Atomic layer deposition reaction chamber capable of performing semi-continuous powder coating and use method thereof
By designing a semi-continuous powder-coated atomic layer deposition reaction chamber, the U-tube reaction chamber and vibrating motor are used to achieve fluidized dispersion of powder, the problem of omitting frequent disassembly and cleaning steps in the prior art is solved, and the production efficiency is improved and coating integrity, suitable for batch and continuous coating.
Patent Information
- Application Number
- CN202410876049.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-15
AI Technical Summary
The existing atomic layer deposition reaction chambers require frequent disassembly and loading during powder coating, resulting in low production efficiency. The omitted cleaning steps will reduce the integrity of the coating and cannot be suitable for batch and continuous coating.
A semi-continuous powder-coated atomic layer deposition reaction chamber is designed, using U-shaped tube reaction chamber body, powder feeding device, powder discharge device, precursor conveying system, fluidized gas conveying system, exhaust gas treatment and vacuum The system, heating and electrical control system realizes bottom-up fluidization and dispersion of powders through vibrating motors and fluidized gases, omitting frequent disassembly operations during the loading and unloading of the reaction chamber, and retaining the cleaning steps of the atomic layer deposition reaction.
It improves the production efficiency of powder coating, is suitable for batch and semi-continuous coating, retains the integrity of the coating, avoids frequent disassembly operations of the reaction chamber, and achieves efficient coating of the powder.
Smart Images

Figure CN118957535A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of atomic layer deposition, and in particular relates to an atomic layer deposition reaction chamber capable of semi-continuous powder coating and a use method thereof. Background Art
[0002] By using the atomic layer deposition method, the surface of the powder particles can be coated with a film with controlled atomic-level thickness to achieve the purpose of surface modification of the powder particles. In order to complete the atomic layer deposition coating on the powder surface, one method is to fluidize the powder to complete the atomic layer deposition reaction, which is to introduce a fluidizing gas from bottom to top to shear and disperse the powder particles, so that the precursor molecules are coated on the powder surface by atomic layer deposition reaction. For a conventional reaction chamber placed vertically, on the one hand, the fluidizing gas enters the reaction chamber from bottom to top through the filter at the bottom air inlet of the reaction chamber to fluidize and disperse the powder, and the installation and removal of the bottom filter is difficult; on the other hand, after the powder coating is completed, the reaction chamber needs to be disassembled as a whole to take out the material and reload it, and the production efficiency of powder coating needs to be improved.
[0003] The document “Continuous production of nanostructured particles using spatialatomic layer deposition” reports a continuous powder atomic layer deposition reaction chamber device based on pneumatic conveying. Although the reaction chamber can continuously coat the powder, the cleaning step in the atomic layer deposition reaction is omitted, so that the coating structure on the powder surface is nano-particle-like. The omission of the cleaning step will reduce the integrity of the coating. In addition, Chinese invention patent CN103451623A discloses a powder fluidized atomic layer deposition reaction chamber device. The reaction chamber uses fluidizing gas to disperse the powder, but a filter is used at the bottom of the reaction chamber, and the loading and unloading of the powder needs to be completed by disassembling the reaction chamber. The reaction chamber device is not suitable for continuous and batch powder coating. Summary of the invention
[0004] The object of the present invention is to provide an atomic layer deposition reaction chamber capable of semi-continuous powder coating and a method of using the same, which omits the frequent reaction chamber disassembly operation during the reaction chamber loading and unloading process while retaining the atomic layer deposition reaction cleaning step, so as to achieve batch coating of powders and improve powder coating efficiency.
[0005] The atomic layer deposition reaction chamber capable of semi-continuous powder coating provided by the present invention comprises a U-shaped tube reaction chamber body, a powder feeding device, a powder discharging device, a precursor conveying system, a fluidizing gas conveying system, an exhaust gas treatment and vacuum system, and a heating and electrical control system; wherein:
[0006] The U-tube reaction chamber body is placed vertically, and its two sides are cylindrical pipes, which are a feed conveying pipe and a powder fluidizing pipe respectively. The feed conveying pipe and the powder fluidizing pipe are connected by a bend pipe to form a U shape; the fluidizing gas and the precursor gas enter from the top of the feed conveying pipe.
[0007] The connecting elbow between the feed conveying pipeline and the powder fluidizing pipeline is semicircular and fixed on a vibration motor to facilitate the loosening and dispersion of the powder at the bottom.
[0008] Preferably, the vibration frequency of the vibration motor is 20-60 Hz.
[0009] The fluidizing gas passes through the feed conveying pipe and the bottom connecting pipe in sequence, pushes the powder to be coated into the powder fluidizing pipe, and fluidizes and disperses the powder from bottom to top in the fluidizing pipe (see Figure 5 ).
[0010] The powder feeding device is connected to the port of the U-tube reaction chamber feeding and conveying pipeline and is air-isolated from the feeding and conveying pipeline. The powder is fed from the feeding device into the feeding and conveying pipeline and enters the bottom area of the U-tube reaction chamber under the action of gravity.
[0011] The powder discharging device is arranged at the gas outlet port of the powder fluidizing pipeline of the U-tube reaction chamber and is connected to the exhaust gas treatment and vacuum system; a bearing net is provided above the powder discharging device near the exhaust gas treatment interface to block and collect attached powder, and the attached powder can fall into the powder discharging device at the lower end by gravity, or fall into the powder discharging device by intermittent mechanical knocking of the tube wall.
[0012] Preferably, the selected carrier mesh is detachable, and the pore size is 10 to 30 microns.
[0013] The precursor delivery system is used for delivering precursor pulses, and its gas outlet port is arranged on the U-tube reaction chamber feed delivery pipeline.
[0014] Preferably, the first precursor (such as trimethylaluminum) is pulsed multiple times, with a flow rate of 30 to 100 sccm, a pulse time of 10 ms to 100 ms, and a number of 1 to 10 times.
[0015] Preferably, the second precursor (such as deionized water) is pulsed multiple times, with a flow rate of 30 to 100 sccm, a pulse time of 10 ms to 100 ms, and a number of 1 to 10 times.
[0016] The fluidizing gas delivery system is used for fluidizing and dispersing the powder in the powder fluidizing pipeline of the U-tube reaction chamber, and its gas outlet port is arranged on the powder feed delivery pipeline and above the gas outlet port of the precursor delivery system. In this way, when the precursor pulse enters the reaction chamber, the fluidizing gas can carry the precursor molecules into the powder fluidizing pipeline of the U-tube reaction chamber.
[0017] Preferably, the fluidizing gas (such as nitrogen) has a gas flow rate of 100 sccm to 5000 sccm.
[0018] The tail gas treatment and vacuum system is used for tail gas treatment and vacuuming of the reaction chamber.
[0019] The heating and electrical control system is used to heat each pipeline part and the fluidized pipeline part of the reaction chamber and to realize electrical control of the reaction chamber.
[0020] Preferably, the heating temperature of the powder fluidizing pipe is 100°C to 300°C.
[0021] The gas outlet port of the powder fluidizing pipeline is connected to the powder discharging device, tail gas treatment and vacuum system in one of the following two ways or a combination thereof:
[0022] (I) The outlet port of the powder fluidization pipeline is connected to the tail gas treatment and vacuum system through the carrier net, and the lower side of the carrier net is connected to the powder discharge device (see Figure 3 );
[0023] (ii) The outlet port of the powder fluidization pipeline is connected to the tail gas treatment and vacuum system through a three-way valve, and the other is connected to the vertical downward powder conveying pipe, vacuum system and powder discharge device. The powder discharge device is on the lower side of the carrier net, and the rear section of the carrier net is connected to a large suction vacuum pump (see Figure 4 ).
[0024] When the above solution (I) is adopted, after the powder coating reaction is completed, it is necessary to increase the gas fluidization speed so that the powder can reach the pneumatic conveying state and be transported to the powder discharging device.
[0025] Preferably, the flow rate of the fluidizing gas is 1000 sccm to 8000 sccm.
[0026] When the above scheme (ii) is adopted, after the powder coating reaction is completed, it is necessary to appropriately increase the gas fluidization speed and cooperate with a large-force vacuum pump to allow the powder to reach the vertically downward powder conveying pipe and fall into the powder discharging device by gravity.
[0027] Preferably, the flow rate of the fluidizing gas is 1000 sccm to 5000 sccm.
[0028] The method for using the atomic layer deposition reaction chamber capable of semi-continuous powder coating comprises the following specific steps:
[0029] The first step is powder feeding;
[0030] Close the powder discharge port, feed a certain amount of powder from the powder feeding device into the U-tube reaction chamber, keep the vacuum pump on, turn on the fluidizing gas and continue to feed the fluidizing gas (such as nitrogen), the gas flow rate is 100sccm~5000sccm, and adjust the vibration frequency of the vibration motor to 20~60Hz, so that the powder is completely fluidized and dispersed in the powder fluidizing pipe of the reaction chamber.
[0031] The second step is powder coating reaction;
[0032] (i) Turn on the first precursor (trimethylaluminum) pulse multiple times, with a flow rate of 30 to 100 sccm, a pulse time of 10 ms to 100 ms, and a number of 1 to 10 times, so that the first precursor molecules are adsorbed on the powder surface.
[0033] (ii) turning off the first precursor pulse, continuing to inject the fluidizing gas, and using the vacuum system to extract the first precursor molecules that have not been adsorbed.
[0034] (iii) starting the second precursor (deionized water) pulse multiple times, with a flow rate of 30 to 100 sccm, a pulse time of 10 ms to 100 ms, and a number of 1 to 10 times, so that the second precursor molecules on the powder surface react fully with the adsorbed first precursor molecules.
[0035] (iv) turning off the second precursor pulse, continuing to inject the fluidizing gas, and using the vacuum system to extract the reaction byproducts and unreacted second precursor molecules.
[0036] (V) Repeat steps (I) to (IV) according to the thickness of the coating layer required for the powder.
[0037] The third step is powder collection;
[0038] After the second step is completed, open the discharge port, increase the fluidizing gas flow rate by 1000 sccm to 8000 sccm, and collect the coated powder through the powder discharge device; or use the combined effect of a vacuum pump with a large suction capacity and the fluidizing gas to collect the coated powder through the downward powder conveying pipe and the powder discharge device.
[0039] Step 4: Start the next batch of powder coating;
[0040] Repeat the first step to the third step, feed the next batch of powder from the powder feeding device, and carry out the next batch of powder coating operation to realize the semi-continuous powder coating process.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) By utilizing the reaction chamber and method of the present invention, during the powder coating process, it is not necessary to frequently disassemble the reaction chamber to load and unload powder. This is suitable for batch and semi-continuous powder coating, thereby improving production efficiency.
[0043] (2) By utilizing the reaction chamber and method of the present invention, the supporting net at the bottom of the air inlet of the powder reaction chamber is omitted and the powder is fluidized and dispersed.
[0044] (3) By utilizing the reaction chamber and method of the present invention, the cleaning step in the atomic layer deposition reaction is retained during the semi-continuous powder coating process, thereby preserving the integrity of the reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a flow chart of a semi-continuous powder coating process using a single U-tube reaction chamber.
[0046] Figure 2 The figure is a flow chart of a semi-continuous powder coating process using a U-shaped-inverted U-shaped composite reaction chamber.
[0047] Figure 3 Schematic diagram of a single U-tube reaction chamber device.
[0048] Figure 4 Schematic diagram of a U-shaped-inverted U-shaped composite reaction chamber device.
[0049] Figure 5 Schematic diagram of powder fluidization in the U-shaped reaction chamber.
[0050] Numbers in the figure: 1—feed storage tank, 2—feed delivery pipe, 3—U-shaped connecting pipe, 4—powder fluidizing pipeline, 5—tee, 6—powder bearing net, 7—exhaust gas treatment and vacuum system, 8—powder discharging device, 9—vibration motor, 10—feed storage tank, 11—feed delivery pipe, 12—U-shaped connecting pipe, 13—powder fluidizing pipeline, 14—tee, 15—first solenoid valve, 16—exhaust gas treatment and first vacuum pump system, 17—second solenoid valve, 18—powder delivery pipe, 19—powder bearing net, 20—second vacuum pump, 21—powder discharging device, 22—vibration motor, 100—powder to be coated. DETAILED DESCRIPTION
[0051] The present invention is further described below by way of embodiments in conjunction with the accompanying drawings.
[0052] Example 1, using a semi-continuous powder coating process with a single U-tube reaction chamber, such as Figure 1 As shown, the specific process is:
[0053] S11: close the discharge port, start the tail gas treatment and vacuum system 7, feed a certain amount of powder from the powder feeding device 1 to the feeding conveying pipeline 2 of the U reaction chamber, and the powder accumulates in the U-shaped connecting pipe 3 under the action of gravity.
[0054] S12: Keep the tail gas treatment and vacuum system 7 open, turn on the fluidizing gas and continue to feed the fluidizing gas (such as nitrogen), the gas flow rate is 200sccm~1000sccm, and turn on the vibration motor 9, adjust the vibration frequency to 20~50Hz, so that the powder is completely fluidized and dispersed in the powder fluidizing pipe 4 of the U-tube reaction chamber, and turn off the vibration motor 9.
[0055] The powder in the powder fluidizing pipe 4 is heated to 120° C. by a heating system and maintained at this temperature for more than 1 hour.
[0056] S13: Turn on the first precursor (trimethylaluminum) pulse multiple times, with a flow rate of 30-100 sccm, a pulse time of 10ms-100ms, and a number of 1-10 times, so that the first precursor molecules are adsorbed on the powder surface.
[0057] S14: Turn off the first precursor pulse, continue to fill the fluidizing gas, and extract the first precursor molecules that have not been adsorbed.
[0058] S15: Turn on the second precursor (deionized water) pulse multiple times, with a flow rate of 30-100 sccm, a pulse time of 10ms-100ms, and a number of 1-10 times, so that the second precursor molecules react fully with the adsorbed first precursor molecules on the powder surface.
[0059] S16: Turn off the second precursor pulse, continue to fill the fluidizing gas, and extract the reaction by-products and unreacted second precursor molecules.
[0060] S17: Repeat steps S13 to S16 according to the thickness of the coating layer required for the powder.
[0061] S18: After the coating is completed, the discharge port is opened, the fluidizing gas flow rate is increased by 2000 sccm to 5000 sccm, and the coated powder is collected through the powder discharge device 8.
[0062] S19: Repeat S11 to S18, feed the next batch of powder from the powder feeding device 1, and then coat the next batch of powder.
[0063] Example 2, using a semi-continuous powder coating process flow of a U-shaped-inverted U-shaped composite reaction chamber as follows Figure 2 As shown, specifically:
[0064] S21: close the second solenoid valve 17 and the discharge port, open the first solenoid valve 15, the tail gas treatment and the first vacuum pump 16 and the second vacuum pump 20, and feed a certain amount of powder from the powder feeding device 10 into the reaction chamber connecting elbow 12.
[0065] S22: Keep turning on the tail gas treatment and the first vacuum pump 16, turn on the fluidizing gas and continue to feed the fluidizing gas (such as nitrogen or argon) at a gas flow rate of 200sccm to 1000sccm, turn on the vibration motor 22, adjust the vibration frequency to 20 to 60Hz, so that the powder is fully fluidized and dispersed in the powder fluidizing pipe 13 of the U-tube reaction chamber, and turn off the vibration motor 22.
[0066] The powder in the powder fluidizing pipe 13 is heated to 125° C. by a heating system and maintained at this temperature for more than 1 hour.
[0067] S23: Turn on the first precursor (trimethylaluminum) pulse multiple times, with a flow rate of 30-100 sccm, a pulse time of 10ms-100ms, and a number of 1-10 times, so that the first precursor molecules are adsorbed on the powder surface.
[0068] S24: Turn off the first precursor pulse, continue to fill the fluidizing gas, and extract the first precursor molecules that have not been adsorbed.
[0069] S25: Turn on the second precursor (deionized water) pulse multiple times, with a flow rate of 30-100 sccm, a pulse time of 10ms-100ms, and a number of 1-10 times, so that the second precursor molecules react fully with the adsorbed first precursor molecules on the powder surface.
[0070] S26: Turn off the second precursor pulse, continue to fill the fluidizing gas, and extract the reaction by-products and unreacted second precursor molecules.
[0071] S27: Repeat steps S23 to S26 according to the thickness of the coating layer required for the powder.
[0072] S28: After the coating is completed, the first solenoid valve 15 is closed, and the second solenoid valve 17 and the discharge port of the powder discharge device are opened. Under the action of the second vacuum pump 20 with large suction capacity and the fluidizing gas, the coated powder is collected through the powder conveying pipe 18 and the powder discharge device 21.
[0073] S29: Repeat S21 to S28, feed the next batch of powder from the powder feeding device 7, and coat the next batch of powder.
Claims
1. An atomic layer deposition reaction chamber capable of semi-continuous powder coating, characterized in that: It includes a U-tube reaction chamber body, a powder feeding device, a powder discharging device, a precursor conveying system, a fluidizing gas conveying system, an exhaust gas treatment and vacuum system, a heating and electrical control system; wherein: The U-shaped tube reaction chamber body is placed vertically, and its two sides are cylindrical pipes, which are respectively a feed delivery pipe and a powder fluidization pipe. The feed delivery pipe and the powder fluidization pipe are connected by a bend pipe to form a U shape and are fixed on a vibration motor; the fluidization gas and the precursor gas enter from the top of the feed delivery pipe; The powder feeding device is connected to the port of the feeding and conveying pipeline of the U-shaped tube reaction chamber and is air-isolated from the feeding and conveying pipeline; the powder is fed from the feeding device into the feeding and conveying pipeline and enters the bottom area of the U-shaped tube reaction chamber under the action of gravity; The powder discharging device is arranged at the gas outlet port of the powder fluidizing pipeline of the U-shaped tube reaction chamber and is connected to the tail gas treatment and vacuum system; a bearing net is provided above the powder discharging device near the tail gas treatment interface to block and collect the attached powder; the attached powder falls into the powder discharging device at the lower end by gravity, or falls into the powder discharging device by intermittent mechanical knocking of the tube wall; The precursor delivery system is used for delivering precursor pulses, and its gas outlet port is arranged on the U-tube reaction chamber feed delivery pipeline; The fluidizing gas delivery system is used for fluidizing and dispersing powder in the powder fluidizing pipeline of the U-tube reaction chamber, and its gas outlet port is arranged on the powder feed delivery pipeline and above the gas outlet port of the precursor delivery system; after the precursor pulse enters the reaction chamber, the fluidizing gas carries the precursor molecules into the powder fluidizing pipeline of the U-tube reaction chamber; The tail gas treatment and vacuum system is used for tail gas treatment and vacuuming of the reaction chamber; The heating and electrical control system is used to heat each pipeline part and the fluidized pipeline part of the reaction chamber and to realize electrical control of the reaction chamber.
2. The atomic layer deposition reaction chamber capable of semi-continuous powder coating according to claim 1, characterized in that: The gas outlet port of the powder fluidizing pipeline is connected to the powder discharging device, tail gas treatment and vacuum system in one of the following two ways or a combination thereof: (i) The gas outlet port of the powder fluidization pipeline is transitioned through a carrier net and connected to the tail gas treatment and vacuum system, and the lower side of the carrier net is connected to the powder discharge device; (ii) The gas outlet port of the powder fluidizing pipeline is connected to the exhaust gas treatment and vacuum system through a three-way valve, and the other port is connected to the vertically downward powder conveying pipe, the vacuum system and the powder discharging device. The powder discharging device is on the lower side of the supporting net, and the rear section of the supporting net is connected to a high-draft vacuum pump.
3. The atomic layer deposition reaction chamber capable of semi-continuous powder coating according to claim 2, characterized in that: The vibration frequency of the vibration motor is 20-60 Hz.
4. The atomic layer deposition reaction chamber capable of semi-continuous powder coating according to claim 2, characterized in that: The carrier net is detachable, and the pore size is 10 to 30 microns.
5. The atomic layer deposition reaction chamber capable of semi-continuous powder coating according to claim 2, characterized in that: The precursor delivery system is used for delivering a precursor pulse, wherein the precursor pulse comprises: The first precursor is trimethylaluminum, the pulse flow rate is 30-100 sccm, the pulse time is 10ms-100ms, and the number of times is 1-10 times; The second precursor is deionized water, the pulse flow rate is 30-100 sccm, the pulse time is 10ms-100ms, and the number of times is 1-10 times.
6. The atomic layer deposition reaction chamber capable of semi-continuous powder coating according to claim 2, characterized in that: In the fluidizing gas delivery system, the fluidizing gas is nitrogen, and the gas flow rate is 100 sccm to 5000 sccm.
7. The atomic layer deposition reaction chamber capable of semi-continuous powder coating according to claim 2, characterized in that: In the heating and electrical control system, the heating temperature of the powder fluidizing pipeline is 100°C to 300°C.
8. The atomic layer deposition reaction chamber capable of semi-continuous powder coating according to claim 2, characterized in that: The connection mode between the gas outlet port of the powder fluidizing pipeline and the powder discharging device, tail gas treatment and vacuum system; For connection scheme (I), after the powder coating reaction is completed, it is necessary to increase the gas fluidization speed so that the powder reaches the pneumatic conveying state and is transported to the powder discharging device; the specific fluidization gas flow rate is controlled to be 1000sccm to 8000sccm; For connection scheme (ii), after the powder coating reaction is completed, it is necessary to appropriately increase the gas fluidization speed and cooperate with a large-force vacuum pump to allow the powder to reach the vertically downward powder conveying pipe and fall into the powder discharge device by gravity. The specific fluidization gas flow rate is controlled to be 1000sccm~5000sccm.
9. The method for using the atomic layer deposition reaction chamber capable of semi-continuous powder coating as claimed in any one of claims 2 to 8, characterized in that: The specific steps are: The first step is powder feeding; Close the powder discharge port, feed a certain amount of powder from the powder feeding device into the U-tube reaction chamber, keep the vacuum pump on, turn on the fluidizing gas and continue to feed the fluidizing gas, the gas flow rate is 100sccm to 5000sccm, and adjust the vibration frequency of the vibration motor to 20 to 60Hz, so that the powder is completely fluidized and dispersed in the powder fluidizing pipe of the reaction chamber; The second step is powder coating reaction. The specific process is as follows: (i) starting the first precursor trimethylaluminum pulse multiple times, with a flow rate of 30 to 100 sccm, a pulse time of 10 ms to 100 ms, and a number of 1 to 10 times, so that the first precursor molecules are adsorbed on the powder surface; (ii) turning off the first precursor pulse, continuing to charge the fluidizing gas, and extracting the unadsorbed first precursor molecules using the vacuum system; (3) starting the second precursor deionized water pulse multiple times, with a flow rate of 30 to 100 sccm, a pulse time of 10 ms to 100 ms, and a number of 1 to 10 times, so that the second precursor molecules react fully with the adsorbed first precursor molecules on the powder surface; (iv) turning off the second precursor pulse, continuing to charge the fluidizing gas, and using the vacuum system to extract the reaction byproducts and unreacted second precursor molecules; (V) Repeat steps (I) to (IV) according to the thickness of the coating required for the powder; The third step is powder collection. The specific process is as follows: Open the discharge port, increase the fluidizing gas flow rate to 1000sccm to 8000sccm, and collect the coated powder through the powder discharge device; or use the combined effect of a vacuum pump with large suction capacity and fluidizing gas to collect the coated powder through the downward powder conveying pipe and the powder discharge device; Step 4: Start the next batch of powder coating; Repeat the first step to the third step, feed the next batch of powder from the powder feeding device, and carry out the next batch of powder coating operation.