Preparation method of resistance copper foil with high sheet resistance value uniformity and product thereof

By accurately controlling the pickling, coarse curing and electroplating process parameters of the resistive copper foil on the printed circuit board, the problem of poor uniformity of the square resistance value of the resistive copper foil is solved, and high uniformity and low-cost preparation of resistive copper foil is achieved.

CN118957688APending Publication Date: 2024-11-15ZHEJIANG GARDEN NEW ENERGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411011671.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the uniformity of square resistance value of resistive copper foil in printed circuit boards in large-scale production, and has poor versatility and high cost.

Method used

By accurately controlling the process parameters in the production process of resistive copper foil, including pickling treatment, rough curing treatment, and the regulation of the current density and production speed of the electroplating resistive layer, the uniformity of the square resistance value of the resistive copper foil is ensured.

Benefits of technology

The difference in square resistance value of resistive copper foil is less than 1.5Ω/□, which is simple to operate and low cost, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957688A_ABST
    Figure CN118957688A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a resistance copper foil with high sheet resistance value uniformity. The preparation method comprises the following steps: (1) carrying out acid pickling treatment on the surface of a raw foil; (2) carrying out coarse curing treatment on the crude foil treated in the step (1); the coarse curing treatment process comprises the steps of coarsening 1, curing 1, coarsening 2 and curing 2; (3) electroplating a resistance layer on the surface of the raw foil treated in the step (2) to obtain a resistance copper foil with high sheet resistance value uniformity; the current density at an inlet anode plate and the current density at an outlet anode plate of the electroplating resistance layer tank are controlled to be independently selected from 12.34-13.83 A / dm < 2 >, and the production speed is 2-5 m / min. According to the preparation method disclosed by the invention, the square resistance value of the prepared resistance copper foil can be more uniform only by accurately regulating and controlling process parameters in the preparation process, the operation is simple, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printed circuit boards, and relates to a preparation method of a resistor copper foil with high square resistance uniformity and a product thereof. Background Art

[0002] With the rapid development of the electronic information industry and the continuous updating of thin, light, short, high-performance portable electronic products, the printed circuit board (PCB) that supports electronic components is also increasingly developing in the direction of high density, multi-layer, easy packaging, and miniaturization. Burying a large number of passive device resistor copper foils in the PCB can effectively improve the electrical performance of the PCB, improve the reliability of the PCB, promote the development of the PCB in the direction of high density, save circuit panel space, and reduce production costs. Therefore, it is widely used in military industry, 5G communications, consumer electronics, automotive electronics and other fields. However, the resistor copper foil is etched into thinner lines in downstream applications, and the uniformity of the square resistance value of the resistor layer is the key indicator that customers are most concerned about. Therefore, improving the uniformity of the square resistance value of the resistor copper foil is a difficulty that copper foil companies need to overcome.

[0003] A Chinese patent document with application publication number CN 110473681 A discloses a method for chemical fine resistance adjustment of a nickel-phosphorus layer buried resistor, which first measures the initial resistance R1 before resistance adjustment, and controls the immersion time T of the resistor in the corrosive agent to obtain the target resistance R2. By controlling the time, the resistance change can be effectively and finely controlled to improve the resistance control accuracy. However, this technical solution is only applicable to buried resistors plated with a nickel-phosphorus alloy layer, and has poor versatility; it also requires additional corrosive agents, which is costly.

[0004] A Chinese patent document with application publication number CN 114582579 A provides a method for preparing a uniform nickel-phosphorus alloy resistor film using an adjustable heterogeneous nickel anode, wherein nickel rods arranged in a matrix perpendicular to the nickel anode plate are arranged on the nickel anode plate, the distance between the anodes is adjusted by adjusting the length of the nickel rods, and the uniformity of the nickel-phosphorus alloy resistor film is improved by adjusting the density of the nickel rods. Although the uniformity of the square resistance value has been improved, the square resistance non-uniformity is still large, and the implementation process of this method is complicated, and it is only suitable for execution in the laboratory, and it is difficult to apply it to mass production. Summary of the invention

[0005] In view of the above problems existing in the prior art, the present invention discloses a method for preparing a resistor copper foil with high uniformity of square resistance. The square resistance of the prepared resistor copper foil can be made more uniform only by precise regulation of process parameters in the preparation process. The operation is simple and the cost is low. The square resistance difference of the prepared resistor copper foil is less than 1.5Ω / □.

[0006] The specific technical solutions are as follows:

[0007] A method for preparing a resistor copper foil with high square resistance uniformity, comprising:

[0008] (1) Pickling the surface of the raw foil;

[0009] (2) performing a rough curing treatment on the raw foil treated in step (1);

[0010] The current density at the anode plate at the entrance of the roughening tank is 31.85-36.79A / dm 2 , the current density at the outlet anode plate is 13.95~14.94A / dm 2 ;

[0011] The current density at the entrance of the anode plate of the roughening tank is 17.9-21.85A / dm 2 The current density at the outlet anode plate is 14.94~15.92A / dm 2 ;

[0012] In the curing 1, the current density at the inlet anode plate and the current density at the outlet anode plate of the curing tank are independently selected from 20.86 to 22.84 A / dm 2 ;

[0013] In the curing 2, the current density at the inlet anode plate and the current density at the outlet anode plate of the curing tank are independently selected from 13.62 to 14.90 A / dm 2 ;

[0014] (3) electroplating a resistance layer on the surface of the raw foil treated in step (2) to obtain a resistance copper foil with high uniformity of square resistance;

[0015] The current density at the anode plate at the entrance of the electroplating resistor layer tank and the current density at the anode plate at the exit are independently selected from 12.34 to 13.83 A / dm 2 The production speed is 2-5m / min.

[0016] The preparation process of the present invention adjusts the uniformity of the square resistance value of the resistor copper foil from the above three aspects by precisely controlling the current density of the rough curing process, the current density of the electroplated resistor layer and the production speed.

[0017] In step (1):

[0018] The raw foil has a rough surface roughness MRz of less than 3.5 μm. The raw foil having a uniform ridge structure and a large number of dense ridges is selected. The raw foil has good ridge uniformity, which is beneficial to improving the uniformity of the square resistance value of the resistor layer in subsequent processes.

[0019] Preferably, the green foil thickness is 18 μm.

[0020] The pickling treatment uses an acidic solution selected from one or more of a sulfuric acid aqueous solution and a hydrochloric acid aqueous solution.

[0021] The purpose of pickling treatment is to remove the oxide layer formed on the surface of the raw foil due to long-term storage, so as to avoid the oxide layer affecting the copper nodule structure generated by the rough curing process.

[0022] Preferably, the pickling treatment is carried out in a 15 wt % sulfuric acid aqueous solution at a temperature of 25° C., and the production speed is 2 to 5 m / min.

[0023] In step (2):

[0024] When performing the rough curing treatment, the size of the copper nodule structure can be made more uniform by matching the appropriate rough curing current density. The experiment found that after the first high current density roughening, the copper nodule was plated on the surface of the copper foil, and then a curing was performed, which allowed the copper nodule to be deeply plated to the rough surface of the copper foil and become dense; then, weak roughening was performed on the basis of the previous strong roughening and consolidation, which allowed the copper nodule to grow further, and finally weak curing was performed to surround and reinforce the roughened copper nodule. By designing a suitable rough curing current, the number of copper nodules on the mountain shape is larger, and the size is larger and rounder, avoiding the tip effect in the subsequent electroplated resistor layer, which leads to uneven electroplating of the resistor layer.

[0025] The present invention not only adopts the rough curing method of roughening 1-curing 1-roughening 2-curing 2, but also further accurately controls the current density at the inlet anode plate and the current density at the outlet anode plate of the roughening tank during each roughening process, thereby ensuring that the square resistance of the electroplated copper foil finally prepared is more uniform.

[0026] Preferred:

[0027] In the plating solution used in the roughening 1, the copper ion concentration is 15-18 g / L, the sulfuric acid concentration is 90-110 g / L, and the plating solution temperature is 20-30°C;

[0028] In the plating solution used for the roughening 2, the copper ion concentration is 15-18 g / L, the sulfuric acid concentration is 90-110 g / L, and the plating solution temperature is 20-30°C.

[0029] In the plating solution used in the curing 1, the copper ion concentration is 35-45 g / L, the sulfuric acid concentration is 90-100 g / L, and the plating solution temperature is 20-50° C.;

[0030] In the plating solution used in the curing 2, the copper ion concentration is 35-45 g / L, the sulfuric acid concentration is 90-100 g / L, and the plating solution temperature is 20-50°C.

[0031] In step (3), the raw foil treated in step (2) is used as a cathode to electroplate a resistor layer, and the plating solution used includes a metal salt, hypophosphite and a buffer.

[0032] Preferably, the metal salt is selected from nickel salt and / or chromium salt;

[0033] If the metal salt contains nickel salt, the nickel ion concentration in the plating solution is 18-24 g / L;

[0034] If the metal salt contains chromium salt, the chromium ion concentration in the plating solution is 5-10g / L.

[0035] More preferably, the metal salt is selected from nickel salts and chromium salts.

[0036] Preferably, the concentration of hypophosphite ions in the plating solution is 5 to 8 g / L.

[0037] Preferably, the buffer is selected from sodium acetate and / or boric acid, and the concentration of the buffer in the plating solution is 16-20 g / L.

[0038] Preferably, the pH value of the plating solution is 1-3, and the plating solution temperature is 50-70°C.

[0039] The invention also discloses a resistor copper foil with high square resistance uniformity prepared according to the method.

[0040] In order to further test the square resistance value of the resistor copper foil prepared by the present invention, the prepared resistor copper foil needs to be cut, such as cutting to 10 cm×10 cm, and then the resistor layer of the resistor copper foil is pressed with the epoxy resin matrix at high temperature, and finally the copper layer is etched with an alkaline etching solution, and a four-probe square resistance tester is used to perform a square resistance test on each point of the exposed resistor layer after etching.

[0041] Compared with the prior art, the present invention has the following advantages:

[0042] The invention discloses a method for preparing a resistor copper foil with high uniform square resistance. On the basis of an existing production route, the square resistance of the resistor copper foil can be made more uniform only by accurately regulating three process parameters in the preparation process, namely, a rough curing current, an electroplating resistor layer current and a production vehicle speed. The method has simple operation and low cost. The square resistance difference of the prepared resistor copper foil is less than 1.5Ω / □. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a schematic diagram of the production process of the resistor copper foil disclosed in the present invention;

[0044] In the figure, 1-pickling tank, 2-roughening tank 1, 3-curing tank 1, 4-roughening tank 2, 5-curing tank 2, 6-electroplating resistor layer tank, 7-inlet anode plate, 8-outlet anode plate;

[0045] Figure 2 The scanning electron microscope morphology images of the resistor copper foil prepared in Example 1 at 0° (a) and 45° (b);

[0046] Figure 3 The scanning electron microscope morphology images of the resistor copper foil prepared in Example 2 at 0° (a) and 45° (b);

[0047] Figure 4 The scanning electron microscope morphology images of the resistor copper foil prepared in Example 3 at 0° (a) and 45° (b);

[0048] Figure 5 The scanning electron microscope morphology images of the resistor copper foil prepared in Comparative Example 1 at 0° (a) and 45° (b);

[0049] Figure 6 The scanning electron microscope morphology images at 0° (a) and 45° (b) of the resistor copper foil prepared in Comparative Example 2;

[0050] Figure 7 The scanning electron microscope morphology images of the resistor copper foil prepared in Comparative Example 3 at 0° (a) and 45° (b). DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below in conjunction with the embodiments and drawings. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0052] Unless otherwise specified, the test materials and reagents used in the following embodiments can be obtained from commercial sources. If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the field or according to the product instructions.

[0053] Example 1

[0054] (1) Take the raw foil

[0055] The raw foil is selected to have a thickness of 18μm and a rough surface roughness MRz=2.4μm. The raw foil with uniform mountain-shaped structure and a large number of dense mountains is selected. The raw foil has good mountain-shaped uniformity, which is beneficial to improving the uniformity of the square resistance value of the resistor layer in the subsequent process.

[0056] (2) Pickling treatment

[0057] The raw foil was pickled in a 15 wt % sulfuric acid aqueous solution at 25° C. and the production speed was 5 m / min.

[0058] The purpose of pickling treatment is to remove the oxide layer formed on the surface of the raw foil due to long-term storage, so as to avoid the oxide layer affecting the copper nodule structure generated by the rough curing process.

[0059] (3) Rough curing treatment

[0060] The pickled raw foil was subjected to a rough curing treatment, and the treatment process was roughening 1→curing 1→roughening 2→curing 2. The two roughening treatments used the same plating solution, the copper ion concentration in the plating solution was 18 g / L, the sulfuric acid concentration was 100 g / L, the plating solution temperature was 25°C, and the current density of the two roughening treatments was different, and the specific values ​​are listed in Table 1 below; the two curing treatments also used the same plating solution, the copper ion concentration in the plating solution was 40 g / L, the sulfuric acid concentration was 100 g / L, the plating solution temperature was 25°C, and the current density of the two curing treatments was also different, and the specific values ​​are listed in Table 1 below. The production speed of the rough curing treatment process is 5 m / min.

[0061] When performing the rough curing treatment, the size of the copper nodule structure can be made more uniform by matching the appropriate rough curing current density. The experiment found that after the first high current density roughening, the copper nodule was plated on the surface of the copper foil, and then a curing was performed, which allowed the copper nodule to be deeply plated to the rough surface of the copper foil and become dense; then, weak roughening was performed on the basis of the previous strong roughening and consolidation, which allowed the copper nodule to grow further, and finally weak curing was performed to surround and reinforce the roughened copper nodule. By designing a suitable rough curing current, the number of copper nodules on the mountain shape is larger, and the size is larger and rounder, avoiding the tip effect in the subsequent electroplated resistor layer, which leads to uneven electroplating of the resistor layer.

[0062] (4) Electroplating resistance layer

[0063] The copper foil after rough curing is used as the cathode for electroplating the alloy resistance layer. The nickel ion concentration in the plating solution is 20g / L, the chromium ion concentration is 5g / L, and the hypophosphite ion concentration is 5g / L; the content of the buffer boric acid in the plating solution is 16g / L. The pH value of the plating solution is adjusted to 1.5 by a 3wt% sodium hydroxide aqueous solution, and the plating solution temperature is controlled to 50°C. The current density at the inlet and outlet of the anode plate of the electroplating resistance layer tank is controlled to be 12.34A / dm 2 The production speed is 5m / min, and a resistor copper foil with high square resistance uniformity is prepared.

[0064] The current density and plating time of the electrodeposited alloy resistor layer can directly change the thickness of the resistor layer. As the current density and plating time increase, the thickness of the electroplated alloy layer increases. The resistance value follows the formula: R = ρL / A (R is the resistance value, ρ is the resistivity of the resistor material, L is the resistor length, and A is the cross-sectional area of ​​the resistor). According to the square resistance formula, the thinner the thickness of the resistor layer, the larger the square resistance value; conversely, the smaller the square resistance value.

[0065] Example 2

[0066] The raw foil of this embodiment has a thickness of 18 μm and a roughness of MRz=1.9 μm. The preparation process is basically the same as that of the embodiment 1, except that:

[0067] During the rough curing treatment in step (3), the rough curing current density is different, and the specific values ​​are listed in Table 1 below;

[0068] When the resistor layer is electroplated in step (4), the current density at the inlet and outlet of the anode plate of the electroplating resistor layer tank is replaced with 13.33A / dm 2 .

[0069] Example 3

[0070] The raw foil of this embodiment has a thickness of 18 μm and a roughness of MRz=1.9 μm. The preparation process is basically the same as that of the embodiment 1, except that:

[0071] During the pickling treatment in step (2), the production speed is replaced with 2 m / min;

[0072] During the rough curing treatment in step (3), the rough curing current density is different, and the specific values ​​are listed in Table 1 below. At the same time, the production vehicle speed of the rough curing treatment is also replaced with 2 m / min;

[0073] When the resistor layer is electroplated in step (4), the nickel ion concentration in the plating solution is 24 g / L, the chromium ion concentration is 9 g / L, and the hypophosphite ion concentration is 8 g / L; the content of the buffer boric acid in the plating solution is 20 g / L; and the current density at the inlet and outlet of the anode plate of the electroplating resistor layer tank is replaced with 13.83 A / dm 2 .

[0074] Comparative Example 1

[0075] The preparation process is basically the same as that of Example 1, the only difference being the rough curing current density during the rough curing treatment in step (3). The specific values ​​are listed in Table 1 below.

[0076] Comparative Example 2

[0077] The preparation process is basically the same as that of Example 2, except that the current density at the inlet and outlet of the anode plate of the electroplating resistor layer tank is replaced with 10.86 A / dm 2 .

[0078] Comparative Example 3

[0079] The preparation process is basically the same as that of Example 3, with the only difference being that when electroplating the resistor layer in step (4), the production vehicle speed is replaced with 10 m / min.

[0080] Table 1

[0081]

[0082] Performance Test:

[0083] The square resistance test was performed on the resistor copper foil prepared in each embodiment and comparative example. The specific test process is as follows:

[0084] The cut 10cm×10cm resistor copper foil resistor layer was glued to the epoxy resin substrate and maintained at 250℃ and 30Mpa pressure for 90min. The copper layer on the surface was etched with an alkaline etching solution composed of 160g / L ammonium chloride, 320g / L copper sulfate pentahydrate, and 360g / L 25wt% ammonia water. The etching time was 6min, and then it was cleaned and dried. The 10cm×10cm resistor copper foil square was divided into 9 equal parts, and each part was tested for transverse and longitudinal square resistance using a four-probe square resistance tester. A total of 18 sets of square resistance data were obtained, among which the square resistance average value was the average value of the 18 sets of square resistance data, the maximum square resistance value was the maximum value among the 18 sets of square resistance data, the minimum square resistance value was the minimum value among the 18 sets of square resistance data, and the square resistance difference was the difference between the maximum square resistance value and the minimum square resistance value. The specific values ​​are listed in Table 2.

[0085] Table 2

[0086]

[0087] From the results in Table 2, it can be seen that the square resistance value differences of Examples 1, 2, and 3, which simultaneously precisely control the rough curing current density, the current density of the electroplating resistor layer, and the production speed in the rough curing treatment process, are relatively low, and are significantly lower than those of Comparative Example 1 (improper control of the rough curing current density), Comparative Example 2 (improper control of the current density of the electroplating resistor layer), and Comparative Example 3 (improper control of the production speed of the electroplating resistor layer), and the square resistance value is more uniform.

[0088] Combined with the attached SEM image analysis, Figure 5 (b) (Comparative Example 1) and Figure 2 (b) (Example 1) Compared with the mountain-shaped copper nodules, the number of copper nodules is relatively large, and the copper nodule structure is more needle-shaped. This may be due to the fact that the rough curing current is too large, resulting in an enhanced tip effect, which in turn affects the uniformity of the square resistance value of the finally prepared resistor copper foil; Figure 6 (b) (Comparative Example 2) and Figure 3 (b) (Example 2) shows some copper nodules, which may be due to the current density during the electroplating of the resistor layer is too small, resulting in uneven plating of the resistor layer, which is not conducive to the uniformity of the square resistance value of the resistor copper foil; Figure 7 (Comparative Example 3) Figure 4(Example 3) Compared with the smaller number of copper nodules, the increase in production speed leads to a decrease in the number of roughly solidified copper nodules, sparse distribution of copper nodules, and uneven square resistance. Figure 2 , 3 、4 SEM morphology ratio Figure 5 , 6 , 7, and the copper nodule structure is more evenly dispersed. It can be seen that by adopting the disclosed solution of the present invention, a resistor copper foil with uniform square resistance can be produced.

Claims

1. A method for preparing a resistor copper foil with high square resistance uniformity, characterized in that: include: (1) Pickling the surface of the raw foil; (2) performing a rough curing treatment on the raw foil treated in step (1); The rough curing process comprises roughening 1-curing 1-roughening 2-curing 2; The current density at the anode plate at the entrance of the roughening tank is 31.85-36.79A / dm 2 The current density at the outlet anode plate is 13.95~14.94A / dm 2 ; The current density at the anode plate at the entrance of the roughening tank is 17.9-21.85A / dm 2 The current density at the outlet anode plate is 14.94~15.92A / dm 2 ; In the curing 1, the current density at the inlet anode plate and the current density at the outlet anode plate of the curing tank are independently selected from 20.86 to 22.84 A / dm 2 ; In the curing 2, the current density at the inlet anode plate and the current density at the outlet anode plate of the curing tank are independently selected from 13.62 to 14.90 A / dm 2 ; (3) electroplating a resistor layer on the surface of the copper nodule treated in step (2) to obtain a resistor copper foil with high uniformity of square resistance; The current density at the anode plate at the entrance of the electroplating resistor layer tank and the current density at the anode plate at the exit are independently selected from 12.34 to 13.83 A / dm 2 The production speed is 2-5m / min.

2. The method for preparing a resistor copper foil with high square resistance uniformity according to claim 1, characterized in that: In step (1): The raw foil has a rough surface roughness MRz < 3.5 μm; The pickling treatment uses an acidic solution selected from one or more of a sulfuric acid aqueous solution and a hydrochloric acid aqueous solution.

3. The method for preparing a resistor copper foil with high uniformity of square resistance according to claim 1, characterized in that: In step (2): In the plating solution used in the roughening 1, the copper ion concentration is 15-18 g / L, the sulfuric acid concentration is 90-110 g / L, and the plating solution temperature is 20-30°C; In the plating solution used in the roughening 2, the copper ion concentration is 15-18 g / L, the sulfuric acid concentration is 90-110 g / L, and the plating solution temperature is 20-30°C.

4. The method for preparing a resistor copper foil with high square resistance uniformity according to claim 1, characterized in that: In step (2): In the plating solution used in the curing 1, the copper ion concentration is 35-45 g / L, the sulfuric acid concentration is 90-100 g / L, and the plating solution temperature is 20-50° C.; In the plating solution used in the curing 2, the copper ion concentration is 35-45 g / L, the sulfuric acid concentration is 90-100 g / L, and the plating solution temperature is 20-50°C.

5. The method for preparing a resistor copper foil with high square resistance uniformity according to claim 1, characterized in that: In step (3), the copper foil treated in step (2) is used as a cathode to electroplate a resistor layer, and the plating solution used includes a metal salt, hypophosphite and a buffer.

6. The method for preparing a resistor copper foil with high square resistance uniformity according to claim 5, characterized in that: The metal salt is selected from nickel salts and / or chromium salts; If the metal salt contains nickel salt, the nickel ion concentration in the plating solution is 18-24 g / L; If the metal salt contains chromium salt, the chromium ion concentration in the plating solution is 5-10g / L.

7. The method for preparing a resistor copper foil with high square resistance uniformity according to claim 5, characterized in that: The concentration of hypophosphite ions in the plating solution is 5 to 8 g / L.

8. The method for improving the uniformity of square resistance of resistor copper foil according to claim 5, characterized in that: The buffer is selected from sodium acetate and / or boric acid, and the concentration of the buffer in the plating solution is 16-20 g / L.

9. The method for preparing a resistor copper foil with high square resistance uniformity according to claim 5, characterized in that: The pH value of the plating solution is 1-3, and the plating solution temperature is 50-70°C.

10. A resistor copper foil with high uniformity of square resistance prepared by the method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Resistance-embedded metal foil and application thereof

    CN121397876A

  • Resistance copper foil with high peel strength and uniform sheet resistance value and preparation method thereof