Method for synchronously and rapidly carburizing during high-energy beam welding of molybdenum alloy

By performing interface pretreatment and magnetron sputtering carbon films when welding molybdenum alloys at high-energy beams, and combining high-energy beams to achieve rapid synchronous carburization, the problem of poor welding performance of molybdenum alloys is solved, and the tensile performance and permeability of the joints are significantly improved. Carbon efficiency.

CN118957491AActive Publication Date: 2024-11-15BEIJING UNIV OF TECH

Patent Information

Application Number
CN202411030885.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Molybdenum and its alloys are poor in welding due to hard brittleness and grain boundary impurities. The traditional carburizing method is inefficient and the performance of the base material is reduced for a long time high-temperature treatment.

Method used

When welding molybdenum alloy with high energy beam, carbon film is sputtered by pretreatment of the welding interface and magnetron sputtering technology, combined with high energy beam welding to achieve rapid synchronous carburization, and carbon atoms are evenly distributed using the molten pool.

Benefits of technology

The mechanical properties of molybdenum and molybdenum alloy joints are significantly improved, and the tensile performance is improved by 200% to 220%, which improves carburizing efficiency and maintains the performance of the base material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004969898920000011
    Figure HDA0004969898920000011
  • Figure HDA0004969898920000012
    Figure HDA0004969898920000012
  • Figure HDA0004969898920000013
    Figure HDA0004969898920000013
Patent Text Reader

Abstract

The invention discloses a method for synchronously and rapidly carburizing during high-energy beam welding of molybdenum alloy, and belongs to the technical field of welding. Comprising the following steps that a molybdenum or molybdenum alloy welding interface is pretreated, and a layer of carbon film is sputtered on the molybdenum or molybdenum alloy welding interface through the magnetron sputtering technology; and relevant parameters are controlled, the treated molybdenum or / and molybdenum alloy sample is welded in a high-energy beam welding mode, and rapid and synchronous carburization can be conducted on a welded joint while molybdenum or / and molybdenum is welded through a high-energy beam. The purpose of rapid and synchronous carburization is achieved while high-energy beam welding is completed, and the mechanical property of the molybdenum or / and molybdenum alloy connector is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding, and in particular relates to a method for synchronous rapid carburizing during high-energy beam welding of molybdenum alloys. Background Art

[0002] Molybdenum and its alloys are refractory metal materials with excellent performance. They not only have the advantages of high melting point, good high temperature strength, good thermal conductivity, small linear expansion coefficient, good corrosion resistance, etc., but also have a small neutron absorption cross section, making them good materials for preparing nuclear fuel cladding tubes. However, because molybdenum and its alloys are hard and brittle materials, there will be problems with poor welding performance due to grain boundary impurities (especially oxygen) and recrystallization during welding, which limits their application.

[0003] Carburizing molybdenum alloy welded joints can greatly improve the mechanical properties of the joints. This is because carburizing purifies the oxygen in the grain boundaries of molybdenum alloys on the one hand, and on the other hand, carbon combines with molybdenum to form Mo2C, which plays a pinning role at the grain boundaries and changes the fracture mode of the joints. However, traditional carburizing requires a long time (100-200h) of carburizing treatment at high temperature (not less than 1200℃). Not only is the efficiency low, but long-term high-temperature aging will make the parent material grains coarse and reduce the performance of the parent material.

[0004] The invention provides a method for synchronous rapid carburizing during high-energy beam welding of molybdenum alloy, which can perform rapid synchronous carburizing during high-energy beam welding of molybdenum alloy. Summary of the invention

[0005] The purpose of the present invention is to provide a method for synchronous rapid carburizing during high-energy beam welding of molybdenum alloys, which can rapidly and synchronously carburize the welding area during high-energy beam welding, greatly improving the carburizing efficiency and improving the mechanical properties of the molybdenum alloy welded joints.

[0006] To achieve the above object, the method for synchronous rapid carburizing during high energy beam welding of molybdenum alloys described in the present invention is implemented based on the following steps:

[0007] Step 1: pre-treating the welding interface of the high-energy beam welded parts, wherein the parts are made of molybdenum or / and molybdenum alloy;

[0008] Step 2: sputtering a layer of carbon film on the molybdenum or molybdenum alloy welding interface using magnetron sputtering technology;

[0009] Step 3: Control relevant parameters and weld the processed molybdenum or / and molybdenum alloy sample by high-energy beam welding, so that the weld joint can be quickly and synchronously carburized while high-energy beam welding the molybdenum or / and molybdenum;

[0010] Furthermore, the welded parts in step 1 may be in the form of thin plates, thin-walled tubes or other complex components.

[0011] Furthermore, the specific operation of pre-treating the welding interface in step one is: grinding and polishing the welding interface of the parts to be welded, and then immersing the polished parts seams in an acetone solution for ultrasonic cleaning, wherein the number of ultrasonic cleanings is greater than or equal to 3, and the acetone solution is replaced after each ultrasonic cleaning, and each cleaning time is greater than or equal to 10 minutes, and then the parts are blown dry.

[0012] Furthermore, in step 2, the magnetron sputtering power is 200W, and the sputtering time can be 0 to 4 hours and is not 0. The thickness of the carbon film is generally not limited, and can be a thin layer with a thickness of nanometer to micrometer level as required.

[0013] Furthermore, the high energy beam welding in step three includes argon shielded / vacuum laser welding and vacuum electron beam welding.

[0014] Furthermore, the tensile properties of the joints welded using this method are improved by 200% to 220%.

[0015] The present invention has the following beneficial effects:

[0016] The method for synchronous rapid carburizing during high-energy beam welding of molybdenum alloys described in the present invention is to pre-treat the welding interface of molybdenum and molybdenum alloy parts during high-energy beam welding. Then, a layer of carbon film is sputtered on the molybdenum or / and molybdenum alloy welding interface by magnetron sputtering technology; finally, the treated molybdenum or molybdenum alloy sample is welded by controlling relevant parameters by high-energy beam welding. At this time, the molten pool can be stirred to make the sputtered carbon atoms evenly distributed in the welding molten pool, so as to achieve the purpose of rapid synchronous carburizing during high-energy beam welding, and greatly improve the mechanical properties of the molybdenum or / and molybdenum alloy joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the principle diagram of magnetron sputtering carbon film on the interface of parts to be welded;

[0018] Figure 2 Schematic diagram of high energy beam welding of sputtered carbon film;

[0019] Figure 3 The hardness of the welded joints of carbon film samples after different magnetron sputtering times. Among them, 21mAC=0 is the Vickers hardness of the joint directly welded without magnetron sputtering; 21mAC=2h is the Vickers hardness of the joint welded after magnetron sputtering for 2 hours; 21mAC=4h is the Vickers hardness of the joint welded after magnetron sputtering for 4 hours.

[0020] Figure 4The tensile strength of the welded joints of carbon film samples after different magnetron sputtering times. Among them, 21mA C=0 is the tensile strength of the joint directly welded without magnetron sputtering; 21mA C=2h is the tensile strength of the joint welded after magnetron sputtering for 2 hours; 21mA C=4h is the tensile strength of the joint welded after magnetron sputtering for 4 hours.

[0021] Figure 5 This is the structure diagram of the tensile test sample;

[0022] Figure 6 is the thickness of the film corresponding to different magnetron sputtering times.

[0023] Figure 7 XRD phase analysis spectra of the films corresponding to different magnetron sputtering times. DETAILED DESCRIPTION

[0024] The present invention is described in detail below with reference to the accompanying drawings and embodiments, but the present invention is not limited to the following embodiments.

[0025] The method for synchronous rapid carburizing during high-energy beam welding of molybdenum alloys according to the present invention comprises the following steps:

[0026] 1) Pre-treating the welding interface of high-energy beam welded parts, wherein the material of the parts is molybdenum or molybdenum alloy;

[0027] 2) sputtering a carbon film on the molybdenum or molybdenum alloy welding interface using magnetron sputtering technology;

[0028] 3) Control relevant parameters and weld the processed molybdenum or molybdenum alloy samples by high-energy beam welding, so that the weld joint can be quickly and synchronously carburized while the molybdenum alloy is welded by high-energy beam.

[0029] The welded parts in step 1) can be thin plates, thin-walled tubes or other complex components.

[0030] The specific operation of pre-treating the welding interface in step 1) is: grinding and polishing the welding interface of the parts to be welded, and then immersing the polished parts seams in an acetone solution for ultrasonic cleaning, wherein the number of ultrasonic cleanings is greater than or equal to 3, and the acetone solution is replaced after each ultrasonic cleaning, and each cleaning time is greater than or equal to 10 minutes, and then the parts are blown dry.

[0031] In step 2), the magnetron sputtering power is 200 W, and the sputtering time is 0 to 4 hours.

[0032] Step 3) Medium and high energy beam welding includes argon shielded / vacuum laser welding and vacuum electron beam welding.

[0033] Example 1

[0034] Taking the electron beam welded joint of commercial molybdenum sheet as an example, the size is 50*30*1.5㎜, the welding interface is in the width direction, and the steps of electron beam welding and rapid synchronous carburizing are as follows:

[0035] Step 1: Grind the welding interface with 240#, 400#, 800#, and 1200# sandpaper in turn, and then soak the polished tensile specimen in acetone solution, and then use ultrasonic cleaning at least three times, replace the acetone solution after each cleaning, and each cleaning time is not less than 10 minutes. Finally, blow dry the specimen for standby use, wherein;

[0036] Step 2: magnetron sputtering carbon film on the polished welding interface, such as Figure 1 The sputtering power is 200W, the sputtering time is 2h and 4h respectively, and the corresponding XRD phase analysis spectrum of the film is shown in Figure 7 ;

[0037] Step 3: Electron beam welding is performed on the thin plates sputtered for different times using the same process, wherein the welding is butt welding, such as Figure 2 Its working parameters are: acceleration voltage 55KV, focusing beam current 668mA, welding speed 900mm / min, welding beam current 21mA;

[0038] The hardness of the samples welded after different sputtering times was measured using a Vickers hardness tester, where BM is the base metal area, HAZ is the heat affected zone, and FZ is the molten pool area. The hardness results are as follows: Figure 3 As shown in the figure, the hardness of the molten pool area of ​​the sample that was rapidly and synchronously carburized by electron beam welding was significantly higher than that of the sample that was not carburized, while the hardness of the heat-affected zone and the base material remained basically unchanged. Further tensile tests were performed on the samples welded after different sputtering times (see the size diagram for details). Figure 5 ), the stretching result is as follows Figure 4 As shown, the average tensile strength of the welds welded after magnetron sputtering carbon film for 2h and 4h are 418.5MPa and 387.7MPa respectively; the strength of the original electron beam welded weld without any treatment is 127.5MPa, and the strength of electron beam welding synchronous carburizing is increased by 200% to 220% compared with the strength of the original electron beam welded weld.

[0039] In summary, the present invention can realize rapid synchronous carburizing during high-energy beam welding, greatly improve the carburizing efficiency, and achieve the purpose of significantly enhancing the hardness and tensile strength of molybdenum and molybdenum alloy joints.

Claims

1. A method for simultaneous rapid carburizing during high energy beam welding of molybdenum alloys, characterized in that: The following steps are involved: Step 1: pre-treating the welding interface of the high-energy beam welded parts, wherein the parts are made of molybdenum or / and molybdenum alloy; Step 2: sputtering a layer of carbon film on the molybdenum or molybdenum alloy welding interface using magnetron sputtering technology; Step 3: Control relevant parameters and weld the processed molybdenum or / and molybdenum alloy samples by high-energy beam welding, so that the weld joint can be quickly and synchronously carburized while high-energy beam welding the molybdenum or / and molybdenum.

2. The method according to claim 1, characterized in that The welded parts in step 1 may be in the form of thin plates, thin-walled tubes or other complex hardware.

3. The method according to claim 1, characterized in that The specific operation of pre-treating the welding interface in step 1 is: grinding and polishing the welding interface of the parts to be welded, and then immersing the polished parts seams in an acetone solution for ultrasonic cleaning, wherein the number of ultrasonic cleanings is greater than or equal to 3, and the acetone solution is replaced after each ultrasonic cleaning, and each cleaning time is greater than or equal to 10 minutes, and then the parts are blown dry.

4. The method according to claim 1, characterized in that In step 2, the magnetron sputtering power is 200 W, and the sputtering time is 0 to 4 hours and is not 0.

5. The method according to claim 1, characterized in that In step three, high energy beam welding includes argon shielded / vacuum laser welding and vacuum electron beam welding.

6. A welded part prepared by the method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method for improving strength of molybdenum and molybdenum alloy fusion welding seam through solid carburization mode

    CN109943802A

  • Preparation method for mechanical chemical carburizing treatment hard abrasion-resistant coating on surface of nickel chromium molybdenum steel

    CN110629155A

  • Method for improving molybdenum and molybdenum alloy laser welding joint in nitrogen alloying manner

    CN112222614A

  • Method for improving weldability of molybdenum and molybdenum alloy through nitriding

    CN112222615A

  • Electron beam welding molybdenum to obtain vacuum tight weld - where joint is coated with other metals before welding

    DE2543444A1

Cited By

  • Method for using C / Re composite foil for electron beam welding of molybdenum joint

    CN119457375A