to obtain a straight seam welded pipe;
[0066] The straight seam steel pipe is subjected to high-frequency heating, three-roll rolling, online quenching and slow cooling in sequence to obtain a straight seam welded hollow anchor rod body;
[0067] In the above steps, the control parameters involved in the steps of billet heating, rough rolling, finishing rolling, laminar cooling, coiling, etc., as well as the indicators such as the obtained mechanical properties, process properties and microstructure types are shown in Tables 2 and 3;
[0068] In the above steps, high-frequency resistance welding, high-frequency heating of straight seam welded pipe, quenching temperature and mechanical properties obtained are shown in Table 4.
[0069] Table 1 Composition data of steel for hollow anchor rod body for straight seam welding
[0070]
[0071]
[0072] Table 2: Related parameter data table in the embodiment
[0073]
[0074] Table 3 Performance data of hot rolled coils prepared in Example
[0075]
[0076] Note: The test condition for impact performance is -40℃, and the market size is 1 / 4 size V-type specimen punch. Note: The diameter of the bending indenter is D, and the thickness of the specimen is a.
[0077] Table 4: Related parameters and performance data in the embodiment
[0078]
[0079]
[0080] It can be seen from Tables 3 and 4 that the performance of the hollow anchor rod body prepared in this application meets the technical requirements for hollow anchor rods in "Railway Tunnel Anchor Rods" (TB / T3356-2021).
[0081] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0082] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A Steel for the rod body of B-containing straight seam welded hollow anchor for railway tunnels, in terms of mass percentage, includes: P≤0.015%; S≤0.005%; N≤0.0040%; Fe balance.
2. The steel for the straight seam welded hollow anchor rod body according to claim 1, characterized in that: The C content is 0.21-0.23%, and the Si content is 0.12-0.29%.
3. The steel for the straight seam welded hollow anchor rod body according to claim 1, characterized in that: The content of Mn is 0.77% to 0.93%, and the content of Ti is 0.033% to 0.049%.
4. The steel for the straight seam welded hollow anchor rod body according to claim 1, characterized in that: The content of B is 0.0026-0.0047%.
5. The method for preparing the straight seam welded hollow anchor rod body according to claim 1 comprises the following steps: The mixture is prepared according to the mass ratio of the steel for the hollow anchor rod body for straight seam welding, and the mixture is smelted, subjected to a converter, LF refining, continuous casting, heated, roughly rolled, coiled in a hot coil box, finished rolled, laminar cooled and coiled in sequence to obtain a hot rolled coil; The hot-rolled coil is sequentially striped, roll-formed and welded to obtain a straight seam welded pipe; The straight seam steel pipe is subjected to high frequency heating, three-roll rolling, online heat treatment and slow cooling in sequence to obtain a straight seam welded hollow anchor rod body.
6. The preparation method according to claim 5, characterized in that: The S of the molten iron obtained by the smelting is ≤0.003% when entering the converter, and the argon blowing time of the small platform process is ≥8min; the LF refining is argon-blown throughout the whole process, and 70TiFe alloy is used for micro-titanium treatment before leaving the station; the heating temperature after continuous casting is 1200-1300°C, the time is 150-250min, and the soaking time is ≥30min.
7. The preparation method according to claim 5, characterized in that: The rough rolling is performed in 5 or 7 passes; the finish rolling is performed in 7 passes, the start rolling temperature of the finish rolling is 1000-1100°C, the reduction rates of the last three stands are ≥17%, ≥15% and ≥12% respectively, and the final rolling temperature is 850-900°C.
8. The preparation method according to claim 5, characterized in that: The laminar cooling adopts a front-stage cooling mode, the cooling rate is 50-70°C / s, and the coiling temperature is 550-650°C.
9. The preparation method according to claim 5, characterized in that: The welding power is 80-90kW, the frequency is 280-290kHz, and the metal flow line angle of the welding joint is 55-65°; the temperature of the high-frequency heating is 920-930°C, and the quenching end temperature of the online heat treatment is 350-360°C.
10. A The B-containing straight seam welded hollow anchor rod body for railway tunnels is prepared from the steel for the B-containing straight seam welded hollow anchor rod body according to any one of claims 1 to 4.
Citation Information
Patent Citations
Low-cost hollow anchor rod welded pipe, hot rolled steel strip and preparation method
CN115976409A
Hot rolled steel strip for high-strength corrosion-resistant hollow anchor rod welded pipe and preparation method of hot rolled steel strip
CN116024493A
Corrosion-resistant hollow anchor rod welded pipe, hot rolled steel strip and preparation method
CN116024494A
Cited By
Steel for 1000MPa-grade hollow anchor rod body and preparation method of rod body
CN121472721A