Preparation method of powder material for electro-catalytic water decomposition oxygen evolution half reaction
Through the preparation of ZnO@NiFeLDH powder material, the scarcity and high cost of existing OER catalysts are solved, and low-cost and efficient electrocatalytic decomposition of water oxygen analysis reaction is achieved, with higher application prospects and efficiency.
Patent Information
- Application Number
- CN202410786775.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-15
AI Technical Summary
Existing OER catalysts are generally scarce, have insufficient reserves and are not efficient in catalytic decomposition rates, which limit their application in the electrolytic process.
ZnO@NiFeLDH powder material was used as a catalyst and prepared by solvothermal method. The reaction conditions were controlled to obtain efficient OER catalysts using zinc oxide suspension and soluble nickel, iron salts and other materials.
Low-cost and low-potential OER catalysis is achieved, production costs are reduced, and the application prospects and efficiency of catalysts are improved, which has higher application value than precious metal catalysts.
Smart Images

Figure CN118957648A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical catalyst preparation, and in particular relates to a method for preparing a powder material for electrocatalytic water decomposition and oxygen evolution half-reaction. Background Art
[0002] Due to the scarcity of earth resources, the development of hydrogen energy is imminent. Hydrogen production by water electrolysis is one of the most promising ways to solve the imminent energy crisis and environmental problems.
[0003] In the process of water electrolysis, oxygen and hydrogen are produced through the oxygen evolution reaction (OER) at the anode and the hydrogen evolution reaction (HER) at the cathode. Among them, the OER reaction, as a half-reaction of water decomposition, has a high overpotential due to the existence of four coupled proton-electron transfer steps between the intermediates (OH*, O*, OOH*) adsorbed on the surface.
[0004] At present, most of the most advanced OER catalysts are precious metals such as iridium and ruthenium and their oxides, which can show good catalytic performance in both acidic and alkaline solutions. However, their scarcity and high cost limit their practical application. Therefore, it is urgent to develop a low-cost, earth-abundant and efficient OER non-precious metal catalyst. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention provides a method for preparing a powder material for the electrocatalytic decomposition of water and oxygen evolution half-reaction, aiming to solve the technical problems in the prior art that OER catalysts are generally scarce, have insufficient reserves, and have an inefficient catalytic decomposition rate.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a powder material for electrocatalytic water decomposition oxygen evolution half reaction, the catalyst is used as a catalyst for the oxygen evolution half reaction in the water decomposition reaction, the catalyst is a ZnO@NiFeLDH material, the catalyst is a powder material, and the preparation method thereof comprises the following steps:
[0007] Step 1: Weigh a certain amount of zinc acetate and dissolve it in alcohol to form a uniform solution;
[0008] Wherein, the alcohol is anhydrous methanol or anhydrous ethanol; and the concentration of the alcohol solution of zinc acetate is 0.01-0.05M;
[0009] Step 2: stirring the obtained alcohol solution of zinc acetate at high temperature to obtain a zinc oxide suspension;
[0010] Wherein, the stirring temperature is 60°C, the stirring speed is 500-700r / min, and the stirring time is 60-120min;
[0011] Step 3, weighing the chemicals required for solvent heat, selecting soluble nickel salt and soluble iron salt as metal sources, urea as pH adjuster, and ammonium fluoride as surfactant;
[0012] The molar ratio of soluble nickel salt to soluble iron salt in the metal source is 3:1, and the feed concentrations are 0.006-0.09M for nickel salt and 0.002-0.03M for iron salt respectively; meanwhile, the urea concentration is 1.59-3.39g / 100ml, and the ammonium fluoride concentration is 0.18-0.25g / 100ml.
[0013] Step 4: Add the medicine weighed in step 3 to the zinc oxide suspension and stir evenly;
[0014] Among them, before the drugs are added, the zinc oxide suspension needs to be cooled to 30 degrees Celsius; and the order of adding the drugs is soluble nickel salt, soluble iron salt, and after stirring for 1 hour, urea and ammonium fluoride are added.
[0015] Step 5, transferring the solution obtained in step 4 to a corrosion-resistant lining (generally preferably a polytetrafluoroethylene lining), and placing it in a stainless steel autoclave for a solvothermal reaction;
[0016] The reactor can be selected in the specifications of 50ml and 100ml; the solvent thermal reaction temperature can be selected in the range of 120-160 degrees Celsius, and the reaction time can be selected in the range of 8-16h.
[0017] Step 6: Collect the powder material in step 5, clean it, and dry it for later use.
[0018] Among them, the drying temperature is 60 degrees Celsius and the drying time is 8-10 hours.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. In the prior art, most OER catalysts are precious metals such as iridium and ruthenium and their oxides. Such catalysts can exhibit good catalytic performance in both acidic and alkaline solutions. However, their scarcity and high cost limit their practical application. Therefore, there is an urgent need to develop a low-cost, earth-rich and efficient OER non-precious metal catalyst. In the present invention, a ZnO suspension is used to promote nucleation growth to obtain a powder material of uniform size for electrocatalytic water decomposition OER reaction, namely, ZnO@NiFeLDH powder material. The material has good controllability, mild reaction conditions, and is environmentally friendly. In the OER reaction, under the condition of ensuring efficient and mild reaction conditions, it also has the characteristics of low cost and abundant earth resources. Compared with more expensive precious metals such as iridium and ruthenium and their oxide catalysts, it has higher application value and application prospects.
[0021] 2. In the present invention, the prepared ZnO@NiFeLDH powder material has high OER catalytic activity at a current density of 10 mA / cm 2 The potential at the time of reaction is only 1.57V. Under the premise of low raw material price and abundant resource reserves, it has better application prospects compared with precious metal oxide catalysts such as RuO2 and IrO2.
[0022] 3. In the present invention, the amount of NiFe used in the raw material preparation process can be effectively reduced, and the production cost of the catalyst for the electrocatalytic water decomposition and oxygen evolution half-reaction can be effectively reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0024] Figure 1 This is a flow chart of preparing ZnO@NiFeLDH in the present invention;
[0025] Figure 2 This is the XRD diffraction pattern of ZnO@NiFeLDH prepared in Example 1 of the present invention;
[0026] Figure 3 This is a scan of the ZnO@NiFeLDH prepared in Example 1 of the present invention;
[0027] Figure 4 This is a linear voltammetric scan of ZnO@NiFeLDH prepared in Example 1 of the present invention;
[0028] Figure 5 This is the XRD diffraction pattern of ZnO@NiFeLDH prepared in Example 2 of the present invention;
[0029] Figure 6 This is a scan of the ZnO@NiFeLDH prepared in Example 2 of the present invention;
[0030] Figure 7 This is the linear voltammetric scan of ZnO@NiFeLDH prepared in Example 2 of the present invention;
[0031] Figure 8 XRD diffraction pattern of NiFeLDH prepared in Comparative Example 1;
[0032] Fig. 9 The linear voltammetric scan diagram of NiFeLDH prepared in Comparative Example 1;
[0033] Fig.10 This is the linear voltammetric scan diagram of ZnO@NiFeLDH prepared in Comparative Example 2. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Unless otherwise specified, all raw materials used in the embodiments of the present invention are commercially available.
[0036] Embodiment 1:
[0037] In this embodiment, the required raw materials are: nickel chloride hexahydrate, ferric chloride hexahydrate, zinc acetate, anhydrous methanol, ammonium fluoride, and urea.
[0038] In this embodiment, see Figure 1 , discloses a method for preparing a powder material for electrocatalytic water decomposition oxygen evolution half reaction, the catalyst is used as a catalyst for the oxygen evolution half reaction in the water decomposition reaction, the catalyst is a ZnO@NiFeLDH material, the catalyst is a powder material, and the preparation method thereof comprises the following steps:
[0039] Step 1: Weigh 0.03 mol of zinc acetate and dissolve it in 100 ml of anhydrous methanol to form a uniform solution;
[0040] Step 2: stirring the obtained zinc acetate methanol solution at 60° C. at a speed of 600 r / min for 1 h to obtain a zinc oxide suspension;
[0041] Step 3, weigh the chemicals required for solvothermal reaction, 0.09M NiCl2·6H2O, 0.03M FeCl3·6H2O, 1.59g urea and 0.22g ammonium fluoride;
[0042] Step 4: Add the drugs weighed in step 3 to the zinc oxide suspension restored to room temperature in order and stir evenly. The order of adding the drugs is nickel chloride hexahydrate and ferric chloride hexahydrate. After stirring for 1 hour, continue to add urea and ammonium fluoride.
[0043] Step 5: Transfer the solution obtained in step 4 to a 50 ml polytetrafluoroethylene liner and place it in a stainless steel autoclave for solvothermal reaction at a reaction temperature of 120° C. for 8 h.
[0044] Step 6: Collect the powder material in step 5, clean it, and dry it at 60 degrees Celsius for 8 hours before use.
[0045] The ZnO@NiFeLDH of this embodiment is used as the working electrode in the electrocatalytic oxygen evolution reaction. Specifically, a mercury / mercury oxide electrode and a platinum wire electrode are selected as the reference electrode and the counter electrode, respectively; 5 mg of ZnO@NiFeLDH catalyst is weighed and dispersed into 1 mL of a mixed solution, wherein the solution includes: 0.5 mL of water, 0.5 mL of ethanol, and 20 μL of naphthol solution. The above solution is ultrasonicated for 30 minutes to obtain a slurry, which is evenly coated on a 1 cm 2 The working electrode was obtained by drying and pressing the nickel foam. The electrocatalytic oxygen evolution test used 1 mol / L KOH solution as the electrolyte and the scanning rate was 2 mV s -1 .
[0046] The results obtained:
[0047] (1) Figure 2 The XRD diffraction pattern of ZnO@NiFeLDH shows that the main component of ZnO@NiFeLDH is NiFe LDH;
[0048] (2) Figure 3 The SEM image of ZnO@NiFeLDH shows that ZnO@NiFeLDH is a ball assembled from nanosheets.
[0049] (3) Figure 4 The LSV diagram of ZnO@NiFeLDH shows that ZnO@NiFeLDH has a high 2 The required voltage is 1.57V.
[0050] Therefore, it can be concluded from this embodiment that the ZnO@NiFeLDH prepared in this embodiment has the characteristics of uniform size and low oxygen evolution potential, and it has good controllability in the electrocatalytic oxygen evolution reaction, mild reaction conditions, and is relatively environmentally friendly.
[0051] Embodiment 2:
[0052] In this embodiment, the required raw materials are: nickel chloride hexahydrate, ferric chloride hexahydrate, zinc acetate, anhydrous ethanol, ammonium fluoride, and urea.
[0053] This embodiment provides another method for preparing ZnO@NiFeLDH powder material for electrocatalytic water decomposition and oxygen evolution half-reaction. The anhydrous methanol in Example 1 is replaced with anhydrous ethanol to prepare the material. The preparation method comprises the following steps:
[0054] Step 1: Weigh 0.03 mol zinc acetate and dissolve it in 100 ml anhydrous ethanol to form a uniform solution;
[0055] Step 2: stirring the obtained zinc acetate ethanol solution at 60° C. at a speed of 600 r / min for 1 h to obtain a zinc oxide suspension;
[0056] Step 3, weigh the chemicals required for solvothermal reaction, 0.09M NiCl2·6H2O, 0.03M FeCl3·6H2O, 1.59g urea and 0.22g ammonium fluoride;
[0057] Step 4: Add the drugs weighed in step 3 to the zinc oxide suspension restored to room temperature in order and stir evenly. The order of adding the drugs is nickel chloride hexahydrate and ferric chloride hexahydrate. After stirring for 1 hour, continue to add urea and ammonium fluoride.
[0058] Step 5: Transfer the solution obtained in step 4 to a 50 ml polytetrafluoroethylene liner and place it in a stainless steel autoclave for solvothermal reaction at a reaction temperature of 120° C. for 8 h.
[0059] Step 6: Collect the powder material in step 5, clean it, and dry it at 60 degrees Celsius for 8 hours before use.
[0060] The ZnO@NiFeLDH of this embodiment is used as the working electrode in the electrocatalytic oxygen evolution reaction. Specifically, a mercury / mercury oxide electrode and a platinum wire electrode are selected as the reference electrode and the counter electrode, respectively; 5 mg of ZnO@NiFeLDH catalyst is weighed and dispersed into 1 mL of a mixed solution, wherein the solution includes: 0.5 mL of water, 0.5 mL of ethanol, and 20 μL of naphthol solution. The above solution is ultrasonicated for 30 minutes to obtain a slurry, which is evenly coated on a 1 cm 2 The working electrode was obtained by drying and pressing the nickel foam. The electrocatalytic oxygen evolution test used 1 mol / L KOH solution as the electrolyte and the scanning rate was 2 mV s -1 .
[0061] The results obtained:
[0062] (1) Figure 5 This is the XRD diffraction pattern of ZnO@NiFeLDH. It can be seen from the figure that the main component of ZnO@NiFeLDH is NiFe LDH.
[0063] (2) Figure 6 This is the SEM image of ZnO@NiFeLDH. It can be seen from the figure that ZnO@NiFeLDH is a sphere assembled from nanosheets.
[0064] (3) Figure 7 The LSV diagram of ZnO@NiFeLDH shows that ZnO@NiFeLDH has a 2 The required voltage is 1.57V.
[0065] It can be seen from this embodiment that the use of anhydrous methanol or anhydrous ethanol as the reaction solution will not affect the excellent properties of the ZnO@NiFeLDH powder material, nor will it change the characteristics of the material having uniform size and low oxygen evolution potential.
[0066] Comparative Example 1:
[0067] In this comparative example, the required raw materials are: nickel chloride hexahydrate, ferric chloride hexahydrate, anhydrous methanol, ammonium fluoride, and urea.
[0068] This comparative example provides a third method for preparing a powder material for electrocatalytic water decomposition and oxygen evolution half-reaction. The catalyst prepared in this comparative example is NiFeLDH, and its preparation method comprises the following steps:
[0069] Step 1: Weigh the chemicals required for solvent thermal, 0.09M NiCl2·6H2O, 0.03M FeCl3·6H2O, 1.59g urea and 0.22g ammonium fluoride;
[0070] Step 2: Add the drugs weighed in step 1 to the methanol solution at room temperature in order and stir evenly. The order of adding the drugs is nickel chloride hexahydrate and ferric chloride hexahydrate. After stirring for 1 hour, continue to add urea and ammonium fluoride;
[0071] Step 3: Transfer the solution obtained in step 2 to a 50 ml polytetrafluoroethylene liner and place it in a stainless steel autoclave for solvothermal reaction at a reaction temperature of 120° C. for 8 h;
[0072] Step 4: Collect the powder material in step 3, clean it, and dry it at 60 degrees Celsius for 8 hours before use.
[0073] The NiFeLDH of this comparative example is used as the working electrode in the electrocatalytic oxygen evolution reaction. Specifically, a mercury / mercury oxide electrode and a platinum wire electrode are selected as the reference electrode and the counter electrode, respectively; 5 mg of NiFeLDH catalyst is weighed and dispersed into 1 mL of a mixed solution, wherein the solution includes: 0.5 mL of water, 0.5 mL of ethanol, and 20 μL of naphthol solution. The above solution is ultrasonicated for 30 minutes to obtain a slurry, which is evenly coated on a 1 cm 2 The working electrode was obtained by drying and pressing the nickel foam. The electrocatalytic oxygen evolution test used 1 mol / L KOH solution as the electrolyte and the scanning rate was 2 mV s -1 .
[0074] The results obtained:
[0075] (1) Figure 8 This is the XRD diffraction pattern of NiFeLDH. It can be seen from the figure that the main component of NiFeLDH is NiFeLDH.
[0076] (2) Fig. 9 This is the LSV diagram of NiFeLDH. It can be seen from the figure that NiFeLDH is 2 The required voltage is 1.60V.
[0077] It can be concluded from this comparative example that in the process of preparing NiFeLDH, there is no ZnO to promote dispersion, the oxygen evolution potential of the obtained NiFeLDH increases, and the performance is significantly reduced. Therefore, ZnO-promoted dispersion is an important step in preparing ZnO@NiFeLDH powder material of the present invention and cannot be omitted. Ignoring this step will cause the problem of increased oxygen evolution potential of the catalyst and decreased performance.
[0078] Comparative Example 2:
[0079] In this comparative example, the required raw materials are: nickel chloride hexahydrate, ferric chloride hexahydrate, anhydrous methanol, ammonium fluoride, urea, and 90 nm ZnO nanospheres.
[0080] This comparative example provides a fourth method for preparing a powder material for electrocatalytic water decomposition and oxygen evolution half-reaction. The catalyst prepared in this comparative example is ZnO@NiFeLDH, and its preparation method comprises the following steps:
[0081] Step 1: Weigh the chemicals required for solvothermal treatment, 0.02 g ZnO nanospheres, 0.09 M NiCl2·6H2O, 0.03 M FeCl3·6H2O, 1.59 g urea and 0.22 g ammonium fluoride;
[0082] Step 2: Add the drugs weighed in step 1 to the methanol solution at room temperature in order and stir evenly. The order of adding the drugs is ZnO nanospheres, nickel chloride hexahydrate, and ferric chloride hexahydrate. After stirring for 1 hour, continue to add urea and ammonium fluoride;
[0083] Step 3: Transfer the solution obtained in step 2 to a 50 ml polytetrafluoroethylene liner and place it in a stainless steel autoclave for solvothermal reaction at a reaction temperature of 120° C. for 8 h;
[0084] Step 4: Collect the powder material in step 3, clean it, and dry it at 60 degrees Celsius for 8 hours before use.
[0085] The ZnO@NiFeLDH of this comparative example is used as the working electrode in the electrocatalytic oxygen evolution reaction. Specifically, a mercury / mercury oxide electrode and a platinum wire electrode are selected as the reference electrode and the counter electrode, respectively; 5 mg of ZnO@NiFeLDH catalyst is weighed and dispersed into 1 mL of a mixed solution, wherein the solution includes: 0.5 mL of water, 0.5 mL of ethanol, and 20 μL of naphthol solution. The above solution is ultrasonicated for 30 minutes to obtain a slurry, which is evenly coated on a 1 cm 2The working electrode was obtained by drying and pressing the nickel foam. The electrocatalytic oxygen evolution test used 1 mol / L KOH solution as the electrolyte and the scanning rate was 2 mV s -1 .
[0086] The results obtained:
[0087] (1) Fig.10 The LSV diagram of ZnO@NiFeLDH shows that ZnO@NiFeLDH has a 2 The required voltage is 1.58V.
[0088] It can be concluded from this comparative example that although 90 nm ZnO nanospheres were added during the preparation of ZnO@NiFeLDH, the larger ZnO still affected the catalytic performance of ZnO@NiFeLDH. Compared with the ZnO@NiFeLDH prepared in Example 1, the oxygen evolution potential of the ZnO@NiFeLDH obtained in this comparative example was increased, and the performance was significantly reduced. Therefore, this comparative example proves that in the preparation method of the present invention, replacing ZnO with ZnO nanospheres is still not feasible, and it will still affect the performance of the obtained ZnO@NiFeLDH.
[0089] Comparative Example 3:
[0090] (1) As stated in the public literature (DOI: 10.1016 / j.matlet.2019.126826), the potential of RuO2 is 1.59 V when the current density is 10 mA cm-2;
[0091] (2) As stated in the public literature (DOI: 10.1021 / acsami.0c14521), the potential of RuO2 is 1.607 V when the current density is 10 mA cm-2;
[0092] (3) For example, in the public literature (DOI: 10.1016 / j.electacta.2020.136108), it is recorded that the potential of IrO2 is 1.77V when the current density is 10mA cm-2;
[0093] (4) As reported in the open literature (DOI: 10.1021 / acsami.0c08969), the IrO2 current density is 10 mA cm -2 The potential is 1.61V.
[0094] Therefore, compared with the oxygen evolution potential of the OER catalyst recorded in the above-mentioned public documents, compared with Example 1, the oxygen evolution potential of the ZnO@NiFeLDH prepared in the present invention is lower, and the performance of the prepared ZnO@NiFeLDH is relatively good.
[0095] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a powder material for electrocatalytic water decomposition and oxygen evolution half-reaction, wherein the catalyst is used as a catalyst for the oxygen evolution half-reaction in the water decomposition reaction, and is characterized by: The catalyst is a ZnO@NiFeLDH material, which is a powder material. The preparation method thereof comprises the following steps: Sp1: Weighing of raw materials: Weigh zinc acetate and dissolve it in alcohol to form a uniform zinc acetate alcohol solution; Sp2: Preparation of zinc oxide suspension: Stirring the alcohol solution of zinc acetate at high temperature to obtain zinc oxide suspension; Sp3: Weighing of solvent thermal reaction raw materials: Weighing of the chemicals required for solvent thermal reaction, including metal source, pH adjuster and surfactant. The metal source is selected from soluble nickel salt and soluble iron salt, the pH adjuster is selected from urea, and the surfactant is selected from ammonium fluoride; Sp4: Mixing and stirring: add the solvent heat required for the drug weighed in Sp3 to the zinc oxide suspension in Sp2, and stir evenly; Sp5: Solvothermal reaction: The solution obtained in Sp4 is transferred to a corrosion-resistant liner and placed in a stainless steel autoclave for a solvothermal reaction to obtain a powder material; Sp6: Drying: Collect the powder material described in Sp5, clean it and dry it for later use, which is the ZnO@NiFeLDH catalyst.
2. The preparation method according to claim 1, characterized in that: In the step Sp1, the alcohol is anhydrous methanol or anhydrous ethanol.
3. The preparation method according to claim 2, characterized in that: In the step Sp1, the concentration of the alcohol solution of zinc acetate is 0.01-0.05M.
4. The preparation method according to claim 1, characterized in that: In the step Sp2, the stirring temperature is 60° C., the stirring speed is 500-700 r / min, and the stirring time is 60-120 min.
5. The preparation method according to claim 1, characterized in that: In the step Sp3, in the metal source, the molar ratio of the soluble nickel salt to the soluble iron salt is 3:1, the feed concentration of the soluble nickel salt is 0.006-0.09M, and the feed concentration of the soluble iron salt is 0.002-0.03M.
6. The preparation method according to claim 5, characterized in that: In the step Sp3, the pH adjusting agent is selected such that the concentration of urea is 1.59-3.39 g / 100 ml; Regarding the selection of the surfactant, the concentration of the ammonium fluoride is 0.18-0.25 g / 100 ml.
7. The preparation method according to claim 1, characterized in that: In the step Sp4, before the solvent heat required chemicals are added, the zinc oxide suspension needs to be cooled to no higher than 30°C.
8. The preparation method according to claim 7, characterized in that: In the step Sp4, the order of adding the chemicals required for the solvent heat is soluble nickel salt and soluble iron salt; After the stirring time is 1 hour, urea and ammonium fluoride are added continuously.
9. The preparation method according to claim 1, characterized in that: In the step Sp5, the temperature of the solvothermal reaction is selected to be 120-160° C., and the reaction time of the solvothermal reaction is selected to be 8-16 h.
10. The preparation method according to claim 1, characterized in that: In the step Sp6, the drying temperature is not higher than 60° C., and the drying time is 8-10 hours.