Preparation method of cobalt-based lattice strain oxygen evolution reaction catalyst
Through the preparation method of the cobalt-based lattice strain oxygen-analysis reaction catalyst, the lattice strain of the catalyst is regulated by gas-phase phosphating and electrochemical oxidation processes, the problem of catalyst activity regulation in the prior art is solved, the overpotential of the catalyst is reduced and the overpotential of the catalyst is improved. Efficiency of electrolyzing water to produce hydrogen.
Patent Information
- Application Number
- CN202411039122.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
In the prior art, there are difficulties in the regulation of activity during phase reconstruction in alkaline media, and the experimental conditions of conventional lattice strain strategies are harsh and complex, making it difficult to effectively regulate the electronic structure of the catalyst active site. .
The preparation method of a cobalt-based lattice strain oxygen-analysis reaction catalyst is adopted to regulate the lattice strain of the precatalyst through gas-phase phosphating and electrochemical oxidation processes to form CoOOH nanosheets, reducing overpotential and improving catalytic performance.
It realizes the reduction of the overpotential of the catalyst without introducing foreign components, promotes the electrocatalytic water decomposition and hydrogen production reaction, reduces the energy consumption of the energy conversion device, and improves the electrolysis by adjusting the Co-O bond length and the valence state of the active site. Efficiency of water to produce hydrogen.
Smart Images

Figure CN118957634A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oxygen evolution reaction catalyst preparation, in particular to a method for preparing a cobalt-based lattice strained oxygen evolution reaction catalyst. Background Art
[0002] Hydrogen is expected to replace fossil energy and become the carrier of future energy. In recent years, transition metal cobalt-based catalysts such as oxides, nitrides, phosphides, sulfides and selenides have been widely reported as catalysts for oxygen evolution reaction in alkaline media. However, the catalysts for oxygen evolution reaction are reconstructed in alkaline media. Compared with directly synthesized oxyhydroxides, oxyhydroxides formed by in-situ reconstruction of precatalysts often show stronger catalytic activity.
[0003] Lattice strain engineering causes changes in interatomic distances, which is a very effective strategy for regulating the electronic structure and local coordination environment of catalyst active sites, and has great potential to overcome the limitations of component regulation. Conventional methods of inducing strain include heat treatment, morphology design, core-shell structure, alloying, doping, etc., but the experimental conditions required are harsh, the experimental process is complicated, or unnecessary components are often introduced, making actual experimental operations difficult. Developing new lattice strain induction strategies to regulate the electronic structure of catalyst active sites has become a difficulty in developing advanced catalysts.
[0004] Therefore, it is necessary to design a cobalt-based catalyst with lattice strain to achieve the regulation of the degree of strain on the performance of the oxygen evolution reaction and to conduct in-depth research on the "structure-activity relationship" between material structure and catalytic activity. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst to solve the problems in the prior art.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst, the preparation method comprising the following steps:
[0008] S1. Weigh Co(NO3)2·6H2O and CO(NH2)2 and dissolve them in the mixed solution in a beaker, and stir at room temperature to obtain solution A;
[0009] S2, transferring solution A to a stainless steel reactor lined with polytetrafluoroethylene, separating the intermediate product by vacuum filtration, and washing and drying to obtain solid powder B;
[0010] S3, grinding the solid powder B obtained in S2, and annealing it in a ceramic ark to obtain solid powder C;
[0011] S4, respectively weighing solid powder C and NaH2PO2·H2O and placing them in different ceramic arks, placing the ceramic arks in a tube furnace for annealing to obtain the precatalyst CoPxNR;
[0012] S5, weigh the pre-catalyst solid powder obtained in S4, and disperse it in the mixed solution in the centrifuge tube, obtain the pre-catalyst slurry by ultrasonication at room temperature, and drop the slurry onto the hydrophilic carbon paper and dry it;
[0013] S6. The pre-catalyst supported on the carbon paper was oxidized for 10 h, and then washed and dried to obtain the oxygen evolution reaction catalyst CoOOHx NS supported on the carbon paper.
[0014] Furthermore, the mixed solution in the beaker in S1 is a mixture of 15 mL of deionized water and 15 mL of anhydrous ethanol, and the stirring time is 10-15 min.
[0015] Furthermore, the specific operation in S2 includes placing the reactor in an oven for hydrothermal reaction, maintaining it at 100°C for 10 hours, and after the reaction is completed and naturally cooled to room temperature, taking out the reactor to obtain a solid-liquid phase mixture, washing it with deionized water for 3-5 times, and finally drying it at 60°C in a vacuum environment for 8-12 hours to obtain solid powder B.
[0016] Furthermore, the grinding time in S3 is 5-10 minutes, and the annealing conditions in the tube furnace are: an air atmosphere with a temperature of 350° C. and an annealing time of 2 hours.
[0017] Furthermore, the specific operation in S4 is: weighing 50 mg of solid powder C and placing it in a ceramic ark 1;
[0018] Weigh 500-2000 mg of NaH2PO2·H2O and place it in Ceramic Ark 2;
[0019] Ceramic ark one is placed downstream of the air flow of the tubular furnace, and ceramic ark two is placed upstream of the air flow of the tubular furnace. The distance between ceramic ark one and ceramic ark two is 2-4 cm. Annealing is carried out in an argon atmosphere at 350°C in the tubular furnace for 2 hours to obtain pre-catalyst CoPxNR, i.e., cobalt phosphide nanorods.
[0020] Furthermore, the specific operation in S5 is: weighing 5 mg of pre-catalyst solid powder, and dispersing it in a mixture of 30 μL of Nafion solution, 250 μL of deionized water and 750 μL of anhydrous ethanol in a centrifuge tube, and ultrasonicating at room temperature for 1-2 hours to obtain a pre-catalyst slurry;
[0021] Under the infrared lamp, use a pipette to take a total of 200 μL of slurry in small amounts and multiple times and evenly apply it on one side to 1 cm 2 on hydrophilic carbon paper.
[0022] Furthermore, the specific operation in S6 is: using the prepared pre-catalyst loaded carbon paper as a working electrode, a carbon rod as a counter electrode, Hg|HgO as a reference electrode, and 1M KOH as an electrolyte to form a typical three-electrode system, and applying 10 mA cm by chronopotentiometry using an electrochemical workstation. -2 The pre-catalyst supported on the carbon paper was oxidized for 10 h with a current of 1.5 %.
[0023] The oxidized carbon paper was washed with deionized water for 3-5 times, and dried at 60° C. in a vacuum environment for 8-12 hours to obtain an oxygen evolution reaction catalyst CoOOHxNS, i.e., cobalt oxyhydroxide nanosheets, on the carbon paper.
[0024] Furthermore, the preparation method requires the following raw material mass ratios for preparing the cobalt-based lattice strain oxygen evolution reaction catalyst: 163.7-164 mg of Co(NO3)2·6H2O, 135-135.2 mg of CO(NH2)2, and 500-2000 mg of NaH2PO2·H2O.
[0025] Beneficial effects of the present invention:
[0026] 1. The preparation method of the present invention regulates the lattice strain of the pre-catalyst CoP nanorods by the Kirkendall effect in the process of preparing the pre-catalyst gas phase phosphating, and completely reconstructs the pre-catalyst to form the real active substance CoOOH nanosheets for catalytic oxygen evolution reaction by means of the electrochemical oxidation process under preferred conditions, so as to achieve the regulation of the lattice strain of the catalyst CoOOH nanosheets by the pre-catalyst CoP nanorods; compared with the conventional lattice strain engineering directly acting on the hydroxyl oxide, the in-situ derivatization of the pre-catalyst can reduce the overpotential of the real catalyst oxygen evolution reaction without introducing foreign components, promote the occurrence of oxygen evolution reaction on the anode side of electrocatalytic water decomposition and hydrogen production, and reduce the energy consumption of the energy conversion device;
[0027] 2. The preparation method of the present invention has a simple preparation process and is easy to operate. The lattice strain degree and the local coordination environment of the pre-catalyst are adjusted by changing the amount of the phosphorus source used in the gas phase phosphating process. The synthesized catalyst material derived in situ from the lattice strain of the pre-catalyst has an adjustable Co-O bond length and a Co active site valence state, and can regulate the electronic structure of the Co active site, thereby presenting different electrocatalytic oxygen evolution reaction performances and improving the energy conversion efficiency of hydrogen production by water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The present invention will be further described below in conjunction with the accompanying drawings.
[0029] Figure 1 is the XRD diagram of the lattice strain precatalyst of the present invention;
[0030] Figure 2 It is a local enlarged XRD diagram of the lattice strain precatalyst of the present invention;
[0031] Figure 3 is the FT-EXAFS graph of the lattice strain precatalyst of the present invention;
[0032] Figure 4 is a SEM image of the lattice strain precatalyst of the present invention;
[0033] Figure 5 is a TEM image of the lattice strain precatalyst of the present invention;
[0034] Figure 6 is a SEM image of the in-situ derived lattice strain catalyst of the present invention;
[0035] Figure 7 is a TEM image of the in-situ derived lattice strain catalyst of the present invention;
[0036] Figure 8 is the XANES graph of the lattice strain catalyst derived in situ of the present invention;
[0037] Fig. 9 is a fitting diagram of the lattice strain catalytic valence state derived in situ of the present invention;
[0038] Fig.10 is the FT-EXAFS graph of the in-situ derived lattice strain catalyst of the present invention;
[0039] Fig.11 It is a performance diagram of the in-situ derived lattice strain catalyst of the present invention. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] A method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst. The raw materials required for the preparation of the cobalt-based lattice strain oxygen evolution reaction catalyst are as follows: cobalt nitrate hexahydrate Co(NO3)2·6H2O, urea CO(NH2)2, deionized water, anhydrous ethanol, sodium hypophosphite monohydrate NaH2PO2·H2O, and Nafion solution.
[0042] A method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst, the preparation method comprising the following steps:
[0043] S1. Mix 15 mL of deionized water and 15 mL of anhydrous ethanol in a beaker, weigh 163.7-164 mg of Co(NO3)2·6H2O and 135-135.2 mg of CO(NH2)2 and dissolve them in the mixed solution in the beaker, and stir at room temperature for 10-15 min to obtain solution A.
[0044] S2. Transfer solution A to a stainless steel reactor with a polytetrafluoroethylene liner, then place the reactor in an oven for hydrothermal reaction, keep it at 100°C for 10 hours, and after the reaction is completed and naturally cooled to room temperature, take out the reactor to obtain a solid-liquid mixture, separate the intermediate product by vacuum filtration, wash it with deionized water for 3-5 times, and finally dry it at 60°C in a vacuum environment for 8-12 hours to obtain solid powder B.
[0045] S3. Grind the solid powder B obtained in S2 for 5-10 minutes, place it in a ceramic ark, and anneal it in a tube furnace at 350° C. in an air atmosphere for 2 hours to obtain solid powder C.
[0046] S4, weigh 50 mg of the obtained solid powder C and place it in a ceramic ark 1;
[0047] Weigh 500-2000 mg of NaH2PO2·H2O and place it in Ceramic Ark 2;
[0048] Ceramic ark one is placed downstream of the air flow of the tubular furnace, and ceramic ark two is placed upstream of the air flow of the tubular furnace. The distance between ceramic ark one and ceramic ark two is 2-4 cm. Annealing is carried out in an argon atmosphere at 350°C in the tubular furnace for 2 hours to obtain pre-catalyst CoPxNR, i.e., cobalt phosphide nanorods.
[0049] S5, weighing 5 mg of the pre-catalyst solid powder CoPx NR obtained in S4, and dispersing it in a centrifuge tube containing 30 μL of Nafion solution, 250 μL of deionized water and 750 μL of anhydrous ethanol mixture, and ultrasonicating at room temperature for 1-2 h to obtain a pre-catalyst slurry;
[0050] Under the infrared lamp, use a pipette to take a total of 200 μL of slurry in small amounts and multiple times and evenly apply it on one side to 1 cm 2 on hydrophilic carbon paper.
[0051] S6. In a typical three-electrode system, the carbon paper loaded with precatalyst prepared in S5 was used as the working electrode, the carbon rod was used as the counter electrode, Hg|HgO was used as the reference electrode, and 1 M KOH was used as the electrolyte.
[0052] The electrochemical workstation was used to apply 10 mA cm -2 The pre-catalyst supported on the carbon paper was oxidized for 10 h with a current of 1.5 %.
[0053] Finally, the oxidized carbon paper was washed with deionized water for 3-5 times and dried at 60° C. in a vacuum environment for 8-12 h to obtain the oxygen evolution reaction catalyst CoOOHxNS, i.e., cobalt oxyhydroxide nanosheets, supported on the carbon paper.
[0054] Example 1
[0055] A method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst, the preparation method comprising the following steps:
[0056] S1. Mix 15 mL of deionized water and 15 mL of anhydrous ethanol in a beaker, weigh 163.7 mg of Co(NO3)2·6H2O and 135.2 mg of CO(NH2)2 and dissolve them in the mixed solution in the beaker, and stir at room temperature for 10 min to obtain solution A.
[0057] S2. Transfer solution A to a stainless steel reactor with a polytetrafluoroethylene liner, then place the reactor in an oven for hydrothermal reaction, and keep it at 100°C for 10 hours. After the reaction is completed and naturally cooled to room temperature, take out the reactor to obtain a solid-liquid mixture, separate the intermediate product by vacuum filtration, wash it with deionized water 3 times, and finally dry it at 60°C in a vacuum environment for 8 hours to obtain solid powder B.
[0058] S3. Grind the solid powder B obtained in S2 for 5 minutes, place it in a ceramic ark, and anneal it in a tube furnace at 350° C. in an air atmosphere for 2 hours to obtain solid powder C.
[0059] S4, weigh 50 mg of the obtained solid powder C and place it in a ceramic ark 1;
[0060] Weigh 500 mg of NaH2PO2·H2O and place it in Ceramic Ark 2;
[0061] Ceramic ark one was placed downstream of the airflow of the tubular furnace, and ceramic ark two was placed upstream of the airflow of the tubular furnace. The distance between ceramic ark one and ceramic ark two was 2 cm. The arks were annealed for 2 h in an argon atmosphere at 350° C. in the tubular furnace to obtain pre-catalyst CoP10 NR, i.e., cobalt phosphide nanorods.
[0062] S5, weighing 5 mg of the precatalyst solid powder CoP10NR obtained in S4, and dispersing it in a centrifuge tube containing 30 μL of Nafion solution, 250 μL of deionized water and 750 μL of anhydrous ethanol mixture, and ultrasonicating at room temperature for 1 h to obtain a precatalyst slurry;
[0063] Under the infrared lamp, use a pipette to take a total of 200 μL of slurry in small amounts and multiple times and evenly apply it on one side to 1 cm 2 on hydrophilic carbon paper.
[0064] S6. In a typical three-electrode system, the carbon paper loaded with precatalyst prepared in S5 was used as the working electrode, the carbon rod was used as the counter electrode, Hg|HgO was used as the reference electrode, and 1 M KOH was used as the electrolyte.
[0065] The electrochemical workstation was used to apply 10 mA cm -2 The pre-catalyst supported on the carbon paper was oxidized for 10 h with a current of 1.5 %.
[0066] Finally, the oxidized carbon paper was washed with deionized water three times and dried at 60°C in a vacuum environment for 8 h to obtain the oxygen evolution reaction catalyst CoOOH10NS, i.e., cobalt oxyhydroxide nanosheets, supported on the carbon paper.
[0067] Example 2
[0068] A method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst, the preparation method comprising the following steps:
[0069] S1. Mix 15 mL of deionized water and 15 mL of anhydrous ethanol in a beaker, weigh 163.8 mg of Co(NO3)2·6H2O and 135.1 mg of CO(NH2)2 and dissolve them in the mixed solution in the beaker, and stir at room temperature for 13 min to obtain solution A.
[0070] S2. Transfer solution A to a stainless steel reactor with a polytetrafluoroethylene liner, then place the reactor in an oven for hydrothermal reaction, and keep it at 100°C for 10 hours. After the reaction is completed and naturally cooled to room temperature, take out the reactor to obtain a solid-liquid mixture, separate the intermediate product by vacuum filtration, wash it with deionized water 4 times, and finally dry it at 60°C in a vacuum environment for 10 hours to obtain solid powder B.
[0071] S3. After grinding the solid powder B obtained in S2 for 7 minutes, the solid powder B was placed in a ceramic ark and annealed in a tube furnace at 350° C. in an air atmosphere for 2 hours to obtain a solid powder C.
[0072] S4, weigh 50 mg of the obtained solid powder C and place it in a ceramic ark 1;
[0073] Weigh 1000 mg of NaH2PO2·H2O and place it in Ceramic Ark 2;
[0074] Ceramic ark one was placed downstream of the air flow of the tubular furnace, and ceramic ark two was placed upstream of the air flow of the tubular furnace. The distance between ceramic ark one and ceramic ark two was 3 cm. The arks were annealed for 2 hours in an argon atmosphere at 350° C. in the tubular furnace to obtain pre-catalyst CoP20 NR, i.e., cobalt phosphide nanorods.
[0075] S5, weighing 5 mg of the precatalyst solid powder CoP20NR obtained in S4, and dispersing it in a centrifuge tube containing 30 μL of Nafion solution, 250 μL of deionized water and 750 μL of anhydrous ethanol mixture, and ultrasonicating at room temperature for 1.5 h to obtain a precatalyst slurry;
[0076] Under the infrared lamp, use a pipette to take a total of 200 μL of slurry in small amounts and multiple times and evenly apply it on one side to 1 cm 2 on hydrophilic carbon paper.
[0077] S6. In a typical three-electrode system, the carbon paper loaded with precatalyst prepared in S5 was used as the working electrode, the carbon rod was used as the counter electrode, Hg|HgO was used as the reference electrode, and 1 M KOH was used as the electrolyte.
[0078] The electrochemical workstation was used to apply 10 mA cm -2 The pre-catalyst supported on the carbon paper was oxidized for 10 h with a current of 1.5 %.
[0079] Finally, the oxidized carbon paper was washed with deionized water for 4 times and dried at 60°C in a vacuum environment for 10 h to obtain the oxygen evolution reaction catalyst CoOOH20NS, i.e., cobalt oxyhydroxide nanosheets, supported on the carbon paper.
[0080] Example 3
[0081] A method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst, the preparation method comprising the following steps:
[0082] S1. Mix 15 mL of deionized water and 15 mL of anhydrous ethanol in a beaker, weigh 164 mg of Co(NO3)2·6H2O and 135 mg of CO(NH2)2 and dissolve them in the mixed solution in the beaker, and stir at room temperature for 15 min to obtain solution A.
[0083] S2. Transfer solution A to a stainless steel reactor with a polytetrafluoroethylene liner, then place the reactor in an oven for hydrothermal reaction, and keep it at 100°C for 10 hours. After the reaction is completed and naturally cooled to room temperature, take out the reactor to obtain a solid-liquid mixture, separate the intermediate product by vacuum filtration, wash it with deionized water 5 times, and finally dry it at 60°C in a vacuum environment for 12 hours to obtain solid powder B.
[0084] S3. After grinding the solid powder B obtained in S2 for 10 minutes, the solid powder B was placed in a ceramic ark and annealed in a tubular furnace at 350° C. in an air atmosphere for 2 hours to obtain a solid powder C.
[0085] S4, weigh 50 mg of the obtained solid powder C and place it in a ceramic ark 1;
[0086] Weigh 2000 mg of NaH2PO2·H2O and place it in Ceramic Ark 2;
[0087] Ceramic ark one was placed downstream of the air flow of the tubular furnace, and ceramic ark two was placed upstream of the air flow of the tubular furnace. The distance between ceramic ark one and ceramic ark two was 4 cm. The arks were annealed for 2 hours in an argon atmosphere at 350° C. in the tubular furnace to obtain pre-catalyst CoP40 NR, i.e., cobalt phosphide nanorods.
[0088] S5, weighing 5 mg of the precatalyst solid powder CoP40 NR obtained in S4, and dispersing it in a centrifuge tube containing 30 μL of Nafion solution, 250 μL of deionized water and 750 μL of anhydrous ethanol mixture, and ultrasonicating at room temperature for 2 h to obtain a precatalyst slurry;
[0089] Under the infrared lamp, use a pipette to take a total of 200 μL of slurry in small amounts and multiple times and evenly apply it on one side to 1 cm 2 on hydrophilic carbon paper.
[0090] S6. In a typical three-electrode system, the carbon paper loaded with precatalyst prepared in S5 was used as the working electrode, the carbon rod was used as the counter electrode, Hg|HgO was used as the reference electrode, and 1 M KOH was used as the electrolyte.
[0091] The electrochemical workstation was used to apply 10 mA cm -2 The pre-catalyst supported on the carbon paper was oxidized for 10 h with a current of 1.5 %.
[0092] Finally, the oxidized carbon paper was washed with deionized water for 5 times and dried at 60°C in a vacuum environment for 12 h to obtain the oxygen evolution reaction catalyst CoOOH40 NS supported on the carbon paper, i.e., cobalt oxyhydroxide nanosheets.
[0093] The performance of the in-situ derived lattice strain oxygen evolution reaction catalyst was tested, and the test data are as follows:
[0094] like Figure 1-3 As shown, the XRD and Co K-edge FT-XAFS patterns of the pre-catalyst CoP nanorods prepared by the vapor phase phosphating process indicate that the tubular furnace vapor phase phosphating can prepare a pre-catalyst with a clear phase, and the degree of lattice strain and the local coordination environment of the pre-catalyst can be regulated by changing the amount of phosphorus source.
[0095] like Figure 4 , Figure 5 As shown, the SEM and TEM images of the pre-catalyst CoP nanorods prepared by the vapor phase phosphating process show that the pre-catalyst has a rod-like morphology and circular voids inside, indicating that the vapor phase phosphating process is affected by the Kirkendall effect.
[0096] like Figure 6 , Figure 7 As shown, the SEM and TEM images of CoOOH nanosheets, the oxygen evolution reaction catalyst formed by electrochemical oxidation reconstruction of the precatalyst, show that the oxyhydroxide derived in situ from the precatalyst has a regular hexagonal morphology.
[0097] like Figure 8-10 As shown, the XANES, valence state fitting and FT-EXAFS diagrams of Co K-edge of CoOOH nanosheets, a catalyst for oxygen evolution reaction, formed by electrochemical oxidation reconstruction of the precatalyst revealed that the in-situ derived oxyhydroxides of the precatalysts with different degrees of lattice strain had different local coordination environments and valence states of metal active sites.
[0098] like Fig.11 As shown in the figure, the oxygen evolution reaction performance of catalysts with different lattice strains was tested in a typical three-electrode system. It was found that CoOOH20 NS with the longest Co-O bond length and higher Co active site valence showed the best oxygen evolution reaction performance. It had the lowest reaction potential in 1 M KOH solution and could be driven continuously for up to 10 h at 10 mA cm -2 Current density of oxygen evolution reaction.
[0099] Compared with the related art, the preparation method of the cobalt-based lattice strain oxygen evolution reaction catalyst provided by the present invention has the following beneficial effects:
[0100] First, the lattice strain of the pre-catalyst CoP nanorods is regulated by the Kirkendall effect during the gas phase phosphating process of the pre-catalyst. With the help of the electrochemical oxidation process under optimal conditions, the pre-catalyst is completely reconstructed to form the real active substance CoOOH nanosheets for catalytic oxygen evolution reaction, so as to achieve the regulation of the lattice strain of the catalyst CoOOH nanosheets by the pre-catalyst CoP nanorods;
[0101] Compared with conventional lattice strain engineering that directly acts on hydroxide oxides, in situ derivatization of pre-catalysts can reduce the overpotential of the oxygen evolution reaction of the real catalyst without introducing foreign components, promote the occurrence of oxygen evolution reaction on the anode side of electrocatalytic water decomposition to produce hydrogen, and reduce the energy consumption of the energy conversion device.
[0102] Second, the preparation process is not only simple and easy to operate, but also can adjust the lattice strain degree and local coordination environment of the pre-catalyst by changing the amount of phosphorus source used in the gas phase phosphating process. The synthesized catalyst material derived in situ from the lattice strain of the pre-catalyst has an adjustable Co-O bond length and Co active site valence state, and can regulate the electronic structure of the Co active site, thereby presenting different electrocatalytic oxygen evolution reaction performances and improving the energy conversion efficiency of hydrogen production by water electrolysis.
[0103] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst, characterized in that: The preparation method comprises the following steps: S1. Weigh Co(NO3)2·6H2O and CO(NH2)2 and dissolve them in the mixed solution in a beaker, and stir at room temperature to obtain solution A; S2, transferring solution A to a stainless steel reactor lined with polytetrafluoroethylene, separating the intermediate product by vacuum filtration, and washing and drying to obtain solid powder B; S3, grinding the solid powder B obtained in S2, and annealing it in a ceramic ark to obtain solid powder C; S4, respectively weighing solid powder C and NaH2PO2·H2O and placing them in different ceramic arks, placing the ceramic arks in a tube furnace for annealing to obtain the precatalyst CoPxNR; S5, weigh the pre-catalyst solid powder obtained in S4, and disperse it in the mixed solution in the centrifuge tube, obtain the pre-catalyst slurry by ultrasonication at room temperature, and drop the slurry onto the hydrophilic carbon paper and dry it; S6. The pre-catalyst supported on the carbon paper was oxidized for 10 h, and then washed and dried to obtain the oxygen evolution reaction catalyst CoOOHx NS supported on the carbon paper.
2. The method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst according to claim 1, characterized in that: The mixed solution in the beaker in S1 is a mixture of 15 mL of deionized water and 15 mL of anhydrous ethanol, and the stirring time is 10-15 min.
3. The method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst according to claim 1, characterized in that: The specific operation in S2 includes placing the reactor in an oven for hydrothermal reaction, maintaining it at 100°C for 10 hours, and after the reaction is completed and naturally cooled to room temperature, taking out the reactor to obtain a solid-liquid phase mixture, washing it with deionized water for 3-5 times, and finally drying it at 60°C in a vacuum environment for 8-12 hours to obtain a solid powder B.
4. The method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst according to claim 1, characterized in that: The grinding time in S3 is 5-10 minutes, and the annealing conditions in the tube furnace are: air atmosphere at a temperature of 350° C. and annealing time of 2 hours.
5. The method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst according to claim 1, characterized in that: The specific operation in S4 is: weigh 50 mg of solid powder C and place it in a ceramic ark 1; Weigh 500-2000 mg of NaH2PO2·H2O and place it in Ceramic Ark 2; Ceramic ark one is placed downstream of the air flow of the tubular furnace, and ceramic ark two is placed upstream of the air flow of the tubular furnace. The distance between ceramic ark one and ceramic ark two is 2-4 cm. Annealing is carried out in an argon atmosphere at 350°C in the tubular furnace for 2 hours to obtain pre-catalyst CoPxNR, i.e., cobalt phosphide nanorods.
6. The method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst according to claim 5, characterized in that: The specific operation in S5 is: weighing 5 mg of pre-catalyst solid powder and dispersing it in a mixture of 30 μL of Nafion solution, 250 μL of deionized water and 750 μL of anhydrous ethanol in a centrifuge tube, and ultrasonicating at room temperature for 1-2 hours to obtain a pre-catalyst slurry; Under the infrared lamp, use a pipette to take a total of 200 μL of slurry in small amounts and multiple times and evenly apply it on one side to 1 cm 2 on hydrophilic carbon paper.
7. The method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst according to claim 6, characterized in that: The specific operation in S6 is: using the prepared pre-catalyst loaded carbon paper as the working electrode, the carbon rod as the counter electrode, Hg|HgO as the reference electrode, and 1M KOH as the electrolyte to form a typical three-electrode system, and applying 10 mA cm-1 by using an electrochemical workstation using a chronopotentiometry. -2 The pre-catalyst supported on the carbon paper was oxidized for 10 h with a current of 1.5 %. The oxidized carbon paper was washed with deionized water for 3-5 times, and dried at 60° C. in a vacuum environment for 8-12 hours to obtain an oxygen evolution reaction catalyst CoOOHxNS, i.e., cobalt oxyhydroxide nanosheets, on the carbon paper.
8. The method for preparing a cobalt-based lattice strain oxygen evolution reaction catalyst according to claim 1, characterized in that: The preparation method requires the following raw material mass ratios for preparing the cobalt-based lattice strain oxygen evolution reaction catalyst: 163.7-164 mg of Co(NO3)2·6H2O, 135-135.2 mg of CO(NH2)2, and 500-2000 mg of NaH2PO2·H2O.
Citation Information
Patent Citations
Preparation method of polyhedral cobalt phosphide catalyst for hydrogen production through water electrolysis
CN105107536A
Preparation method and application of vanadium carbide-loaded CoP microsphere three-function catalytic material
CN111437853A
Cited By
Method for measuring ash content of high-purity graphite by using ceramic ark
CN120820399A