Molybdenum disulfide film on patterned substrate, preparation method and application
By growing the molybdenum disulfide film in situ on the patterned substrate, the problems of pollution and small crystal domain in the traditional transfer method are solved, and large-size and high-quality molybdenum disulfide growth and performance improvement are achieved. The photodetector built is built Better performing.
Patent Information
- Application Number
- CN202411013976.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art easily introduces contamination, wrinkles and damage when transferring molybdenum disulfide to a patterned undulating substrate, resulting in low carrier mobility and low light absorption, and small single crystal domain, which cannot achieve large-area high-quality Monolayer molybdenum disulfide growth.
In situ growth method is used to grow molybdenum disulfide film on the patterned substrate. Through oxygen plasma pretreatment and chemical vapor deposition processes, the single crystal of molybdenum disulfide closely covers the undulating parts of the substrate, avoids voids and bubbles, and achieves large size. , high-quality monolayer molybdenum disulfide growth.
The conformal coverage of the molybdenum disulfide film is achieved, and the carrier mobility and light absorption performance is improved. The built photoconductivity photodetector performs better than traditional methods in response time, light-dark current ratio and detection rate.
Smart Images

Figure CN118957534A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of two-dimensional materials, and more specifically, relates to a molybdenum disulfide film on a patterned substrate, a preparation method and an application thereof. Background Art
[0002] Two-dimensional materials have attracted widespread attention in scientific and engineering research. Among them, molybdenum disulfide (MoS2) has excellent physical properties, such as a direct band gap (1.85 eV) for a single layer, good stability, excellent strain-regulated performance, and high mechanical strength. It is considered to be a potential material for the next generation of electronic and optoelectronic devices. However, due to its low mobility caused by strong phonon scattering and low light absorption caused by its atomically thin size, the performance of electronic and optoelectronic devices based on MoS2 still has huge room for improvement.
[0003] In recent years, the application of substrate engineering in two-dimensional electronic and optoelectronic devices has received widespread attention and reports. This method can greatly improve the properties of materials and enhance the performance of devices. According to previous literature reports (Nature Electronics, 2022, 5(8): 489-496), by using an undulating substrate to introduce lattice distortion into two-dimensional MoS2, electron-phonon scattering in two-dimensional materials can be reduced, thereby improving carrier mobility.
[0004] At present, the realization of substrate engineering mostly relies on dry or wet transfer methods to transfer MoS2 to a specially patterned undulating target substrate, which will inevitably bring about problems such as contamination, wrinkles and breakage, greatly limiting its practical application. In addition, the transfer method in the prior art often adopts mechanical peeling, and the obtained single crystal domain is small, often only 10 to 20 μm. When transferred to the patterned undulating target substrate, it will only cover the undulating protrusions, and the depressions cannot be covered by MoS2, which easily forms gaps and air cavities, and produces bubbles. The corresponding photodetector has limited performance (as shown in Table 1 below).
[0005] Direct in-situ epitaxial growth on a specially patterned substrate is undoubtedly more advantageous, but it is currently quite challenging to achieve large-area, high-quality monolayer MoS2 on a non-flat substrate. Summary of the invention
[0006] In view of the above defects or improvement needs of the prior art, the purpose of the present invention is to provide a molybdenum disulfide thin film on a patterned substrate, a preparation method and an application. By using in-situ growth, a conformally grown molybdenum disulfide thin film is obtained on a patterned substrate. The molybdenum disulfide single crystal domain is in close contact with the patterned substrate, without gaps and bubbles, and the performance is better than the molybdenum disulfide thin film on a patterned substrate obtained by a traditional transfer method. The photoconductive photodetector constructed based on the molybdenum disulfide thin film on the patterned substrate has better performance in terms of response time, light-dark current ratio, and specific detection rate. At the same time, the preparation process of the present invention is simple, the production cost is low, and it is suitable for mass production.
[0007] To achieve the above-mentioned purpose, according to one aspect of the present invention, a molybdenum disulfide film on a patterned substrate is provided, characterized in that it includes a patterned undulating substrate and a molybdenum disulfide layer grown in situ on the substrate; the molybdenum disulfide layer contains a molybdenum disulfide single crystal domain with a thickness of a monomolecular layer; and in the substrate region below any molybdenum disulfide single crystal domain, the undulating protrusions and depressions of the substrate are tightly covered by the molybdenum disulfide single crystal domain.
[0008] As a further preferred embodiment of the present invention, the patterned undulating substrate is specifically a patterned undulating sapphire substrate, a patterned undulating silicon dioxide substrate or a patterned undulating silicon substrate.
[0009] As a further preferred embodiment of the present invention, the molybdenum disulfide layer comprises a molybdenum disulfide single crystal domain having a monomolecular layer with a size of 100 μm to 300 μm.
[0010] According to another aspect of the present invention, the present invention provides a method for preparing a molybdenum disulfide thin film on the above-mentioned patterned substrate, characterized in that it comprises the following steps:
[0011] (1) Preparing a patterned undulating substrate;
[0012] (2) dispersing molybdate in water to prepare a molybdenum source solution;
[0013] (3) pre-treating the cleaned patterned undulating substrate with oxygen plasma, and then coating the molybdenum source solution obtained in step (2) on the patterned undulating surface of the pre-treated substrate by a spin coating process, followed by drying, thereby obtaining a substrate with a molybdenum source layer;
[0014] (4) Sulfur powder is used as a sulfur source, and a molybdenum disulfide film is grown in situ on the surface of a substrate by a chemical vapor deposition process; the chemical vapor deposition process specifically adopts a three-zone heating furnace, and chemical vapor deposition is performed under the condition of introducing a carrier gas flow; the three-zone heating furnace includes a first temperature zone, a second temperature zone and a third temperature zone distributed in sequence along the gas flow direction, the substrate with a molybdenum source layer is located in the center of the third temperature zone, and the surface where the molybdenum source layer is located can be in direct contact with the carrier gas flow; the sulfur powder is located in the center of the first temperature zone, the temperature of the first temperature zone is set to 150-250°C, the temperature of the second temperature zone is set to 300-450°C, and the temperature of the third temperature zone is set to 850°C.
[0015] As a further preferred embodiment of the present invention, a base is also used in step (2), specifically, molybdate and base are mixed in a molar ratio greater than or equal to 1:1 and then dispersed in water at the same time, thereby preparing a molybdenum source solution;
[0016] The base is an alkali metal hydroxide.
[0017] As a further preferred embodiment of the present invention, in step (2), the molybdate is selected from sodium molybdate and ammonium molybdate;
[0018] In step (3), the clean patterned undulating substrate is specifically obtained by ultrasonically cleaning the patterned undulating substrate in acetone, isopropanol, and deionized water for more than 5 minutes, and then drying it with nitrogen;
[0019] The oxygen plasma pretreatment is specifically to treat with oxygen plasma for more than 1 minute;
[0020] The spin coating speed used in the spin coating process is greater than 1000 rpm, and the spin coating time is greater than 30 s;
[0021] In step (4), the flow rate of the carrier gas is greater than 200 sccm, and the chemical vapor deposition time is more than 3 minutes.
[0022] According to another aspect of the present invention, the present invention provides a photoconductive photodetector constructed based on the molybdenum disulfide thin film on the above-mentioned patterned substrate, characterized in that it is obtained by respectively depositing electrode materials at both ends of the molybdenum disulfide single crystal in the molybdenum disulfide thin film on the above-mentioned patterned substrate.
[0023] As a further preferred embodiment of the present invention, the deposited electrode material is firstly photolithographically patterned and then developed to evaporate the electrode;
[0024] Preferably, the photolithography is specifically ultraviolet photolithography, laser direct writing or electron beam exposure; and the evaporation is specifically thermal evaporation or electron beam evaporation.
[0025] Through the above technical scheme conceived by the present invention, compared with the prior art, the molybdenum disulfide thin film on the patterned substrate of the present invention is obtained by in-situ growing a monomolecular layer of molybdenum disulfide single crystal domains on a patterned undulating substrate, and has the characteristics of conformal coverage (that is, the substrate area below any molybdenum disulfide single crystal domain, the undulating protrusions and depressions of the substrate are all tightly covered by the molybdenum disulfide single crystal domains, without gaps and bubbles), which is obviously different from the molybdenum disulfide thin film on the patterned substrate obtained by the traditional transfer method, and the performance is also better than the molybdenum disulfide thin film on the patterned substrate obtained by the traditional transfer method.
[0026] At the same time, the monolayer molybdenum disulfide obtained by the present invention has the characteristics of large size, high coverage and high quality, and the size can reach 100 μm to 300 μm, and the maximum can exceed 300 μm, which is much larger than the crystal domain with a size of 10 to 20 μm obtained by the traditional transfer method. Based on the present invention, a large-size, high-quality monolayer molybdenum disulfide with a size exceeding 300 μm can be obtained on patterned substrates of various patterns.
[0027] In addition, the molybdenum disulfide film on the patterned substrate obtained by the present invention also inherits the substrate engineering to achieve the regulation of material stress and the improvement of device performance. For example, the present invention uses a patterned substrate to apply periodic stress to a monolayer of molybdenum disulfide, which can effectively achieve periodic regulation of its energy band structure. For another example, the present invention also improves the light absorption of a monolayer of molybdenum disulfide by the localized effect of the light field of the incident light on the patterned substrate.
[0028] Specifically, the present invention can achieve the following beneficial effects:
[0029] (1) The present invention directly grows a monolayer of MoS2 in situ on a patterned substrate, effectively avoiding contamination and defects introduced by cumbersome dry or wet transfer processes.
[0030] The molybdenum disulfide thin film on the patterned substrate of the present invention has the characteristic of conformal coverage. Any substrate area below a molybdenum disulfide single crystal domain, the undulating protrusions and depressions of the substrate are tightly covered by the molybdenum disulfide single crystal domain without gaps and bubbles, thus avoiding other pollution and defects and achieving better performance. For this reason, the photoconductive photodetector constructed based on the molybdenum disulfide thin film on the patterned substrate of the present invention has better performance in response time, light-dark current ratio, and specific detection rate than the molybdenum disulfide thin film on the patterned substrate obtained by the traditional transfer method.
[0031] (2) The preparation method of the present invention adopts the method of pre-spin coating the reactant solution on the substrate, and effectively improves the wetting properties of the solution and the substrate by oxygen plasma treatment. Compared with the method of using reactant powders for both the molybdenum source and the sulfur source, it is more conducive to obtaining a monolayer of molybdenum disulfide with better uniformity on the substrate.
[0032] (3) The present invention is the first to prepare a monolayer of MoS2 single crystals on a patterned substrate by a hydroxide-assisted gas-liquid-solidification vapor deposition method. The prepared single crystal has a maximum size of more than 300 μm, which is the largest size MoS2 single crystal reported on a patterned substrate.
[0033] (4) The present invention can achieve conformal growth of large-sized MoS2 single crystals on a patterned substrate by selecting a suitable temperature range. Too low a temperature cannot achieve complete coverage of the pattern, while too high a temperature causes the evaporation rate of the reaction source to be too fast, resulting in rapid cessation of the reaction, resulting in a smaller crystal size.
[0034] In summary, the present invention can in-situ grow a large-sized monolayer of high-coverage, high-quality molybdenum disulfide on the surface of a patterned substrate. At the same time, the photodetector can be further prepared by micro-nano processing technology. This substrate engineering method can greatly improve the properties of the material and the performance of the device. Since the method is simple and controllable, low-cost, and the obtained photodetector based on the molybdenum disulfide film on the patterned substrate has good photoelectric performance, it has great potential in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of the preparation process of the molybdenum disulfide film on the patterned substrate in Example 1.
[0036] Figure 2 Schematic diagram of the structure of the molybdenum disulfide film on the patterned sapphire substrate in Example 1.
[0037] Figure 3 This is an optical microscopic image of the molybdenum disulfide film on the patterned sapphire substrate prepared in Example 1.
[0038] Figure 4 This is a scanning electron microscopic image of the molybdenum disulfide film on the patterned sapphire substrate prepared in Example 1.
[0039] Figure 5 This is an atomic force microscope image of the molybdenum disulfide film on the patterned sapphire substrate prepared in Example 1.
[0040] Figure 6 The peak position and intensity spectrum of the photoluminescence of the molybdenum disulfide film on the patterned sapphire substrate prepared in Example 1.
[0041] Figure 7 Schematic diagram of the structure of the photodetector based on the molybdenum disulfide film on the patterned sapphire substrate in Example 2.
[0042] Figure 8 This is a performance characterization diagram of the photodetector based on the molybdenum disulfide film on the patterned sapphire substrate prepared in Example 2.
[0043] Fig. 9 A single-layer molybdenum disulfide film obtained on a patterned undulating substrate by a traditional transfer method as reported in the prior art (ACS Nano 2019, 13, 8, 9057–9066); wherein, Fig. 9 a in the figure is a scanning electron microscope image. Fig. 9 b in the figure is an atomic force microscopy image.
[0044] Fig.10 This is an optical microscopic image of the molybdenum disulfide film on the patterned sapphire substrate prepared in Example 3.
[0045] Fig.11 This is an optical microscopic image of the molybdenum disulfide film on the patterned sapphire substrate prepared in Example 4.
[0046] Fig.12 The scanning electron microscopic images of molybdenum disulfide films grown on patterned sapphire substrates in Comparative Example 1 and Comparative Example 2 at different third temperature settings; wherein, Fig.12 a in the figure is grown at 700℃. Fig.12 b in the figure is grown at 900°C. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0048] Based on the present invention, sodium molybdate solution can be used as a molybdenum source, sodium hydroxide solution can be used as a catalyst, sulfur powder can be used as a sulfur source, and patterned sapphire can be used as a substrate to obtain a molybdenum disulfide film on the patterned substrate through a chemical vapor deposition method.
[0049] Example 1
[0050] Combination Figure 1 As shown, the preparation process of a molybdenum disulfide film on a patterned substrate is as follows:
[0051] (1) Preparation of patterned sapphire substrate: A 200 nm thick SiO2 layer is deposited on a flat sapphire substrate by plasma enhanced chemical vapor deposition (PECVD). Then, a photoresist is spin-coated on the top of the SiO2 layer, and exposed and developed to obtain a circular pattern with a size of 1 μm and a periodic interval of 1 μm (that is, the diameter of any circular shape is 1 μm, and the distance from the edge to the edge of any two adjacent circular shapes is 1 μm). Then, the patterned SiO2 is obtained by inductively coupled plasma etching (ICP). After degumming with a stripping solution, the substrate is wet-etched in a mixed solution of H2SO4 and H3PO4 heated to 270°C (the mixed solution of H2SO4 and H3PO4 is specifically obtained by mixing 98% concentrated sulfuric acid and 85% concentrated phosphoric acid in a volume ratio of 3:1) for several minutes. Finally, the residual SiO2 is removed by a buffered oxide etchant (BOE) to obtain a patterned sapphire substrate;
[0052] (2) preparing a mixed solution of sodium molybdate and sodium hydroxide: dissolving 155 mg of sodium molybdate and 30 mg of sodium hydroxide in 100 ml of deionized water (the corresponding molar ratio of sodium molybdate to sodium hydroxide is 1.003:1) to obtain a mixed solution;
[0053] (3) Substrate pretreatment and source solution spin coating: The patterned sapphire substrate was cut into small squares of 1.5 cm × 1.5 cm, ultrasonically cleaned in acetone, isopropanol, and deionized water for 10 min, and blown dry with nitrogen; then treated with an oxygen plasma treatment machine for 3 min; the prepared mixed solution was dripped on it, spin coated at a speed of 1500 rpm for 90 s, and then naturally air-dried;
[0054] (4) Growth by chemical vapor deposition method: A 3-inch three-zone tube furnace (Hefei Kejing, OTF-1200X-Ⅲ) is used. The three zones are the first zone, the second zone and the third zone, which are distributed in sequence along the direction of the gas flow. The spin-coated substrate is placed flat in a quartz boat with the front side facing up and placed in the center of the third zone in the three-zone tube furnace. At the same time, a ceramic boat containing 400 mg of sulfur powder is placed in the center of the first zone on the upstream side, with a distance of 60 cm between the two. After vacuuming and purging, the gas flow rate of the carrier gas (nitrogen) is controlled to 300 sccm, and the gas pressure is maintained at normal pressure. The three zones are heated from room temperature to 200°C, 350°C and 850°C respectively (wherein the temperature used in the first zone is to sublimate the sulfur powder; the second zone is used for temperature transition; and the third zone is used to grow MoS2 thin film). The third zone is maintained at 850°C for 5 minutes of growth. After the growth is completed, the sample is taken out after natural cooling to room temperature.
[0055] like Figure 2As shown, the structure of the molybdenum disulfide film on the patterned substrate prepared by Example 1 is: the bottom is a patterned sapphire substrate, and the top is a conformally covered single-layer molybdenum disulfide film.
[0056] The sample prepared in Example 1 was examined by optical microscope, and the results were as follows: Figure 3 As shown, it is not difficult to see that in Example 1, a single layer of MoS2 is grown in situ on the surface of the patterned sapphire substrate, and has the characteristics of high coverage and large size. The maximum size of the generated MoS2 single crystal domain can reach 300 μm (such as Figure 3 As shown, the largest single crystal domain has a triangular side exceeding 300 μm).
[0057] The sample prepared in Example 1 was examined by scanning electron microscopy, and the results were as follows: Figure 4 As shown, it can be seen that the molybdenum disulfide single crystal grows on the patterned sapphire surface, completely covering the pyramid pattern underneath it. At the same time, no wrinkles or bubbles are observed, indicating conformal coverage.
[0058] The sample prepared in Example 1 was tested by atomic force microscopy, and the results were as follows: Figure 5 As shown, it is not difficult to see that the single-layer MoS2 film generated in situ in Example 1 is conformal coverage, and the undulating substrate area below the single crystal domain, whether it is the undulating protrusions or depressions, has been tightly covered by the grown MoS2, which is obviously different from the MoS2 film formed on the patterned undulating substrate by the traditional transfer method (such as Fig. 9 As shown, ACS Nano 2019, 13, 8, 9057–9066).
[0059] And, if Figure 6 As shown, the molybdenum disulfide film on the patterned substrate prepared by the preparation method of Example 1 is subjected to the periodic stress applied by the pattern on the substrate. The molybdenum disulfide on the patterned triangular pyramid is subjected to more compressive stress than the molybdenum disulfide in the flat area, and the band gap becomes larger, causing the photoluminescence peak to blue shift. At the same time, due to the local effect of the patterned structure on the incident light field, the molybdenum disulfide on the patterned triangular pyramid exhibits a greater photoluminescence intensity than the molybdenum disulfide in the flat area.
[0060] Example 2
[0061] Based on the molybdenum disulfide film on the patterned substrate prepared by the preparation method described in Example 1, at both ends of a single crystal domain, such as Figure 7As shown, by photolithography of the electrode pattern, 10 nm of titanium and 50 nm of gold are deposited by electron beam evaporation after development to form a titanium / gold stacked electrode (wherein the titanium layer is in direct contact with the molybdenum disulfide film), and after acetone immersion and degumming, a photoconductive photodetector based on the molybdenum disulfide film on the patterned substrate is obtained.
[0062] like Figure 8 As shown in the figure, the dark current of the photodetector is less than 1pA, and the light-to-dark current ratio is more than 10 6 When the bias voltage is 2V, the responsivity exceeds 10A / W and the specific detection rate is close to 10 14 Jones, the parameter performance is better than the prior art reported (as shown in the table below).
[0063] Table 1: Performance comparison table of the device in Example 2 and the device reported in the prior art
[0064]
[0065] Example 3
[0066] The difference between this embodiment and embodiment 1 is that:
[0067] The molar ratio of sodium molybdate to sodium hydroxide in the prepared molybdenum source solution is 1:0.33 (specifically, 155 mg of sodium molybdate and 10 mg of sodium hydroxide are dissolved in 100 ml of deionized water to obtain a mixed solution), and the remaining parameters of the preparation method are the same as those in Example 1.
[0068] like Fig.10 As shown, at this time, due to the smaller NaOH catalyst content, the fluidity of the droplet intermediates during the reaction is weakened, which will lead to a reduction in the crystal domain of the obtained MoS2 single crystal to about 100-200μm, but MoS2 that conformally covers the bottom patterned substrate can still be obtained.
[0069] Example 4
[0070] The difference between this embodiment and embodiment 1 is that:
[0071] No sodium hydroxide was added to the prepared molybdenum source solution (specifically, 155 mg of sodium molybdate was dissolved in 100 ml of deionized water), and the remaining parameters of the preparation method were the same as those in Example 1.
[0072] like Fig.11 As shown, at this time, due to the lack of NaOH addition, the fluidity of the droplet intermediates during the reaction is further restricted, which will cause the obtained MoS2 single crystal domain to be further reduced to 100μm, but MoS2 that conformally covers the bottom patterned substrate can still be obtained.
[0073] Comparative Example 1
[0074] The difference between this comparative example and Example 1 is that:
[0075] The reaction temperature in the third temperature zone is 700° C., and the other parameters of the preparation method are the same as those in Example 1.
[0076] Combined with supplements Fig.12 As shown in (a), when the reaction temperature is low, it is impossible to achieve complete coverage of the patterned sapphire underneath by a single layer of molybdenum disulfide.
[0077] Comparative Example 2
[0078] The difference between this comparative example and Example 1 is that:
[0079] The reaction temperature in the third temperature zone is 900° C., and the other parameters of the preparation method are the same as those in Example 1.
[0080] Combined with supplements Fig.12 As shown in (b), when the reaction temperature is too high, the Mo source evaporates too quickly, and the size of the obtained MoS2 film is very small.
[0081] Comparative Example 3
[0082] The difference between this comparative example and Example 1 is that:
[0083] The molar ratio of sodium molybdate to sodium hydroxide in the prepared molybdenum source solution is 1:1.33 (specifically, 155 mg of sodium molybdate and 40 mg of sodium hydroxide are dissolved in 100 ml of deionized water to obtain a mixed solution), and the remaining parameters of the preparation method are the same as those in Example 1.
[0084] At this time, due to the excess of NaOH, the fluidity of the droplet intermediates during the reaction is too strong, and the MoS2 precipitation rate is lower than the lateral flow rate of the droplet intermediates, resulting in the inability to form a single crystal film.
[0085] The above embodiments are only examples. For example, in addition to nitrogen, the carrier gas may also be an inert gas such as argon. In another example, in addition to NaOH, the base may also be other alkali metal hydroxides such as KOH. In addition, the monolayer of molybdenum disulfide in the present invention refers to a monomolecular layer of molybdenum disulfide (thickness ≈0.8 nm).
[0086] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A molybdenum disulfide film on a patterned substrate, It is characterized in that It includes a patterned undulating substrate and a molybdenum disulfide layer grown in situ on the substrate; the molybdenum disulfide layer contains a molybdenum disulfide single crystal domain with a thickness of a monomolecular layer; and in a substrate region below any molybdenum disulfide single crystal domain, the undulating protrusions and depressions of the substrate are tightly covered by the molybdenum disulfide single crystal domain.
2. The molybdenum disulfide thin film on the patterned substrate as claimed in claim 1, It is characterized in that The patterned undulating substrate is specifically a patterned undulating sapphire substrate, a patterned undulating silicon dioxide substrate or a patterned undulating silicon substrate.
3. The molybdenum disulfide thin film on the patterned substrate as claimed in claim 1, It is characterized in that The molybdenum disulfide layer comprises a molybdenum disulfide single crystal domain having a monomolecular layer with a size of 100 μm to 300 μm.
4. The method for preparing a molybdenum disulfide thin film on a patterned substrate according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) Preparing a patterned undulating substrate; (2) dispersing molybdate in water to prepare a molybdenum source solution; (3) pre-treating the cleaned patterned undulating substrate with oxygen plasma, and then coating the molybdenum source solution obtained in step (2) on the patterned undulating surface of the pre-treated substrate by a spin coating process, followed by drying, thereby obtaining a substrate with a molybdenum source layer; (4) Sulfur powder is used as a sulfur source, and a molybdenum disulfide film is grown in situ on the surface of a substrate by a chemical vapor deposition process; the chemical vapor deposition process specifically adopts a three-zone heating furnace, and chemical vapor deposition is performed under the condition of introducing a carrier gas flow; the three-zone heating furnace includes a first temperature zone, a second temperature zone and a third temperature zone distributed in sequence along the gas flow direction, the substrate with a molybdenum source layer is located in the center of the third temperature zone, and the surface where the molybdenum source layer is located can be in direct contact with the carrier gas flow; the sulfur powder is located in the center of the first temperature zone, the temperature of the first temperature zone is set to 150-250°C, the temperature of the second temperature zone is set to 300-450°C, and the temperature of the third temperature zone is set to 850°C.
5. The preparation method according to claim 4, It is characterized in that In step (2), a base is also used, specifically, molybdate and base are mixed in a molar ratio greater than or equal to 1:1 and then dispersed in water at the same time, thereby preparing a molybdenum source solution; The base is an alkali metal hydroxide.
6. The preparation method according to claim 4, It is characterized in that In step (2), the molybdate is selected from sodium molybdate and ammonium molybdate; In step (3), the clean patterned undulating substrate is specifically obtained by ultrasonically cleaning the patterned undulating substrate in acetone, isopropanol, and deionized water for more than 5 minutes, and then drying it with nitrogen; The oxygen plasma pretreatment is specifically to treat with oxygen plasma for more than 1 minute; The spin coating speed used in the spin coating process is greater than 1000 rpm, and the spin coating time is greater than 30 s; In step (4), the flow rate of the carrier gas is greater than 200 sccm, and the chemical vapor deposition time is more than 3 minutes.
7. A photoconductive photodetector constructed based on a molybdenum disulfide thin film on a patterned substrate as claimed in any one of claims 1 to 3, It is characterized in that The method is obtained by respectively depositing electrode materials on both ends of the molybdenum disulfide single crystal in the molybdenum disulfide film on the patterned substrate.
8. The photoconductive photodetector according to claim 7, It is characterized in that The deposition of electrode material is achieved by first photolithography of electrode pattern and then evaporation of electrode after development; Preferably, the photolithography is specifically ultraviolet photolithography, laser direct writing or electron beam exposure; and the evaporation is specifically thermal evaporation or electron beam evaporation.
Citation Information
Cited By
Preparation method, product and application of MoS2 nano island modified WS2 film
CN122501919A