Preparation method of high-temperature anti-oxidation coating on surface of aviation blade

Depositing TiAlCrNbSiY six-membered alloy coating on TiAl alloy blades through high-energy pulse magnetron sputtering method solves the problems of poor high-temperature oxidation resistance and complex process of aviation blades, achieving efficient high-temperature oxidation resistance and strong binding force, suitable for Large-scale industrial application.

CN118957518APending Publication Date: 2024-11-15XIAN SURFACE MATERIAL PROTECTION CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411038446.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art has problems such as poor performance, easy fatigue and cumbersome processes in improving the high-temperature oxidation resistance of TiAl alloy aviation blades, especially the poor fatigue resistance and corrosion resistance of plasma spraying methods, and the electron beam physical vapor deposition equipment is complex and costly. .

Method used

The TiAlCrNbSiY six-membered alloy coating was deposited on TiAl alloy blades by high-energy pulse magnetron sputtering. Through cleaning, sputtering and multiple surface plasma etching, the mechanical properties and density of the hard film of the coating were significantly improved. Improves bond strength with the matrix.

Benefits of technology

It significantly improves the mechanical properties and uniformity of the hard film of the six-member alloy coating, has good high-temperature oxidation resistance, solves the problems of poor coating performance and easy fatigue and cumbersome process, and is simple in process and low in cost. , suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957518A_ABST
    Figure CN118957518A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-temperature anti-oxidation coating on the surface of an aviation blade. The method comprises the following steps: 1, cleaning a TiAl alloy blade; secondly, an oxide layer on the surface of the TiAl alloy blade is subjected to sputtering cleaning; thirdly, the TiAl alloy blade subjected to sputtering cleaning is subjected to multiple times of surface plasma etching; and 4, the TiAl alloy blade subjected to multiple times of surface plasma etching in the step 3 is subjected to magnetron sputtering, and the TiAlCrNbSiY coating is prepared. According to the method, the TiAlCrNbSiY six-element alloy coating is deposited on the TiAl alloy blade through the high-energy pulse magnetron sputtering method, high ionization of sputtering ions is improved, the mechanical property of a hard film of the six-element alloy coating is remarkably improved, the uniformity of performance distribution is improved, meanwhile, the TiAlCrNbSiY six-element alloy coating is compact and continuous in structure, the bonding strength with a base body is high, and the service life of the TiAlCrNbSiY six-element alloy coating is prolonged. Therefore, the material has good high-temperature oxidation resistance and is suitable for the field of aviation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature anti-oxidation coating preparation, and in particular relates to a method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade. Background Art

[0002] TiAl-based alloy is an intermetallic compound with low density and high melting point. Compared with titanium alloy and nickel-based high-temperature alloy, γ-TiAl-based alloy has low density (3.9g / cm 3 ), large elastic modulus and high specific strength, it has become one of the most competitive alternative materials for nickel-based high-temperature alloys for aircraft engines. In recent years, TiAl alloys have been used in some low-pressure turbine blades of aircraft engines, but the limited oxidation resistance of TiAl alloys when they are in service at high temperatures above 800°C has become an obstacle to their further application.

[0003] At present, the high-temperature oxidation resistance of TiAl alloy can be improved by alloying and preparing surface coating. However, the overall use of alloy technology has a long research cycle, large workload, high research cost and high risk. Overall alloying will also seriously affect the comprehensive mechanical properties of TiAl alloy, especially increasing the brittleness of the alloy and reducing the fatigue performance of the alloy. Surface treatment technology can organically combine the characteristics of the substrate and the coating to give full play to the comprehensive advantages of the two types of materials. At present, the preparation methods of aviation blade surface coating mainly include: thermal spraying (plasma spraying, flame spraying, explosion spraying), physical vapor deposition (electron beam physical vapor deposition, ion plating, magnetron sputtering), etc. Among them, plasma spraying and electron beam physical vapor deposition are the most widely used, but the fatigue resistance and corrosion resistance of the plasma spraying method are poor, and fatigue shedding is easy to occur under high temperature environment and cyclic stress; electron beam physical vapor deposition has the problems of complex equipment, high price, cumbersome process and relatively low production efficiency. High-energy pulse magnetron sputtering is a type of physical vapor deposition. High-energy pulse magnetron sputtering has the following advantages: 1. Fast deposition speed, low substrate temperature rise, and little damage to the film layer; 2. For most materials, sputtering can be achieved as long as the target material can be made; 3. The film obtained by sputtering has a good bond with the substrate; 4. The film obtained by sputtering has high purity, good density, and good film uniformity; 5. The sputtering process has good repeatability, and a film layer with uniform thickness can be obtained on a large-area substrate; 6. It is conducive to the sputtering of high-melting-point metals or complex alloys. Therefore, the study uses the method of high-energy pulse magnetron sputtering to realize the preparation of multi-alloy high-temperature anti-oxidation coating on the surface of TiAl blades. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade in view of the deficiencies of the above-mentioned prior art. The method deposits a TiAlCrNbSiY hexa-alloy coating on a TiAl alloy blade by a high-energy pulse magnetron sputtering method, thereby increasing the high ionization of sputtered ions, significantly improving the mechanical properties of the hard film of the hexa-alloy coating, and improving the uniformity of the performance distribution. At the same time, the TiAlCrNbSiY hexa-alloy coating has a dense and continuous structure and a high bonding strength with the substrate, thereby having good high-temperature oxidation resistance, and solving the problems of poor performance, easy fatigue shedding, and complicated process in the preparation of aviation blade surface coatings by the existing method.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade, characterized in that the method comprises the following steps:

[0006] Step 1, cleaning the TiAl alloy blade until there is no dust, oil stain, water stain or other impurities on the surface, then washing and drying to obtain a prefabricated TiAl blade;

[0007] Step 2: Place the TiAl alloy blade and target material prepared in step 1 into the reaction chamber of the high-energy pulse magnetron sputtering equipment, and turn on the vacuum system to make the pressure in the reaction chamber not exceed 5×10 -3 Pa, then Ar gas is introduced, and then bias voltage is applied to the TiAl alloy blade, and a high-energy pulsed magnetron sputtering power supply is turned on to sputter and clean the oxide layer on the surface of the TiAl alloy blade;

[0008] Step 3, turn off the high-energy pulse magnetron sputtering power supply, turn on the plasma power supply and control the voltage to 200V-300V, then adjust the bias voltage and time to perform multiple surface plasma etching on the TiAl alloy blade after sputtering cleaning in step 2 to enhance the nucleation points on the surface of the TiAl alloy blade;

[0009] Step 4: Turn on the high-energy pulsed magnetron sputtering power supply, and use the target material to perform magnetron sputtering on the TiAl alloy blades that have been subjected to multiple surface plasma etchings in step 3 to prepare a TiAlCrNbSiY coating.

[0010] The above-mentioned method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade is characterized in that the cleaning process described in step one is: first use an industrial degreasing cleaning agent for degreasing cleaning, and then use deionized water and ethanol solution in sequence to ultrasonically clean for 15 minutes to 20 minutes at 25°C to 40°C.

[0011] The above-mentioned method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade is characterized in that, in step 2, Ar gas is introduced to make the pressure in the reaction chamber 1Pa~3Pa, and then the TiAl alloy blade is biased to -500V~-1000V; during the sputtering cleaning process, the temperature of the coating chamber is 180℃~300℃, and the sputtering cleaning time is 10min~20min.

[0012] The above-mentioned method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade is characterized in that the target material in step 2 is a TiAlCrNbSiY hexavalent alloy, and the high-energy pulsed magnetron sputtering power supply voltage is 300V to 500V.

[0013] The above-mentioned method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade is characterized in that the number of surface plasma etching described in step three is three times: the first etching bias is 100V, the time is 200s, the second etching bias is 200V, the time is 30min, and the third etching bias is 250V, the time is 300s. The present invention removes impurities on the surface of the TiAl alloy blade by etching; at the same time, the etching intensity and depth are different depending on the bias voltage used. The present invention uses a method of gradually increasing the bias voltage for etching. On the one hand, it avoids arcing on the blade surface caused by directly using a large bias voltage, and on the other hand, it is conducive to the generation of various complex micro-nano nucleation points on the blade surface, effectively improving the bonding force of the subsequent TiAlCrNbSiY coating.

[0014] The above-mentioned method for preparing a high-temperature anti-oxidation coating on the surface of an aviation blade is characterized in that the power supply voltage of the magnetron sputtering in step four is 300V~500V, the workpiece bias is -100V~-150V, the time is 90min~120min, and the vacuum degree of the reaction chamber during the magnetron sputtering process is 0.5Pa~1Pa, and the temperature is 150℃~300℃.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] 1. The present invention first performs surface cleaning pretreatment including surface cleaning, sputtering cleaning and etching on the TiAl alloy blade, and then uses a high-energy pulse magnetron sputtering method to deposit a TiAlCrNbSiY hexa-alloy coating on the cleaned TiAl alloy blade. The discharge characteristics are changed by pulse power regulation to improve the high ionization of sputtered ions. Through momentum conversion, TiAlCrNbSiY hexa-alloy atoms are sputtered and deposited on the surface of the TiAl alloy blade to form a hexa-alloy coating, which significantly improves the mechanical properties of the hexa-alloy coating hard film and improves the uniformity of performance distribution, thereby forming a dense and highly adhesive coating on a large area of ​​TiAl alloy blades.

[0017] 2. The present invention adopts TiAlCrNbSiY hexametal alloy as a target material to prepare a TiAlCrNbSiY coating, wherein the corresponding proportions of Al, Cr, Si and Nb ensure the formation of a dense and continuous Al2O3 film on the surface of the coating, while also inhibiting the competitive oxidation of Ti. The introduction of Si element improves the toughness of the coating, while the addition of trace element Y increases the viscosity of the coating and improves the bonding strength between the coating and the substrate. The above elements work together to ensure that the Ti-Al-Cr-Nb-Si-Y hexametal alloy coating has good high-temperature oxidation resistance.

[0018] 3. The present invention performs multiple surface plasma etching on the TiAl alloy blade after sputtering cleaning in advance, and prepares a micro-nano structure on the surface of the TiAl alloy blade, thereby enhancing the nucleation points on the surface of the TiAl alloy blade, thereby effectively improving the bonding strength between the coating and the substrate TiAl alloy blade, and the stable film-base bonding strength also helps to improve the high-temperature oxidation resistance of the coating.

[0019] 4. The preparation process of the present invention is simple, operable, and low in production cost, which is conducive to large-scale industrial application.

[0020] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a SEM scan image of the TiAlCrNbSiY coating prepared in Example 1 of the present invention.

[0022] Figure 2 This is a graph showing the weight gain of the TiAlCrNbSiY coatings prepared in Examples 2 to 3 of the present invention after oxidation at 850°C for 200 hours. DETAILED DESCRIPTION

[0023] Example 1

[0024] This embodiment includes the following steps:

[0025] Step 1: Clean the TiAl alloy blade until there is no dust, oil, water stains or other impurities on the surface, then clean and dry to obtain a prefabricated TiAl blade; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil, then use deionized water and ethanol solution in turn to ultrasonicate for 15 minutes at 25°C to 40°C;

[0026] Step 2: Place the TiAl alloy blade and target material prepared in step 1 into the reaction chamber of the high-energy pulse magnetron sputtering equipment, and turn on the vacuum system to make the pressure in the reaction chamber not exceed 5×10 -3Pa, then Ar gas is introduced to make the pressure in the reaction chamber 1Pa, and then the TiAl alloy blade is biased to -500V, and the high-energy pulse magnetron sputtering power supply is turned on to sputter and clean the oxide layer on the surface of the TiAl alloy blade; the target material is Ti 0.1 Al 0.6 Cr 0.1 Nb 0.05 Si 0.1 Y 0.05 Hexavalent alloy, high energy pulse magnetron sputtering power supply voltage is 300V; the temperature of the coating chamber during the sputtering cleaning process is 200°C, and the sputtering cleaning time is 15min;

[0027] Step 3, turn off the high-energy pulse magnetron sputtering power supply, turn on the plasma power supply and control the voltage to 200V, then adjust the bias voltage and time to perform three surface plasma etching on the TiAl alloy blade after sputtering cleaning in step 2 to enhance the nucleation points on the surface of the TiAl alloy blade; the three surface plasma etchings are: the first etching bias is 100V, the time is 200s, the second etching bias is 200V, the time is 30min, and the third etching bias is 250V, the time is 300s;

[0028] Step 4, turn on the high-energy pulsed magnetron sputtering power supply, and use the target material to magnetron sputter the TiAl alloy blades after multiple surface plasma etching in step 3 to prepare a TiAlCrNbSiY coating; the power supply voltage of the magnetron sputtering is 300V, the workpiece bias is -150V, the time is 90min, and the vacuum degree of the reaction chamber during the magnetron sputtering process is 0.5Pa and the temperature is 300℃.

[0029] Figure 1 The SEM scanning image of the TiAlCrNbSiY coating of this embodiment is shown in FIG. Figure 1 It can be seen that the TiAlCrNbSiY coating prepared in this embodiment is evenly distributed, has no defects such as pores and cracks, and has good compactness.

[0030] Example 2

[0031] This embodiment includes the following steps:

[0032] Step 1: Clean the TiAl alloy blade until there is no dust, oil stain, water stain or other impurities on the surface, then clean and dry to obtain a prefabricated TiAl blade; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil, then use deionized water and ethanol solution in turn to ultrasonicate for 20 minutes at 25°C to 40°C;

[0033] Step 2: Place the TiAl alloy blade and target material prepared in step 1 into the reaction chamber of the high-energy pulse magnetron sputtering equipment, and turn on the vacuum system to make the pressure in the reaction chamber not exceed 5×10 -3 Pa, then Ar gas is introduced to make the pressure in the reaction chamber 2Pa, and then the TiAl alloy blade is biased to -1000V, and the high-energy pulse magnetron sputtering power supply is turned on to sputter and clean the oxide layer on the surface of the TiAl alloy blade; the target material is Ti 0.2 Al 0.5 Cr 0.15 Nb 0.04 Si 0.1 Y 0.01 Hexa-element alloy, high-energy pulse magnetron sputtering power supply voltage is 400V; the temperature of the coating chamber during the sputtering cleaning process is 180°C, and the sputtering cleaning time is 20min;

[0034] Step 3, turn off the high-energy pulse magnetron sputtering power supply, turn on the plasma power supply and control the voltage to 200V, then adjust the bias voltage and time to perform three surface plasma etching on the TiAl alloy blade after sputtering cleaning in step 2 to enhance the nucleation points on the surface of the TiAl alloy blade; the three surface plasma etchings are: the first etching bias is 100V, the time is 200s, the second etching bias is 200V, the time is 30min, and the third etching bias is 250V, the time is 300s;

[0035] Step 4, turn on the high-energy pulse magnetron sputtering power supply, and use the target material to magnetron sputter the TiAl alloy blades after multiple surface plasma etching in step 3 to prepare a TiAlCrNbSiY coating; the power supply voltage of the magnetron sputtering is 400V, the workpiece bias is -150V, the time is 100min, and the vacuum degree of the reaction chamber during the magnetron sputtering process is 0.7Pa and the temperature is 150°C.

[0036] Example 3

[0037] This embodiment includes the following steps:

[0038] Step 1: Clean the TiAl alloy blade until there is no dust, oil stain, water stain or other impurities on the surface, then clean and dry to obtain a prefabricated TiAl blade; the cleaning process is: first use an industrial degreasing cleaning agent to remove oil, then use deionized water and ethanol solution in turn to ultrasonicate for 20 minutes at 25°C to 40°C;

[0039] Step 2: Place the TiAl alloy blade and target material prepared in step 1 into the reaction chamber of the high-energy pulse magnetron sputtering equipment, and turn on the vacuum system to make the pressure in the reaction chamber not exceed 5×10 -3Pa, then Ar gas is introduced to make the pressure in the reaction chamber 3Pa, and then the TiAl alloy blade is biased to -800V, and the high-energy pulse magnetron sputtering power supply is turned on to sputter and clean the oxide layer on the surface of the TiAl alloy blade; the target material is Ti 0.3 Al 0.4 Cr 0.15 Nb 0.04 Si 0.1 Y 0.01 Hexavalent alloy, high energy pulse magnetron sputtering power supply voltage is 500V; the temperature of the coating chamber during the sputtering cleaning process is 300°C, and the sputtering cleaning time is 10min;

[0040] Step 3, turn off the high-energy pulse magnetron sputtering power supply, turn on the plasma power supply and control the voltage to 300V, then adjust the bias voltage and time to perform three surface plasma etching on the TiAl alloy blade after sputtering cleaning in step 2 to enhance the nucleation points on the surface of the TiAl alloy blade; the three surface plasma etchings are: the first etching bias is 100V, the time is 200s, the second etching bias is 200V, the time is 30min, and the third etching bias is 250V, and the time is 300s;

[0041] Step 4, turn on the high-energy pulse magnetron sputtering power supply, and use the target material to perform magnetron sputtering on the TiAl alloy blades that have undergone multiple surface plasma etching in step 3 to prepare a TiAlCrNbSiY coating; the power supply voltage of the magnetron sputtering is 500V, the workpiece bias is -100V, the time is 120min, and the vacuum degree of the reaction chamber during the magnetron sputtering process is 1Pa and the temperature is 250°C.

[0042] Figure 2 The weight gain curve of the TiAlCrNbSiY coating prepared in Examples 2 to 3 of the present invention after oxidation at 850°C for 200h. Figure 2 It can be seen that the TiAlCrNbSiY coating on the surface of the TiAl alloy blade substrate has an obvious anti-oxidation effect.

[0043] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a high temperature anti-oxidation coating on the surface of an aviation blade, characterized in that: The method comprises the following steps: Step 1, cleaning the TiAl alloy blade until there is no dust, oil stain, water stain or other impurities on the surface, then washing and drying to obtain a prefabricated TiAl blade; Step 2: Place the TiAl alloy blade and target material prepared in step 1 into the reaction chamber of the high-energy pulse magnetron sputtering equipment, and turn on the vacuum system to make the pressure in the reaction chamber not exceed 5×10 -3 Pa, then Ar gas is introduced, and then bias voltage is applied to the TiAl alloy blade, and a high-energy pulsed magnetron sputtering power supply is turned on to sputter and clean the oxide layer on the surface of the TiAl alloy blade; Step 3, turn off the high-energy pulse magnetron sputtering power supply, turn on the plasma power supply and control the voltage to 200V-300V, then adjust the bias voltage and time to perform multiple surface plasma etching on the TiAl alloy blade after sputtering cleaning in step 2 to enhance the nucleation points on the surface of the TiAl alloy blade; Step 4: Turn on the high-energy pulsed magnetron sputtering power supply, and use the target material to perform magnetron sputtering on the TiAl alloy blades that have been subjected to multiple surface plasma etchings in step 3 to prepare a TiAlCrNbSiY coating.

2. The method for preparing a high temperature anti-oxidation coating on the surface of an aviation blade according to claim 1, characterized in that: The cleaning process in step 1 is: first use an industrial degreasing cleaning agent for degreasing cleaning, and then use deionized water and ethanol solution in turn for ultrasonic cleaning at 25° C. to 40° C. for 15 min to 20 min respectively.

3. The method for preparing a high temperature anti-oxidation coating on the surface of an aviation blade according to claim 1, characterized in that: In step 2, Ar gas is introduced to make the pressure in the reaction chamber 1Pa~3Pa, and then the TiAl alloy blade is biased to -500V~-1000V; during the sputtering cleaning process, the temperature of the coating chamber is 180℃~300℃, and the sputtering cleaning time is 10min~20min.

4. The method for preparing a high temperature anti-oxidation coating on the surface of an aviation blade according to claim 1, characterized in that: The target material in step 2 is TiAlCrNbSiY hexametal alloy, and the power supply voltage of the high-energy pulse magnetron sputtering is 300V to 500V.

5. The method for preparing a high temperature anti-oxidation coating on the surface of an aviation blade according to claim 1, characterized in that: The surface plasma etching in step three is performed three times: the first etching bias is 100V, the time is 200s, the second etching bias is 200V, the time is 30min, and the third etching bias is 250V, the time is 300s.

6. The method for preparing a high temperature anti-oxidation coating on the surface of an aviation blade according to claim 1, characterized in that: The power supply voltage of the magnetron sputtering described in step 4 is 300V~500V, the workpiece bias is -100V~-150V, the time is 90min~120min, the vacuum degree of the reaction chamber during the magnetron sputtering process is 0.5Pa~1Pa, and the temperature is 150℃~300℃.

Citation Information

Cited By

  • Titanium-aluminum alloy blade high-temperature coating homogenizing deposition method based on profiling fastening clamp

    CN120738610A