Manufacturing method of low pressure chemical vapor deposition (LPCVD) in-situ doped polycrystalline silicon film

By adjusting the temperature and gas flow in the LPCVD furnace tube to form a polycrystalline silicon film layer, the defect problems caused by many slots and small spacing are solved, and the low-defect polycrystalline silicon film film formation process is achieved, maintaining the stability of resistivity.

CN118957533APending Publication Date: 2024-11-15HUA HONG SEMICON WUXI LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410868361.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When LPCVD in-situ doped polysilicon furnace tubes use crystal boats with more slots and smaller slot spacing, serious problems of bulging or buried-type granular defects will occur.

Method used

By adjusting the temperature and gas flow in the furnace tube cavity, a doped amorphous and doped polysilicon film layer is formed to reduce the number of defects. The specific steps include passing silane and phosphane into a first polysilicon film layer at 520°C to 540°C, and further forming a second polysilicon film layer at 560°C to 580°C, controlling cavity pressure and gas deposition time.

Benefits of technology

The process defects of LPCVD in-situ doped polysilicon furnace tubes in crystal boats with more slots and smaller slot spacing are effectively reduced, and the preset range of test resistivity is maintained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957533A_ABST
    Figure CN118957533A_ABST
Patent Text Reader

Abstract

The invention provides a method for manufacturing an LPCVD (low pressure chemical vapor deposition) in-situ doped polycrystalline silicon film, which comprises the following steps: providing a furnace tube for LPCVD in-situ doped polycrystalline silicon, arranging a plurality of crystal boats with slot spacing smaller than or equal to a target distance in a cavity in the furnace tube, and arranging a substrate on the crystal boats; the temperature in the cavity is adjusted to be 520-540 DEG C, then silane and phosphine are introduced into the cavity, and a doped first polycrystalline silicon film layer is formed on the wafer; and adjusting the temperature in the cavity to be 560-580 DEG C, then introducing silane and phosphorane into the cavity, and forming a doped second polycrystalline silicon film layer on the first polycrystalline silicon film layer, so that the number of defects on the first polycrystalline silicon film layer and the number of defects on the second polycrystalline silicon film layer are lower than the target number. According to the invention, the process defects occurring when the LPCVD in-situ doped polycrystalline silicon furnace tube adopts a wafer boat with more slot positions and smaller slot position spacing can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for manufacturing a LPCVD in-situ doped polysilicon film. Background Art

[0002] The vertical furnace tube machine is one of the important process equipment in the front process of semiconductor production line. It is used for diffusion, oxidation, annealing and alloying processes in industries such as large-scale integrated circuits, discrete devices, power electronics, optoelectronic devices and optical fibers.

[0003] Due to the limited height of the clean room and the limited height design of the vertical furnace, in order to more effectively improve the utilization efficiency of the machine, a wafer boat with more slots and smaller slot spacing can be used to load more wafers. This also means that the spacing between wafers on the wafer boat is smaller, but this will bring various process problems.

[0004] See also Figure 2 LPCVD in-situ doped polysilicon furnace tubes will have serious defects when using a wafer boat with more slots and smaller slot spacing (the wafer boat height is the same in the embodiment, the slot spacing is increased from 6.5mm-->5.32mm, and the number of slots is increased from 143-->170). Figure 2 The defects are specifically manifested as bulges or buried layer type granular defects, with sizes ranging from about 0.2-2.0um.

[0005] In order to solve the above problems, it is necessary to propose a new method for manufacturing LPCVD in-situ doped polysilicon thin film. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a method for manufacturing LPCVD in-situ doped polysilicon thin film, which is used to solve the problem that serious defects will occur in the prior art LPCVD in-situ doped polysilicon furnace tube when using a crystal boat with more slots and smaller slot spacing.

[0007] To achieve the above-mentioned and other related purposes, the present invention provides a method for manufacturing a LPCVD in-situ doped polysilicon thin film, comprising:

[0008] Step 1, providing a furnace tube for LPCVD in-situ doping of polysilicon, wherein a cavity in the furnace tube is provided with a plurality of wafer boats with slot spacing less than or equal to a target distance, and a substrate is provided on the wafer boat;

[0009] Step 2: adjusting the temperature in the chamber to 520° C.-540° C., then introducing silane and phosphine into the chamber to form a first amorphous doped polysilicon film layer on the wafer;

[0010] Step three, adjusting the temperature in the cavity to 560° C.-580° C., then introducing silane and phosphine into the cavity to form a doped second polysilicon film layer on the first polysilicon film layer, so that the number of defects on the first and second polysilicon film layers is lower than the target number.

[0011] Preferably, the substrate in step 1 comprises a bulk semiconductor substrate or a silicon-on-insulator (SOI) substrate.

[0012] Preferably, the step 2 further includes the step of forming an undoped film layer on the substrate before forming the first polysilicon film layer.

[0013] Preferably, the undoped film layer can be diffused into by phosphorus atoms in the doped polysilicon film layer.

[0014] Preferably, the influence of the undoped film layer on the resistivity test is within a preset range.

[0015] Preferably, the cavity is provided with a plurality of wafer boats with a slot spacing less than or equal to 8.5 mm.

[0016] Preferably, the pressure in the cavity in step 2 is 0.6 to 0.8 Torr.

[0017] Preferably, in step 2, the gas flow rate of the silane is 1.0-1.4 slm, the gas flow rate of the phosphine is 80-150 sccm, and the deposition time is 5-12 min.

[0018] Preferably, in step 3, the gas flow rate of the silane is 1.0-1.4 slm, the gas flow rate of the phosphine is 80-150 sccm, and the deposition time is 150-200 min.

[0019] Preferably, the pressure in the cavity in step three is 0.2 to 0.4 Torr.

[0020] Preferably, in step three, the thickness of the first polysilicon film layer is less than 10% of the total thickness of the first and second polysilicon film layers.

[0021] Preferably, the defect in step three is a bulge or buried layer type granular defect.

[0022] As described above, the method for manufacturing the LPCVD in-situ doped polysilicon thin film of the present invention has the following beneficial effects:

[0023] The present invention can reduce the process defects that occur when a LPCVD in-situ doped polysilicon furnace tube uses a crystal boat with more slots and smaller slot spacing. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Shown is a schematic diagram of a wafer boat of the prior art;

[0025] Figure 2 Shown is a schematic diagram of defect formation in the prior art;

[0026] Figure 3 Shown is a schematic diagram of the process flow of the present invention;

[0027] Figure 4 Shown is a schematic diagram comparing the number of defects of the present invention and the prior art;

[0028] Figure 5 It is a schematic diagram showing the comparison of the test resistivity of the present invention and the prior art. DETAILED DESCRIPTION

[0029] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0030] See also Figure 1 The present invention provides a method for manufacturing a LPCVD in-situ doped polysilicon thin film, comprising:

[0031] Step 1, providing a furnace tube for LPCVD in-situ doping of polysilicon, wherein a cavity in the furnace tube is provided with a plurality of wafer boats with slot spacing less than or equal to a target distance, and a substrate is provided on the wafer boat;

[0032] In some embodiments, the substrate in step one includes a bulk semiconductor substrate or a silicon-on-insulator (SOI) substrate. The SOI substrate includes an insulator layer located below a thin semiconductor layer as an active layer of the SOI substrate. The semiconductor of the active layer and the bulk semiconductor typically include crystalline semiconductor material silicon, but may also include one or more other semiconductor materials, such as germanium, silicon-germanium alloys, compound semiconductors (e.g., GaAs, AlAs, InAs, GaN, AlN, etc.) or their alloys (e.g., GaxAl1-xAs, GaxAl1-xN, InxGa1-xAs, etc.), oxide semiconductors (e.g., ZnO, SnO2, TiO2, Ga2O3, etc.) or combinations thereof. The semiconductor material may be doped or undoped. Other substrates that may be used include multilayer substrates, gradient substrates, or mixed orientation substrates.

[0033] In some embodiments, the step 2 further includes forming an undoped film layer on the substrate before forming the first polysilicon film layer. For example, the undoped film layer may be a gate oxide layer.

[0034] In some embodiments, the undoped film layer can be diffused into by phosphorus atoms in the doped polysilicon film layer.

[0035] In some embodiments, the influence of the undoped film layer on the resistivity test is within a preset range.

[0036] In some embodiments, the cavity in step 1 is provided with a plurality of wafer boats with a slot spacing less than or equal to 8.5 mm.

[0037] For example, the specifications of the wafer boat used are: silicon carbide material, 988mm length, 170 slots, and 5.32mm slot spacing.

[0038] Step 2: adjusting the temperature in the chamber to 520° C.-540° C., for example, 520° C., 525° C., 530° C., 535° C. or 540° C., and then introducing silane and phosphine into the chamber to form a doped amorphous first polysilicon film layer on the wafer. By further lowering the temperature of the chamber to form the doped amorphous first polysilicon film layer, the formation of defects can be reduced.

[0039] In some embodiments, the pressure in the chamber in step 2 is 0.6 to 0.8 Torr (the chamber pressure in the prior art is about 0.2 Torr), for example, 0.6 Torr, 0.65 Torr, 0.7 Torr, 0.75 Torr or 0.8 Torr.

[0040] In some embodiments, the gas flow rate of silane introduced in step 2 is 1.0-1.4 slm, for example, 1.0 slm, 1.1 slm, 1.2 slm, 1.3 slm or 1.4 slm, the gas flow rate of phosphine introduced is 80-150 sccm, for example, 80 sccm, 90 sccm, 100 sccm, 110 sccm, 120 sccm, 130 sccm, 140 sccm, 150 sccm, and the deposition time is 5-12 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min or 12 min.

[0041] Step three, adjust the temperature in the chamber to 560°C-580°C, for example, 560°C, 565°C, 570°C, 575°C or 580°C, and then introduce silane and phosphine into the chamber to form a doped second polysilicon film layer on the first polysilicon film layer, so that the number of defects on the first and second polysilicon film layers is lower than the target number.

[0042] In some embodiments, the gas flow rate of silane introduced in step three is 1.0-1.4 slm, for example, 1.0 slm, 1.1 slm, 1.2 slm, 1.3 slm or 1.4 slm, the gas flow rate of phosphine introduced is 80-150 sccm, for example, 80 sccm, 90 sccm, 100 sccm, 110 sccm, 120 sccm, 130 sccm, 140 sccm, 150 sccm, and the deposition time is 150-200 min, for example, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min or 150 min.

[0043] In some embodiments, the pressure in the chamber in step 3 is 0.2 to 0.4 Torr, such as 0.2 Torr, 0.3 Torr or 0.4 Torr.

[0044] In some embodiments, the thickness of the first polysilicon film layer in step three is less than 10% of the total thickness of the first and second polysilicon film layers.

[0045] In some embodiments, see Figure 2 The defects in step three are bulge or buried granular defects. When the groove spacing is reduced, the gas flowability is affected. The phosphine containing lone pair electrons has a stronger adsorption capacity, which greatly prioritizes silane to nucleate on the substrate surface, resulting in abnormal defect formation during the film formation process.

[0046] See also Figure 4 , which shows a schematic diagram comparing the number of defects in the embodiment of the present invention and the prior art. The method of the present invention can reduce the process defects that occur when the LPCVD in-situ doped polysilicon furnace tube uses a wafer boat with more slots and smaller slot spacing. At the same time, please refer to Figure 5 The test resistivity of a product sheet of the implementation scheme is equivalent to that of the prior art and is not affected by the formation of the film layer at low temperature.

[0047] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner. Therefore, the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0048] In summary, the present invention can reduce the process defects that occur when the LPCVD in-situ doped polysilicon furnace tube uses a wafer boat with more slots and smaller slot spacing. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.

[0049] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for manufacturing a LPCVD in-situ doped polysilicon thin film, It is characterized in that At least: Step 1, providing a furnace tube for LPCVD in-situ doping of polysilicon, wherein a cavity in the furnace tube is provided with a plurality of wafer boats with slot spacing less than or equal to a target distance, and a substrate is provided on the wafer boat; Step 2: adjusting the temperature in the chamber to 520° C.-540° C., then introducing silane and phosphine into the chamber to form a first amorphous doped polysilicon film layer on the wafer; Step three, adjusting the temperature in the cavity to 560° C.-580° C., then introducing silane and phosphine into the cavity to form a doped second polysilicon film layer on the first polysilicon film layer, so that the number of defects on the first and second polysilicon film layers is lower than the target number.

2. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: The substrate in step 1 includes a bulk semiconductor substrate or a silicon-on-insulator (SOI) substrate.

3. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: The step 2 further includes the step of forming an undoped film layer on the substrate before forming the first polysilicon film layer.

4. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 3, Features: The undoped film layer can be diffused into by phosphorus atoms in the doped polysilicon film layer.

5. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 3, Features: The influence of the undoped film layer on the resistivity test is within a preset range.

6. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: The cavity in step one is provided with a plurality of wafer boats with a slot spacing less than or equal to 8.5 mm.

7. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: The pressure in the chamber in step 2 is 0.6 to 0.8 Torr.

8. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: In step 2, the gas flow rate of the silane is 1.0-1.4 slm, the gas flow rate of the phosphine is 80-150 sccm, and the deposition time is 5-12 min.

9. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: In step 3, the gas flow rate of the silane is 1.0-1.4 slm, the gas flow rate of the phosphine is 80-150 sccm, and the deposition time is 150-200 min.

10. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: The pressure in the chamber in step three is 0.2 to 0.4 Torr.

11. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: In step three, the thickness of the first polysilicon film layer is less than 10% of the total thickness of the first and second polysilicon film layers.

12. The method for manufacturing a LPCVD in-situ doped polysilicon thin film according to claim 1, Features: The defect in step three is a bulge or buried layer type granular defect.