Cerium dioxide loaded iridium-based alloy catalyst as well as preparation method and application thereof

By uniformly dispersing the Ir-based alloy on the ceria support, the problem of corrosion of Pt-based catalysts under high current density is solved, and an efficient and stable acidic water electrolytic catalyst is achieved, which reduces the use of precious metals and the preparation cost, and promotes the The industrialization of electrolytic water.

CN118957645APending Publication Date: 2024-11-15HAINAN DEEP SEA NEW ENERGY TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411065281.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, Pt-based catalysts are prone to corrosion under high current density, which hinders its promotion in PEM electrolytic cells. The preparation of supported catalysts requires a strong acid or strong alkali solution, which has safety risks, high energy consumption, and catalyst size. Uncontrollable and difficult to achieve uniformity.

Method used

By using the strong interaction between metal and support, the Ir-based alloy is uniformly dispersed on the ceria support to prepare a ceria-supported iridium-based alloy catalyst. The oil-bath reaction and hydrothermal reaction methods are used, and the Ir-based alloy is realized by combining the calcination step. High dispersion and dimensional control.

Benefits of technology

A catalyst with good electrochemical activity and high stability in acidic electrolytic water is realized, which reduces the load of precious metals, reduces the cost, and promotes the development of the industrialization of electrolytic water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957645A_ABST
    Figure CN118957645A_ABST
Patent Text Reader

Abstract

The invention provides a cerium dioxide loaded iridium-based alloy catalyst as well as a preparation method and application thereof, and belongs to the field of hydrogen production by acidic electrolysis of water. The preparation method comprises the following steps: (1) carrying out oil bath reaction on iridium trichloride and another metal chloride in a solution containing polyvinylpyrrolidone and ethylene glycol to obtain a solution A; (2) putting cerium trichloride, sodium hydroxide and sodium chloride into water, mixing, carrying out hydrothermal reaction, and centrifuging to obtain a precursor B; (3) adding the precursor B into the solution A, stirring and centrifuging to obtain a precursor C; and (4) calcining the precursor C to obtain the cerium dioxide loaded iridium-based alloy catalyst. The size of the prepared iridium-based alloy is about 2.5-3.5 nm. Dispersion of metal active sites is improved through a carrier loading process, the loading amount of precious metal is reduced, and the prepared catalyst shows excellent electrochemical performance in an acidic hydrogen evolution reaction and can be well applied to acidic hydrogen production through water electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts for hydrogen production by electrolysis of water, and in particular to a cerium dioxide-supported iridium-based alloy catalyst and a preparation method and application thereof. Background Art

[0002] Hydrogen energy is a promising sustainable energy source in the future, and water electrolysis is the most scalable technology for producing green hydrogen. The hydrogen evolution reaction (HER) during electrolysis is closely related to the pH value of the electrolyte, and acidic solutions are conducive to the production of hydrogen. Currently, Pt-based catalysts are considered to be the best catalysts for HER, but they are prone to corrosion at high current densities, which hinders their promotion in PEM electrolyzers. Developing catalysts with good activity and stability at high current density is crucial for hydrogen production using proton exchange membrane electrolyzers.

[0003] Iridium-based nanomaterials have become promising acidic HER electrocatalysts due to their intrinsic activity and corrosion resistance similar to Pt. However, the high price of Ir limits its use in PEM electrolyzers. Therefore, it is particularly important to reduce the loading of Ir metal while ensuring activity. Alloying has attracted attention as an effective strategy to improve catalyst and stability. At the same time, the strong interaction between metal and support can effectively reduce the metal agglomeration caused by high temperature, which can not only achieve good dispersion but also further reduce the loading of precious metals.

[0004] In the existing technology, the preparation of supported catalysts requires the use of strong acid or strong base solutions, which poses certain safety risks. The reaction process also requires high temperatures (600-900°C), which consumes a lot of energy. In addition, the size of the catalysts prepared by most technical processes is uncontrollable, making it difficult to achieve uniformity. Summary of the invention

[0005] In view of this, the purpose of the present invention is to propose a ceria-supported iridium-based alloy catalyst and its preparation method and application, and utilize the strong interaction between metal and carrier to uniformly disperse the Ir-based alloy on the ceria carrier to prepare a series of ceria-supported iridium-based alloy catalysts, and apply them to acidic HER. The preparation method has certain application prospects for electrocatalysis and has important research significance for promoting the industrialization process of low-loaded precious metals in electrolyzed water.

[0006] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:

[0007] A method for preparing a ceria-supported iridium-based alloy catalyst comprises the following steps:

[0008] (1) conducting an oil bath reaction with iridium trichloride and another metal chloride in a solution containing polyvinyl pyrrolidone and ethylene glycol to obtain a solution A;

[0009] (2) placing cerium trichloride, sodium hydroxide and sodium chloride in ultrapure water, mixing, hydrothermally reacting, and centrifuging to obtain precursor B;

[0010] (3) adding the precursor B from step (2) to the solution A from step (1), stirring, and centrifuging to obtain a precursor C;

[0011] (4) Calcining the precursor C in step (3) to obtain a cerium dioxide-supported Ir-based alloy catalyst.

[0012] A further technical solution is that the another metal chloride includes one or more of ruthenium chloride, cobalt chloride, nickel chloride, manganese chloride, and ferric chloride, but is not limited to the above metal chlorides.

[0013] A further technical solution is that in step (1), the molar ratio of iridium trichloride to another metal compound is 3.5-4.5:0.8-1.2; the solid-liquid ratio of iridium trichloride to polyvinyl pyrrolidone and ethylene glycol is 0.06-0.1mM:30-50mg:25-40mL.

[0014] A further technical solution is that in step (1), the temperature of the oil bath reaction is 150-200° C., and the insulation time is 2-8 hours.

[0015] A further technical solution is that in step (2), the molar ratio of the cerium trichloride, sodium hydroxide and sodium chloride is 1.3-1.6:0.1-0.2:0.1-0.2; and the molar volume of the total amount of the cerium trichloride, sodium hydroxide and sodium chloride to ultrapure water is 1.5-1.8mM:20-50ml.

[0016] A further technical solution is that in step (2), the temperature of the hydrothermal reaction is 160-200° C. and the insulation time is 12-36 hours.

[0017] A further technical solution is that in step (3), the stirring temperature is 15-30°C and the stirring time is 12-36h; in steps (2) and (3), the centrifugal speed is 5000-10000rpm and the centrifugal time is 3-10min.

[0018] A further technical solution is that in step (3), the molar mass ratio of iridium trichloride to precursor B in the solution A raw material is 0.06-0.1mM:90-110mg.

[0019] A further technical solution is that the specific operation of step (4) is: the precursor C is calcined in an inert atmosphere, the calcination temperature is 200-500°C, the heating rate is 2-10°C / min, and the insulation time is 60-180min.

[0020] A ceria-supported iridium-based alloy catalyst is prepared by any preparation method described in the present invention.

[0021] The invention discloses an application of the cerium dioxide-supported iridium-based alloy catalyst prepared by the invention in the production of hydrogen by acidic water electrolysis.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The present invention provides a cerium dioxide-supported iridium-based alloy catalyst and a preparation method and application thereof. The method utilizes the strong interaction between metal carriers to simply achieve high dispersion of a series of Ir-based alloy catalysts, and can effectively reduce the precious metal loading and reduce costs. The preparation method of the present invention has a simple process, convenient operation, low cost, good electrochemical activity and high stability. The catalyst prepared by the present invention is suitable for acidic water electrolysis, and can show relatively excellent electrochemical performance in the HER reaction, and can be used in the production of hydrogen by acidic water electrolysis, thereby promoting the industrial development of water electrolysis.

[0024] (2) The size of the cerium dioxide-supported iridium-based alloy prepared by the present invention is about 2.5-3.5 nm. The present invention improves the dispersion of metal active sites and reduces the loading of precious metals through the carrier loading process. The prepared catalyst exhibits excellent electrochemical performance in the acidic hydrogen evolution reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The XRD pattern of the ceria-supported IrRu alloy catalyst (IrRu / CeO2) prepared in Example 1; Figure 1 PDF#65-5546 and PDF#65-2975 represent the standard cards of the corresponding catalysts, which can distinguish the composition of the catalysts.

[0026] Figure 2 This is the TEM image of the cerium dioxide supported IrRu based alloy catalyst (IrRu / CeO2) prepared in Example 1.

[0027] Figure 3 This is the HER polarization curve of the ceria-loaded IrRu-based alloy catalyst (IrRu / CeO2) prepared in Example 1 in 0.5MH2SO4.

[0028] Figure 4 This is a stability diagram of the ceria-supported IrRu-based alloy catalyst (IrRu / CeO2) prepared in Example 1 in 0.5MH2SO4.

[0029] Figure 5This is the HER polarization curve of the cerium dioxide-loaded IrRu-based alloy catalyst (IrRu / CeO2) in 0.5M H2SO4 prepared by regulating the metal precursor in Comparative Example 1.

[0030] Figure 6 This is the HER polarization curve of the cerium dioxide-loaded IrRu-based alloy catalyst (IrRu / CeO2) prepared by hydrothermal reaction conditions in Comparative Example 2 in 0.5M H2SO4.

[0031] Figure 7 This is the HER polarization curve of the cerium dioxide-loaded IrRu-based alloy catalyst (IrRu / CeO2) in 0.5M H2SO4 prepared by changing the stirring conditions in Comparative Example 3.

[0032] Figure 8 This is the HER polarization curve of the cerium dioxide-loaded IrRu-based alloy catalyst (IrRu / CeO2) in 0.5M H2SO4 prepared by changing the calcination conditions in Comparative Example 4. DETAILED DESCRIPTION

[0033] In order to explain the present invention more clearly, the present invention is further described in detail below in conjunction with embodiments and with reference to the accompanying drawings. It should be understood by those skilled in the art that the content described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0034] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0035] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0036] Example 1 - Preparation of Ceria-supported IrRu Alloy Catalyst (IrRu / CeO2)

[0037] (1) Preparation of solution A: Ruthenium trichloride (0.02 mM), iridium trichloride (0.08 mM) and polyvinyl pyrrolidone (40 mg) were placed in a three-necked flask containing 30 mL of ethylene glycol, and then kept in an oil bath at 200° C. for 4 h and cooled to obtain solution A.

[0038] (2) Preparation of Precursor B: Ce trichloride (1.5 mM), sodium hydroxide (0.18 M) and sodium chloride (0.018 mM) were placed in a polytetrafluoroethylene reactor lined with 40 mL of ultrapure water. The hydrothermal reaction temperature was 180°C, the insulation time was 24 h, the centrifugal speed was 8000 rpm, the time was 3 min, and the precursor was dried in a vacuum oven to obtain Precursor B.

[0039] (3) Preparation of Precursor C: The entire solution of Solution A was mixed with Precursor B (100 mg) and stirred at a stirring temperature of 25° C. for 24 h, a centrifugal speed of 8000 rpm, and a centrifugal time of 5 min to obtain Precursor C.

[0040] (4) Preparation of ceria-supported IrRu alloy catalyst: Precursor C (50 mg) was calcined in an inert atmosphere in a tubular furnace to obtain a ceria-supported IrRu alloy catalyst; the tubular furnace temperature was 400°C, the heating rate was 5°C / min, and the holding time was 60 min.

[0041] The structure and electrochemical performance of the ceria-supported IrRu alloy catalyst of Example 1 are as follows:

[0042] (A) Structural morphology and elemental characterization of the catalyst

[0043] X-ray diffraction was used to characterize the elemental composition of the ceria-supported IrRu alloy catalyst ( Figure 1 ).from Figure 1 It can be seen that the material prepared in Example 1 corresponds to the standard card, which further confirms that the catalyst is IrRu / CeO2.

[0044] The morphology of the ceria-supported IrRu alloy catalyst can be seen by field emission transmission electron microscopy (TEM). Figure 2 ). It can be seen that CeO2 is a nanorod-like structure, and the particles loaded on its surface are IrRu alloy, which is evenly distributed. Figure 2 The inset in a shows the particle size of IrRu alloy in IrRu / CeO2. The particle size of IrRu alloy is about 2.5-3.5nm.

[0045] (B) Cathode hydrogen evolution performance test

[0046] A linear scan test was performed using a three-electrode system in 0.5 M H2SO4 at a scan rate of 5 mV / s.

[0047] In Example 1, Figure 3 The polarization curves show that the IrRu / CeO2 catalyst has a -2 The overpotential at a current density of 32 mV is close to that of Pt / C catalyst (26 mV).

[0048] The catalyst prepared in Example 1 exhibits hydrogen evolution performance close to that of Pt / C catalyst ( Figure 3 ).

[0049] The catalyst prepared in Example 1 exhibited excellent stability ( Figure 4). It can be seen that the IrRu / CeO2 catalyst can -2 It ran for more than 200 h at a current density of 1.5 Å, showing excellent stability.

[0050] Unless otherwise specified, the test method for cathode hydrogen evolution of the catalyst involved in the present invention is the same as the above test method.

[0051] Example 2 - Preparation of Ceria-supported IrCo Alloy Catalyst (IrCo / CeO2)

[0052] (1) Preparation of Solution A: Cobalt chloride (0.015 mM), iridium trichloride (0.06 mM) and polyvinyl pyrrolidone (30 mg) were placed in a three-necked flask containing 25 mL of ethylene glycol, and then kept in an oil bath at 200° C. for 4 h and cooled to obtain Solution A.

[0053] (2) Preparation of Precursor B: Ce trichloride (1.5 mM), sodium hydroxide (0.18 M) and sodium chloride (0.018 mM) were placed in a polytetrafluoroethylene-lined reactor containing 40 mL of ultrapure water. The hydrothermal reaction temperature was 180 °C, the insulation time was 24 h, the centrifugal speed was 8000 rpm, the time was 3 min, and the product was dried in a vacuum oven.

[0054] (3) Preparation of Precursor C: Solution A and Precursor B (100 mg) were mixed and stirred at a stirring temperature of 25° C. for 24 h, a centrifugal speed of 8000 rpm, and a centrifugal time of 5 min to obtain Precursor C.

[0055] (4) Preparation of ceria-supported IrCo alloy catalyst: Precursor C (50 mg) was calcined in an inert atmosphere in a tubular furnace to obtain a ceria-supported IrCo alloy catalyst; the tubular furnace temperature was 400°C, the heating rate was 5°C / min, and the holding time was 60 min.

[0056] Example 3 - Preparation of Ceria-supported IrNi Alloy Catalyst (IrNi / CeO2)

[0057] (1) Preparation of Solution A: Nickel chloride (0.025 mM), iridium trichloride (0.1 mM) and polyvinyl pyrrolidone (50 mg) were placed in a three-necked flask containing 40 mL of ethylene glycol, and then kept in an oil bath at 200° C. for 4 h and cooled to obtain Solution A.

[0058] (2) Preparation of Precursor B: Ce trichloride (1.5 mM), sodium hydroxide (0.18 M) and sodium chloride (0.018 mM) were placed in a polytetrafluoroethylene-lined reactor containing 40 mL of ultrapure water. The hydrothermal reaction temperature was 180 °C, the insulation time was 24 h, the centrifugal speed was 8000 rpm, the time was 3 min, and the product was dried in a vacuum oven.

[0059] (3) Preparation of Precursor C: Solution A and Precursor B (100 mg) were mixed and stirred at a stirring temperature of 25° C. for 24 h, a centrifugal speed of 8000 rpm, and a centrifugal time of 5 min to obtain Precursor C.

[0060] (4) Preparation of ceria-supported IrNi alloy catalyst: Precursor C (50 mg) was calcined in an inert atmosphere in a tubular furnace to obtain a ceria-supported IrNi alloy catalyst; the tubular furnace temperature was 400°C, the heating rate was 5°C / min, and the holding time was 60 min.

[0061] The hydrogen evolution performance test results of Examples 2 and 3 are substantially consistent with those of Example 1.

[0062] In other embodiments,

[0063] Step (1), hydrothermal reaction temperature 150-200°C, insulation time 2-8h;

[0064] Step (2), hydrothermal reaction temperature 160-200°C, insulation time 12-36h;

[0065] In steps (2) and (3), the centrifugal speed is 5000-10000 rpm and the centrifugal time is 3-10 min;

[0066] Step (4), the temperature of the tube furnace is 200-500°C, the heating rate is 2-10°C / min, and the holding time is 60-180min;

[0067] By adjusting the process within the above range, the purpose of the present invention can also be achieved.

[0068] Comparative Example 1

[0069] The main difference between Example 1 and Solution A is that ruthenium trichloride is replaced by ruthenium acetate, and iridium trichloride is replaced by iridium acetate. Specifically: (1) Preparation of Solution A: Ruthenium acetate (0.02 mM), iridium acetate (0.08 mM) and polyvinyl pyrrolidone (40 mg) are placed in a three-necked flask containing 30 mL of ethylene glycol, and then kept in an oil bath at 200°C for 4 h, and cooled to obtain Solution A. Other operations are consistent with Example 1. The results are shown in FIG. Figure 5 As shown, the hydrogen evolution performance test results of the material prepared in this comparative example are significantly reduced.

[0070] Comparative Example 2

[0071] The main difference between Example 1 and Precursor B is that the hydrothermal reaction temperature is adjusted to 100°C and the insulation time is 16h. Specifically, cerium trichloride (1.5mM), sodium hydroxide (0.18M) and sodium chloride (0.018mM) are placed in a polytetrafluoroethylene reactor lined with 40mL ultrapure water, the hydrothermal reaction temperature is 100°C, the insulation time is 16h, the centrifugal speed is 8000rpm, the time is 3min, and the precursor B is dried in a vacuum oven to obtain the precursor B. The other operations are consistent with Example 1. The results are shown in FIG. Figure 6 As shown, the hydrogen evolution performance test results of the material prepared in this comparative example are significantly reduced.

[0072] Comparative Example 3

[0073] The main difference between Example 1 and the preparation of precursor C is that the stirring temperature is 40°C. Specifically, solution A and precursor B (100 mg) are mixed and stirred at a stirring temperature of 25°C for 24 hours, a centrifugal speed of 8000 rpm, and a centrifugal time of 5 minutes to obtain precursor C. Other operations are consistent with Example 1. The results are shown in FIG. Figure 7 As shown, the hydrogen evolution performance test results of the material prepared in this comparative example are significantly reduced.

[0074] Comparative Example 4

[0075] The main difference between the preparation of the cerium oxide supported IrRu alloy catalyst and the calcination temperature is 600°C. Specifically, the precursor C (50 mg) is placed in a tube furnace in an inert atmosphere and calcined to obtain the cerium oxide supported IrRu alloy catalyst; wherein the tube furnace temperature is 400°C, the heating rate is 5°C / min, and the holding time is 60min. The other operations are consistent with those of Example 1. The results are shown in FIG. Figure 8 As shown, the hydrogen evolution performance of the material prepared in this comparative example is greatly reduced.

[0076] Obviously, the above embodiments of the present invention are merely examples to more clearly illustrate the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing a ceria-supported iridium-based alloy catalyst, characterized in that: The following steps are involved: (1) conducting an oil bath reaction with iridium trichloride and another metal chloride in a solution containing polyvinyl pyrrolidone and ethylene glycol to obtain a solution A; (2) adding cerium trichloride, sodium hydroxide and sodium chloride into water, mixing, hydrothermally reacting, and centrifuging to obtain precursor B; (3) adding precursor B to solution A in step (1), stirring, and centrifuging to obtain precursor C; (4) Calcinate the precursor C to obtain a cerium dioxide-supported Ir-based alloy catalyst.

2. The preparation method according to claim 1, characterized in that: In step (1), the molar ratio of iridium trichloride to another metal compound is 3.5-4.5:0.8-1.2; the solid-liquid ratio of iridium trichloride to polyvinyl pyrrolidone and ethylene glycol is 0.06-0.1 mM:30-50 mg:25-40 mL.

3. The preparation method according to claim 1 or 2, characterized in that: In step (1), the temperature of the oil bath reaction is 150-200° C., and the insulation time is 2-8 hours.

4. The preparation method according to claim 1, characterized in that: In step (2), the molar ratio of cerium trichloride, sodium hydroxide and sodium chloride is 1.3-1.6:0.1-0.2:0.1-0.2; and the molar volume ratio of the total amount of cerium trichloride, sodium hydroxide and sodium chloride to water is 1.5-1.8 mM:20-50 ml.

5. The preparation method according to claim 1 or 4, characterized in that: In step (2), the temperature of the hydrothermal reaction is 160-200° C., and the insulation time is 12-36 hours.

6. The preparation method according to claim 1, characterized in that: In step (3), the stirring temperature is 15-30° C. and the stirring time is 12-36 h. In steps (2) and (3), the centrifugal speed is 5000-10000 rpm and the centrifugal time is 3-10 min.

7. The preparation method according to claim 1 or 6, characterized in that: In step (3), the molar mass ratio of iridium trichloride to precursor B in the solution A raw material is 0.06-0.1 mM:90-110 mg.

8. The preparation method according to claim 1, characterized in that: The specific operation of step (4) is as follows: the precursor C is calcined in an inert atmosphere, the calcination temperature is 200-500° C., the heating rate is 2-10° C. / min, and the insulation time is 60-180 min.

9. A ceria-supported iridium-based alloy catalyst, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the cerium dioxide-supported iridium-based alloy catalyst according to claim 9 in producing hydrogen by acidic water electrolysis.

Citation Information

Cited By

  • High-activity supported IrOx / CeO2 catalyst as well as preparation method and application thereof

    CN119465281A

  • Preparation method of platinum-based alloy rare earth metal oxide fuel cell anode catalyst

    CN120473518A