Preparation method of metal oxide nano layer, metal oxide nano laminated structure and sensor
Through the focused ion beam exposure technology, the existing metal oxide nanolayer preparation methods are solved, and nanolayer preparation with simple operation and low cost is achieved under low temperature conditions, suitable for flexible substrates and patterning and provide seed layers for a variety of nanostructures.
Patent Information
- Application Number
- CN202411028931.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing metal oxide nanolayer preparation methods are complex in operation, harsh reaction conditions, high cost, and difficult to achieve patterned growth on a flexible substrate.
The metal salt layer is exposed by focusing ion beams to convert it into metal oxide nanolayers. Patterning is achieved by controlling the ion beam parameters, reducing reaction temperature and cost, and carrying out the entire process under low temperature conditions, suitable for flexible lining end.
It realizes the preparation of metal oxide nanolayers with simple operation, low cost, low toxicity and high substrate compatibility. It can be patterned in designated areas, meets a variety of processing needs, and grows materials in other dimensions such as nanowires and nanometers. Sheets and nanorods provide seed layers.
Smart Images

Figure CN118957550A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of metal oxide nanolayer preparation, and specifically relates to a method for preparing a metal oxide nanolayer, a metal oxide nanolaminate structure and a sensor. Background Art
[0002] With the development of science and technology, sensors are increasingly widely used. In related technologies, metal oxide nanolayers are usually prepared by wet chemical methods and gas phase methods to prepare sensors. However, the above preparation methods are complicated to operate, have harsh reaction conditions, and have high preparation costs. Summary of the invention
[0003] In view of this, the first aspect of the present application provides a method for preparing a metal oxide nanolayer, the preparation method comprising:
[0004] Providing a substrate and a metal salt substrate;
[0005] Placing a metal salt substrate on the surface of the substrate to form a metal salt layer disposed on one side of the substrate;
[0006] The metal salt layer is exposed by using a focused ion beam to convert the metal salt layer into a metal oxide nanolayer.
[0007] The metal salt layer includes an area to be exposed and a non-exposed area, and the step of exposing the metal salt layer using the focused ion beam includes:
[0008] Exposing the metal salt layer in the area to be exposed to light, so that the metal salt layer in the area to be exposed is converted into the metal oxide nanolayer to obtain a laminated structure to be processed;
[0009] The stacked structure to be processed is immersed in a processing solution to remove the metal salt layer in the non-exposed area.
[0010] Wherein, after the step of immersing the to-be-processed stacked structure in a processing solution, the metal salt layer in the non-exposed area is dissolved, and the substrate corresponding to the non-exposed area is exposed.
[0011] Wherein, after the step of removing the metal salt layer in the non-exposed area, the method further comprises:
[0012] A plurality of metal oxide nanorods arranged at intervals are obtained, and the metal oxide nanolayer is composed of the plurality of metal oxide nanorods.
[0013] Wherein, the metal oxide nanolayer further includes a doping element, and the doping element is selected from at least one of transition elements.
[0014] Wherein, the metal salt substrate and the metal salt layer satisfy at least one of the following conditions:
[0015] The concentration c of the metal salt substrate satisfies the following conditions: c≥0.015 mol / L;
[0016] The thickness H of the metal salt layer satisfies the following condition: H≥50 nm.
[0017] The metal oxide nanolayer is composed of a plurality of nanorods, the height h of the nanorods satisfies the following condition: 0<h≤1000nm, and the width w of the nanorods satisfies the following condition: 10nm≤w≤200nm.
[0018] The second aspect of the present application provides a metal oxide nano-laminated structure, which includes a substrate and a metal oxide nano-layer arranged on one side of the substrate, and the metal oxide nano-layer is obtained by the preparation method of the metal oxide nano-layer provided in the first aspect of the present application.
[0019] A third aspect of the present application provides a sensor, comprising a conductive layer and the metal oxide nano-laminated structure provided in the second aspect of the present application, wherein the conductive layer is electrically connected to the metal oxide nano-layer.
[0020] The present application provides a preparation method of a metal oxide nanolayer, a metal oxide nanolaminated structure and a sensor, wherein a focused ion beam is used to expose a metal salt layer to decompose the ions of the metal salt layer, thereby converting the metal salt layer into a metal oxide nanolayer. The preparation method is simple to operate, has low reaction conditions, low cost, low toxicity and high substrate compatibility. Furthermore, by controlling the focused ion beam, the preparation of the metal oxide nanolayer can be achieved in a specified area, that is, the patterning of the metal oxide nanolayer can be achieved to meet various processing requirements.
[0021] Specifically, compared to the metal oxide nanolayer prepared by the gas phase method, which cannot be applied on a flexible substrate, the entire process of the preparation method provided by the present application is carried out under a low temperature process, the reaction conditions are loose, and the compatibility with the substrate is good. In addition, the metal oxide nanolayer generated by the preparation method of the present application has great application potential and can be used as a seed layer to grow materials of other dimensions, such as nanowires, nanosheets, nanorods, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the implementation modes of the present application, the drawings required for use in the implementation modes of the present application will be described below.
[0023] Figure 1 A schematic flow chart of a method for preparing a metal oxide nanolayer provided in one embodiment of the present application.
[0024] Figure 2A schematic flow chart of a method for preparing a metal oxide nanolayer provided in another embodiment of the present application.
[0025] Figure 3 The process flow of the method for preparing the metal oxide nanolayer provided in one embodiment of the present application is as follows: Figure 1 .
[0026] Figure 4 The process flow of the method for preparing the metal oxide nanolayer provided in one embodiment of the present application is as follows: Figure 2 .
[0027] Figure 5 The process flow of the method for preparing the metal oxide nanolayer provided in one embodiment of the present application is as follows: Figure 3 .
[0028] Figure 6 The process flow of the method for preparing the metal oxide nanolayer provided in one embodiment of the present application is as follows: Figure 4 .
[0029] Figure 7 This is a SEM image of an unexposed zinc acetate film provided in one embodiment of the present application.
[0030] Figure 8 This is a SEM image of a ZnO metal oxide nanolayer formed by exposure according to one embodiment of the present application.
[0031] Fig. 9 for Figure 8 Locally enlarged SEM image.
[0032] Fig.10 for Figure 8 SEM image from another perspective
[0033] Fig.11 This is a SEM image of a Co-Ni doped ZnO metal oxide nanolayer provided in one embodiment of the present application.
[0034] Fig.12 Process flow of a method for preparing a sensor provided in one embodiment of the present application Figure 1 .
[0035] Fig.13 Process flow of a method for preparing a sensor provided in one embodiment of the present application Figure 2 .
[0036] Fig.14 Process flow of a method for preparing a sensor provided in one embodiment of the present application Figure 3 .
[0037] Fig.15Process flow of a method for preparing a sensor provided in one embodiment of the present application Figure 4 .
[0038] Fig.16 Process flow of a method for preparing a sensor provided in one embodiment of the present application Figure 5 .
[0039] Description of labels:
[0040] Metal oxide nano-laminated structure 1, substrate 10, metal salt layer 11, metal oxide nano-layer 12, metal oxide nano-strip 121, focused ion beam 2, sensor 3, conductive layer 31, UV negative resist 32. DETAILED DESCRIPTION
[0041] The following are preferred implementations of the present application. It should be noted that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
[0042] Unless otherwise specified or there is a contradiction, the terms and phrases used in this application have the following meanings:
[0043] In this application, "first", "second", etc. are used only for descriptive purposes and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0044] In this application, "one or several" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0045] The value of x in the chemical formula: if it is clearly defined, it shall be within the defined range. If it is not clearly defined, it can be determined based on the deposition in a stoichiometric, substoichiometric or superstoichiometric manner in the magnetron sputtering process.
[0046] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be connected, detachably connected, or integrated. It can be mechanically connected or electrically connected. It can be directly connected or indirectly connected through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances.
[0047] The following is a detailed introduction to the preparation of metal oxide nanolayers using wet chemical methods and gas phase methods in related technologies.
[0048] The wet chemical method mainly refers to the reaction of the target metal oxide nanolayer in a hot liquid. The liquid is composed of chemical substances for adjusting the pH (such as NaOH, urotropine, etc.) and salts containing the target metal (such as zinc nitrate hexahydrate, nickel nitrate hexahydrate, etc.). The wet chemical method can be divided into hydrothermal method and microwave hydrothermal method. The disadvantage is that it cannot grow directly in a specified micro-area. In other words, if you want to grow a nanolayer on a patterned micro-area, you first need to pattern the seed layer or expose the patterned seed layer area to the hot liquid through a mask.
[0049] The full name of the gas phase method is chemical vapor deposition, which can be divided into gas-solid and gas-liquid-solid according to the principle process. The target metal or its oxide powder is used as a raw material, and it becomes a gas phase under a high temperature (for example, 500℃-1200℃) environment (for example, normal pressure, vacuum, etc.), and then the gas phase is brought to the substrate by a carrier gas (or reacts with a carrier gas at the same time), and the target metal oxide semiconductor is precipitated on the substrate or on the catalyst. The disadvantage is first that the reaction conditions are harsh, and high temperature, vacuum, carrier gas, etc. make the operation complicated and the cost increased; secondly, if it is necessary to grow in a specified micro-area, the catalyst must first be patterned on the substrate in the specified area; the disadvantage is that it is completely unsuitable to grow nanolayers on flexible substrates at high temperatures.
[0050] Please refer to Figure 1 This embodiment provides a method for preparing a metal oxide nanolayer, the preparation method comprising:
[0051] S100, providing a substrate and a metal salt substrate.
[0052] Optionally, the material of the substrate may be Si, quartz, SiO2, PI, PET, PDMS, etc.
[0053] Before providing the substrate, the process further includes: cleaning the substrate and bombarding the substrate with plasma. For example, the substrate is ultrasonically cleaned in acetone, ethanol and deionized water in sequence. For another example, the substrate is bombarded with Ar / O2 / Ar+O2 plasma to remove organic residues on the substrate and flatten the substrate.
[0054] By cleaning and plasma bombarding the substrate, impurities on the substrate are removed, the substrate is flattened, and the hydrophilicity of its surface is increased, so that the subsequent metal salt substrate arranged on the substrate surface can be quickly expanded and evenly distributed, providing a basis for the subsequent formation of a uniform metal salt layer.
[0055] Optionally, the non-metal ions in the metal salt substrate are selected from at least one of acetate ions, formate ions, propionate ions, and butyrate ions; the metal ions in the metal salt substrate are selected from at least one of zinc ions, copper ions, cobalt ions, titanium ions, molybdenum ions, and tin ions. For example, the metal salt substrate can be zinc acetate, copper acetate, cobalt acetate, titanium acetate, molybdenum acetate, tin acetate, etc.
[0056] It should be noted that the metal salt substrate also includes hydrates of the above-mentioned components. In addition, the metal salt substrate may also be an organic metal salt or a hydrate of a salt other than the above-mentioned.
[0057] Optionally, the concentration c of the metal salt substrate satisfies the following condition: c≥0.015mol / L. Specific examples include, the concentration c of the metal salt substrate can be 0.015mol / L, or 0.02mol / L, or 0.025mol / L, or 0.03mol / L, or 0.035mol / L, or 0.04mol / L, etc. The concentration of the metal salt substrate is based on the formation of a metal salt layer on the substrate. If the concentration of the metal salt substrate is too high or too low, the quality of the subsequently generated metal oxide nanolayer will be reduced. By limiting the concentration of the metal salt substrate c≥0.015mol / L, the quality of the subsequently generated metal oxide nanolayer can be improved.
[0058] Optionally, the thickness H of the metal salt layer satisfies the following condition: H≥50nm. Specifically, for example, the thickness H of the metal salt layer can be 50nm, or 60nm, or 70nm, or 80nm, or 90nm, or 100nm, or 120nm, or 140nm, or 160nm, or 180nm, or 200nm, or 220nm, or 250nm, etc. If the thickness of the metal salt layer is too small, it will be unfavorable for the subsequent generation of the metal oxide nanolayer. If the thickness of the metal salt layer is too large, it will affect the exposure effect of the focused ion beam on the metal salt layer, thereby reducing the quality of the metal oxide nanolayer. By limiting the thickness H of the metal salt layer to 50nm, it is convenient to use the focused ion beam to expose the metal salt layer in the future, thereby improving the quality of the metal oxide nanolayer generated in the future.
[0059] S200, placing a metal salt substrate on the surface of the substrate to form a metal salt layer disposed on one side of the substrate.
[0060] For example, a metal salt solution is spin-coated on a substrate at a certain rotation speed by a spin coating method, thereby forming a metal salt layer.
[0061] For another example, a sublimation / evaporation method is used to slowly heat metal salt powder in a vacuum environment to convert it into a gas phase, and a substrate is placed above the metal salt powder to receive the deposition of the gas phase, thereby forming a metal salt layer.
[0062] S300, exposing the metal salt layer with a focused ion beam to convert the metal salt layer into a metal oxide nanolayer.
[0063] It should be noted that the structures constituting the nanolayer include but are not limited to nanowires, nanorods, and the like.
[0064] Optionally, the metal oxide nanolayer is composed of a plurality of nanorods, the height h of the nanorods satisfies the following condition: 0<h≤1000nm, and the width w of the nanorods satisfies the following condition: 10nm≤w≤200nm.
[0065] Specific examples include, the height h of the nanorod can be 20nm, or 50nm, or 80nm, or 100nm, or 150nm, or 200nm, or 250nm, or 300nm, or 350nm, or 400nm, or 500nm, or 600nm, or 700nm, or 800nm, or 900nm, or 1000nm, etc. The width w of the nanorod can be 10nm, or 20nm, or 25nm, or 30nm, or 35nm, or 40nm, or 45nm, or 50nm, or 55nm, or 60nm, or 80nm, or 100nm, or 120nm, or 150nm, or 180nm, or 200nm, etc. For example, a plurality of nanorod arrays are arranged on a substrate and form a metal oxide nanolayer, and the plurality of nanorods are in contact with each other and / or spaced from each other.
[0066] The method of exposing the metal salt layer by a focused ion beam decomposes the ions in the metal salt layer, thereby converting the metal salt layer into a metal oxide nanolayer. The preparation method is simple to operate, has low reaction conditions, low cost, low toxicity, and high substrate compatibility. In addition, by controlling the focused ion beam, the preparation of the metal oxide nanolayer can be achieved in a specified area, that is, the patterning of the metal oxide nanolayer can be achieved to meet various processing requirements.
[0067] Specifically, compared to the metal oxide nanolayer prepared by the gas phase method, which cannot be applied on a flexible substrate, the entire process of the preparation method provided in this embodiment is carried out under a low temperature process, the reaction conditions are loose, and the compatibility with the substrate is good. In addition, the metal oxide nanolayer generated by the preparation method of this embodiment has great application potential and can be used as a seed layer to grow materials of other dimensions, such as nanowires, nanosheets, nanorods, etc.
[0068] In addition, the preparation method proposed in this embodiment can be used as a parallel preparation method of metal oxide nanolayers by wet chemical method and gas phase method. The advantages of these three methods are complementary and can provide new solutions for different processing requirements.
[0069] In one embodiment, the focused ion beam satisfies at least one of the following conditions: an acceleration voltage V of the focused ion beam satisfies the following condition: 1 kV≤V≤50 kV. Specific examples include that the acceleration voltage V of the focused ion beam may be 1 kV, or 5 kV, or 10 kV, or 15 kV, or 20 kV, or 25 kV, or 30 kV, or 35 kV, or 40 kV, or 45 kV, or 50 kV, etc.
[0070] The accelerating voltage of the focused ion beam is usually selected to correspond to the stable operating voltage of the ion source, for example, Ga + The acceleration voltage of the ion source can be selected as 30 kV or others. The selection of the acceleration voltage is based on achieving ion energy sufficient to decompose the metal salt layer.
[0071] And / or, the beam spot S of the focused ion beam satisfies the following condition: 0≤S≤200nm. Specific examples include that the beam spot S of the focused ion beam can be 10nm, or 20nm, or 30nm, or 40nm, or 50nm, or 60nm, or 70nm, or 80nm, or 90nm, or 100nm, or 120nm, or 140nm, or 160nm, or 180nm, or 200nm, etc.
[0072] And / or, the dwell time t1 of the focused ion beam satisfies the following condition: 0<t1≤100μs. Specific examples include that the dwell time t1 of the focused ion beam can be 10μs, or 30μs, or 50μs, or 80μs, or 100μs, etc.
[0073] The beam spot and dwell time of the focused ion beam may affect the morphology of the metal oxide nanolayer, and can be selected according to the pattern of the metal oxide nanolayer to be prepared.
[0074] Therefore, in actual preparation, various parameters of the focused ion beam can be adaptively adjusted according to actual needs, for example, they can be adjusted according to the properties of the metal salt substrate and the thickness of the metal salt layer.
[0075] In summary, this embodiment limits various parameters of the focused ion beam so that the focused ion beam satisfies at least one of the above conditions to ensure that the focused ion beam has sufficient energy to expose the metal salt layer, decompose the metal salt, and thus convert the metal salt layer into a metal oxide nanolayer.
[0076] Please refer to Figure 2 In one embodiment, the metal salt layer includes an area to be exposed and a non-exposed area, and the step of exposing the metal salt layer using the focused ion beam includes:
[0077] S310, exposing the metal salt layer in the area to be exposed to convert the metal salt layer in the area to be exposed into the metal oxide nanolayer to obtain a laminated structure to be processed.
[0078] For example, a pattern to be exposed is imported or generated in a focused ion beam (FIB) equipment control system, and the pattern area is exposed. The pattern area is the area to be exposed.
[0079] S320, immersing the stacked structure to be processed in a processing solution to remove the metal salt layer in the non-exposed area.
[0080] Optionally, the treatment solution is selected from one of water, ethanol, ether, and chloroform. The treatment solution is usually a solvent that can dissolve the metal salt substrate. In actual preparation, it can be selected according to the properties of the metal salt substrate.
[0081] Optionally, in the step of soaking the laminated structure to be treated, the soaking time t2 satisfies the following condition: 0<t2≤2h; and / or the temperature T of the treatment solution satisfies the following condition: 50℃≤T≤80℃.
[0082] Specific examples include, the immersion time t2 can be 0.2h, or 0.5h, or 0.7h, or 1h, or 1.2h, or 1.5h, or 1.7h, or 2h, etc. The temperature T of the treatment solution can be 50°C, or 55°C, or 60°C, or 65°C, or 70°C, or 75°C, or 80°C, etc. By limiting the immersion time and the temperature of the treatment solution, the metal salt layer in the non-exposed area can be fully removed, thereby improving the preparation efficiency.
[0083] Wherein, after the step of immersing the to-be-processed stacked structure in a processing solution, the metal salt layer in the non-exposed area is dissolved, and the substrate corresponding to the non-exposed area is exposed.
[0084] In summary, through the processing characteristics of "direct writing" based on focused ion beam (importing the pattern to be exposed in the equipment control software), the growth of metal oxide nanolayers in the specified pattern (micro-area) can be easily achieved, and the pattern width of the metal oxide nanolayer can be easily reduced to sub-micron level. In addition, the metal salt layer in the non-exposed area is removed by immersion in the treatment solution, which is simple and convenient to operate and has low preparation difficulty.
[0085] In one embodiment, after the step of removing the metal salt layer in the non-exposed area, the method further comprises:
[0086] A plurality of metal oxide nanorods arranged at intervals are obtained, and the metal oxide nanolayer is composed of the plurality of metal oxide nanorods.
[0087] The plurality of metal oxide nano-strips are arranged along an arrangement direction perpendicular to the substrate to the metal oxide nano-layer. The plurality of metal oxide nano-strips are spaced from each other and arranged on the substrate.
[0088] This embodiment only schematically illustrates the patterning of a metal oxide nanolayer to obtain a plurality of metal oxide nanostrips, and does not mean that the preparation method of the metal oxide nanolayer provided in this application is only applicable to the preparation of metal oxide nanostrips. The preparation method of the metal oxide nanolayer provided in this application can be used to pattern the metal oxide nanolayer according to product requirements, and the shape of the patterned metal oxide nanolayer includes but is not limited to strips, triangles, quadrilaterals, polygons, circles, rings, trapezoids, etc.
[0089] In one embodiment, the metal oxide nanolayer further includes a doping element, and the doping element is selected from at least one of transition elements.
[0090] Optionally, the transition element is selected from at least one of titanium, molybdenum, manganese, iron, cobalt, nickel, and copper. Specific examples include that the transition element may be titanium (Ti), molybdenum (Mo), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), etc. It should be noted that the transition element may also be other transition elements except titanium, molybdenum, manganese, iron, cobalt, nickel, and copper.
[0091] After the step of obtaining the metal oxide nanolayer by focused ion beam exposure, the metal oxide nanolayer is subjected to a preset treatment so that the metal oxide nanolayer further includes a doping element, wherein the doping element is selected from at least one of transition elements. The preset treatment may be a hydrothermal method or an ion implantation method.
[0092] For example, after a metal oxide nanolayer is obtained by focused ion beam exposure, a hydrothermal method is used to allow the metal oxide nanolayer to further include doping elements, thereby increasing the application range of the metal oxide nanolayer.
[0093] The present application also provides a metal oxide nano-laminated structure, which includes a substrate and a metal oxide nano-layer arranged on one side of the substrate, and the metal oxide nano-layer is obtained by the preparation method of the metal oxide nano-layer provided in the present application.
[0094] Among them, the metal oxide nano-laminated structure can be applied to various sensors, such as photoelectric sensors, gas sensors, electrochemical sensors, piezoelectric sensors, etc.
[0095] The metal oxide nano-laminated structure provided in this embodiment uses a focused ion beam to expose the metal salt layer to decompose the ions in the metal salt layer, thereby converting the metal salt layer into a metal oxide nano-layer, which is simple to operate, has low reaction conditions, low cost, low toxicity, and high substrate compatibility. In addition, by controlling the focused ion beam, the preparation of the metal oxide nano-layer can be achieved in a specified area, that is, the patterning of the metal oxide nano-layer can be achieved, meeting various processing requirements.
[0096] The present application also provides a sensor, which includes a conductive layer and the metal oxide nano-laminated structure provided above in the present application, wherein the conductive layer is electrically connected to the metal oxide nano-layer.
[0097] The sensor can be a photoelectric sensor, a gas sensor, an electrochemical sensor, a piezoelectric sensor, etc. Specifically, the conductive layer and the metal oxide nanolayer are arranged on the same side of the substrate, and the conductive layer is directly connected to the metal oxide nanolayer. The material of the conductive layer is selected from metals or alloys, such as chromium, gold, etc.
[0098] In order to make the purpose and advantages of the present application more clear, the preparation method of the metal oxide nanolayer of the present application is further described in detail below in conjunction with specific examples.
[0099] Embodiment 1:
[0100] First, if Figure 3 As shown, a SiO2 oxide wafer is used as a substrate 10, the SiO2 oxide wafer is cleaned, and the SiO2 oxide wafer is ultrasonically treated with acetone, ethanol and deionized water in sequence, the concentrations of the selected acetone and ethanol are both analytically pure, and then the substrate surface is bombarded with oxygen plasma and argon plasma to obtain hydrophilicity.
[0101] Afterwards, if Figure 4 As shown, a zinc acetate ethanol solution with a molar concentration of 0.035 mol / L is used, and 35 μL of the solution is spin-coated on a SiO2 oxide sheet at a rotation speed of 600 rpm, and then the ethanol is waited for evaporation and dried to obtain a zinc acetate film with a thickness of about 150 nm. The zinc acetate film is the metal salt layer 11.
[0102] Furthermore, if Figure 5 As shown, a focused ion beam 2 is used to expose the set area to be exposed (acceleration voltage: 30 kV; beam spot: 50 nm; dwell time: 0.2 μs; beam current: 20 pA; micro-area pattern and size: 700 nm×30 μm×6), so that the metal salt layer 11 in the area to be exposed is converted into a metal oxide nanolayer 12 to obtain a laminated structure to be processed.
[0103] Then, if Figure 6As shown, the laminated structure to be processed is immersed in deionized water to remove the metal salt layer 11 in the non-exposed area, thereby obtaining the metal oxide nano-laminated structure 1.
[0104] Among them, the unexposed zinc acetate film, that is, the metal salt layer in the non-exposed area, such as Figure 7 As shown. Figure 7 In the SEM image, SEM HV is 5.0kV, WD is 8.10mm, SEM MAG is 60.6kx, and View field is 3.43μm.
[0105] The ZnO metal oxide nanolayer 12 formed by exposure, such as Figure 8 As shown, the metal oxide nanolayer 12 is composed of 6 metal oxide nanorods 121, each of which is 700 nm×30 μm. Figure 8 In the SEM image, the EHT is 3.00kV, the WD is 5.8mm, and the SEM MAG is 1.50kx.
[0106] A local magnified SEM image of a single metal oxide nanorod 121 is shown in FIG. Fig. 9 As shown. Fig. 9 In the SEM image, the EHT is 3.00kV, the WD is 5.8mm, and the SEM MAG is 40.00kx.
[0107] The SEM image of a single metal oxide nanorod 121 at an oblique viewing angle is shown in FIG. Fig.10 As shown. Fig.10 In the SEM image, the EHT is 4.50kV, the WD is 14.4mm, and the SEM MAG is 15.00kx.
[0108] Embodiment 2:
[0109] On the basis of Example 1, a Co-Ni doped ZnO metal oxide nanolayer was prepared.
[0110] The preparation was carried out by a hydrothermal method, i.e., a ZnO metal oxide nanolayer was used as a seed layer to hydrothermally grow a Co-Ni doped ZnO metal oxide nanolayer. Specifically, zinc nitrate hexahydrate and urotropine were uniformly mixed in equal volumes at a concentration of 0.015 mol / L, and then cobalt nitrate hexahydrate and nickel nitrate hexahydrate (Ni:Co:Zn=4:4:100) with an atomic ratio of 4% were doped, the reaction temperature was 95°C, the reaction time was 150 minutes, and then the sample was taken out and dried under N2 to obtain a Co-Ni doped ZnO metal oxide nanolayer.
[0111] Co-Ni doped ZnO metal oxide nanolayers, such as Fig.11 As shown. Fig.11In the SEM image, the EHT is 4.50kV, the WD is 8.6mm, and the SEM MAG is 8.00kx.
[0112] Embodiment 3:
[0113] Based on Example 1, an MSM type UV sensor with a photosensitive structure was prepared.
[0114] First, the process of preparing the patterned ZnO metal oxide nanolayer by using a focused ion beam is the same as that in Example 1, except that the size of the pattern is set to 15 μm×45 μm.
[0115] Afterwards, if Figure 12-16 As shown, the key point of preparing the MSM type UV sensor 3 is to deposit a Cr / Au (20nm / 100nm) conductive layer 31 on both sides of the metal oxide nanolayer 12 .
[0116] UV negative photoresist 32 was used for UV lithography, the photoresist thickness was 2 μm, and the exposure parameters were 100 mJ / cm 2 , developing time 45s, fixing time 30s. Fig.13 After local exposure, Fig.14 Then, a stripping process was performed using acetone, and then the prepared UV sensor 3 was dried by nitrogen.
[0117] The above is a detailed introduction to the contents provided in the implementation mode of the present application. This article explains and illustrates the principles and implementation modes of the present application. The above explanation is only used to help understand the method and core idea of the present application. At the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation mode and application scope. In summary, the contents of this specification should not be understood as limiting the present application.
Claims
1. A method for preparing a metal oxide nanolayer, characterized in that: The preparation method comprises: Providing a substrate and a metal salt substrate; Placing a metal salt substrate on the surface of the substrate to form a metal salt layer disposed on one side of the substrate; The metal salt layer is exposed by using a focused ion beam to convert the metal salt layer into a metal oxide nanolayer.
2. The method for preparing a metal oxide nanolayer according to claim 1, characterized in that: The metal salt layer includes an area to be exposed and a non-exposed area, and the step of exposing the metal salt layer using the focused ion beam includes: Exposing the metal salt layer in the area to be exposed to light, so that the metal salt layer in the area to be exposed is converted into the metal oxide nanolayer to obtain a laminated structure to be processed; The stacked structure to be processed is immersed in a processing solution to remove the metal salt layer in the non-exposed area.
3. The method for preparing a metal oxide nanolayer according to claim 2, characterized in that: After the step of immersing the stacked structure to be processed in a processing solution, the metal salt layer in the non-exposed area is dissolved, and the substrate corresponding to the non-exposed area is exposed.
4. The method for preparing a metal oxide nanolayer according to claim 2, characterized in that: After the step of removing the metal salt layer in the non-exposed area, the method further comprises: A plurality of metal oxide nanorods arranged at intervals are obtained, and the metal oxide nanolayer is composed of the plurality of metal oxide nanorods.
5. The method for preparing a metal oxide nanolayer according to claim 1, characterized in that: The metal oxide nanolayer further comprises a doping element, and the doping element is selected from at least one of transition elements.
6. The method for preparing a metal oxide nanolayer according to any one of claims 1 to 5, characterized in that: The metal salt substrate and the metal salt layer satisfy at least one of the following conditions: The concentration c of the metal salt substrate satisfies the following conditions: c≥0.015 mol / L; The thickness H of the metal salt layer satisfies the following condition: H≥50 nm.
7. The method for preparing a metal oxide nanolayer according to any one of claims 1 to 5, characterized in that: The metal oxide nanolayer is composed of a plurality of nanorods, the height h of the nanorods satisfies the following condition: 0<h≤1000nm, and the width w of the nanorods satisfies the following condition: 10nm≤w≤200nm.
8. A metal oxide nano-laminated structure, characterized in that: The metal oxide nano-laminated structure comprises a substrate and a metal oxide nano-layer arranged on one side of the substrate, and the metal oxide nano-layer is obtained by the preparation method of the metal oxide nano-layer according to any one of claims 1 to 7.