Middle-high voltage electrode foil pretreatment method for improving specific volume and reducing boosting time and leakage current
Optimizing the pretreatment process of medium and high voltage electrode foil through ultrasonic treatment and pretreatment liquid treatment, the problem of difficult reduction of leakage current and boost time in the prior art is solved, and the specific capacity and comprehensive performance are significantly improved, which is suitable for high voltage and medium voltage. Electrode foil.
Patent Information
- Application Number
- CN202410966398.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to improve leakage current performance and reduce the boost time while ensuring other performance of medium and high voltage electrode foils, especially the boost time after boiling, and the existing methods do not have the effect of pretreatment of medium and high voltage foils. This results in low service life and productivity of the capacitor.
A medium and high voltage electrode foil pretreatment method is adopted, including pretreatment and boiling treatment, through sonication and pretreatment liquid treatment, the specific steps include ultrasonication of the corrosive foil in water of 45 to 60°C, and then in the pretreatment liquid The pretreatment solution is an aqueous solution of subphosphites and their salts and phosphate and their ammonium salts. The ultrasonic treatment temperature is 50-85℃, the frequency is 30-100kHz, and the time is 3-10 minutes. It is optimized to be transformed into Process to reduce the amount of boric acid.
The specific capacitance of the medium and high voltage electrode foil is significantly improved, the leakage current and boost time is reduced, the boost time after boiling is improved, and the comprehensive performance of the electrode foil is improved. It is suitable for high-voltage and medium-voltage foil.
Smart Images

Figure BDA0004951892880000101 
Figure BDA0004951892880000111 
Figure BDA0004951892880000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemically formed foil production, and in particular relates to a medium- and high-voltage electrode foil pretreatment method for improving specific capacity and reducing boost time and leakage current. Background Art
[0002] Capacitors have the functions of filtering, coupling and energy storage in electronic circuits. They are irreplaceable basic components in various electronic products and are widely used in various fields. Aluminum foil is a commonly used electrode material for capacitors. As the anode of the capacitor, the performance of aluminum foil largely determines the performance of the capacitor and is a key consideration in the design, production and application of capacitors.
[0003] The parameters that measure the performance of formed foil mainly include: boost time, leakage current, specific capacitance, boost time after boiling, residual chloride ion, etc. The boost time and leakage current of formed foil affect the performance and service life of capacitors. Long boost time and large leakage current of formed foil will lead to low aging pass rate and long aging time during capacitor production, affecting the overall yield and production efficiency. It may also cause the capacitor leakage current to rebound and increase, and even cause early failure of capacitors. Therefore, while the current trend of formed foil is developing towards high withstand voltage and high specific capacitance, the requirements for its leakage current and boost time are becoming more and more stringent.
[0004] CN103177878A discloses a method for forming an ultra-high voltage anode foil, which comprises placing the ultra-high voltage corrosion foil in water vapor at 130-150°C for 5-20 minutes; taking it out and soaking it in a diammonium hydrogen citrate solution containing 0.2-1.0 wt% at 60-80°C for 1-5 minutes; taking it out and performing subsequent forming treatment. The method can make the formed anode foil have stable performance, the boost time is less than 200 seconds, and the product leakage current is less than 25μA / cm 2 However, the voltage rise time is still relatively long, and since this method produces ultra-high voltage anode foil, it is not suitable for medium and high voltage anode foil.
[0005] CN111613446A discloses a chemical treatment method for a high water-resistant low-voltage anode foil. An ultrasonic treatment step is added during the electrochemical oxidation process to accelerate the dissolution of bubbles in the pores during the reaction, reduce the generation of oxide film defects, and in the heat treatment process, microwave heating is used to replace the traditional oven to selectively heat the area with high water content, further improving the uniformity and density of the oxide film. Compared with aluminum foil prepared by conventional chemical formation process, the hydration resistance of aluminum foil prepared by the method disclosed in the present invention can be improved by 50-80%, and the service life is extended to 20,000 hours. However, this method produces low-pressure platinum, and the low-pressure foil is a hard foil with a sponge-like hole shape; the medium and high-voltage foil is a soft foil with a tunnel-like hole shape; the two are essentially different, with different application fields and different parameter requirements, and the requirements for low-pressure foil are very loose. In addition, the longer the pressure-boosting time before hydration, the poorer the oxide film on the surface of the aluminum foil, and the oxide film needs to be repaired during the pressure-boosting time test (the process of detecting the pressure-boosting time is also a process of forming or repairing the oxide film); the longer the pressure-boosting time after hydration, the more oxide film is destroyed during the hydration process (high temperature or boiling water), so the hydration resistance cannot be improved as described in this method.
[0006] CN113026073A A method for forming an ultra-high voltage electrode foil, which relates to the technical field of electrode foil, comprises the following steps:
[0007] Step 1: boiling the corroded foil in a silicate solution at a temperature above 95°C to obtain a pre-treated foil; Step 2: chemically converting the pre-treated foil in a boric acid and ammonium pentaborate solution to obtain a primary chemically converted foil; Step 3: chemically converting the primary chemically converted foil in a boric acid and ammonium pentaborate solution to obtain a secondary chemically converted foil; Step 4: subjecting the secondary chemically converted foil to multi-stage chemical conversion in a boric acid, ammonium pentaborate and ammonium glutarate solution to obtain a final chemically converted foil product; The beneficial effects of the present invention are: the electrolyte composition is simple and easy to control in production, and the wastewater treatment is relatively simple; the present invention does not increase the flash voltage by reducing the conductivity of the chemically converted solution, the ineffective power loss in the chemically converted process is greatly reduced, there is no flash spot on the surface of the chemically converted foil, the dielectric property of the oxide film is good, the product boost time is less than 150 seconds, and the leakage current is less than 12μA / cm 2 , which is suitable for the production needs of 1000-1500V ultra-high voltage electrode foil. However, in this method, the purpose of the pretreatment step is only to increase the flash voltage; its leakage current and boost time are related to its formation process, that is, this method reduces the boost time and leakage current through high content of boric acid, but this will inevitably lead to a very low specific capacitance.
[0008] CN114197004B discloses a method for forming medium and high voltage foil for aluminum electrolytic capacitors. Through a specific process design, the hydration treatment can form a hydrated oxide film on the surface of the aluminum foil, which provides a basis for the subsequent formation of a crystalline oxide film; the primary and secondary formation treatments can form a basic oxide film on the surface of the aluminum foil, and the use of ammonium hydrogen phosphate, hypophosphite and fumaric acid can generate a phosphating film of a substance that is difficult to dissolve in water and a fumaric acid polymer film, inhibiting the reaction between aluminum and water and improving the hydration resistance; the tertiary, quaternary, five-level and six-level formation treatments form a stable oxide film on the surface of the aluminum foil to improve the specific volume. The method does not contain boron elements in the entire formation process, and the medium-voltage and high-voltage foils prepared by the formation method have high specific volume, high bending properties and high hydration resistance. However, the inventor found in production that the leakage current performance of this method is poor. However, in this field, due to the demand for the fields in which capacitors made of chemical foil are used, the chemical foil focuses on or tends to have a certain performance parameter. If the boric acid content is increased, although the leakage current will be improved, the specific capacitance will be reduced. Therefore, the inventors think about how to improve the leakage current performance while ensuring other properties of medium and high voltage chemical foil.
[0009] CN109859949A discloses a method for reducing leakage current of medium and high voltage chemical foil, comprising: sequentially subjecting the corroded foil or the laminated foil to pretreatment, four-stage chemical formation, first heat treatment, first immersion, first re-forming treatment, second immersion, second re-forming treatment, second heat treatment, third re-forming treatment, third immersion and post-treatment to obtain the chemical foil. The pretreatment comprises hydration treatment and solution immersion treatment. The method removes the loose porous hydrated oxide layer of the outermost layer of the oxide film by immersing the corroded foil or the laminated foil after the hydration treatment in an organic acid solution or a weakly alkaline inorganic salt solution for solution immersion treatment, and improves the properties of the hydrated oxide film, thereby reducing leakage current and increasing the service life of the electrolytic capacitor. However, in this method, although the organic acid solution or the weakly alkaline inorganic salt solution has the effect of dissolving the loose porous hydrated oxide layer with defects, its pretreatment effect is general; and in this method, the leakage current performance is improved by high boric acid, but the specific volume is significantly reduced.
[0010] CN114540908A discloses a chemical formation treatment method for high-quality low-voltage anode foil, which includes adding ultrasonic treatment during energization; performing chemical formation treatment on the energized anode foil; placing the anode foil to be chemically treated in an ammonium dioxide solution for chemical formation, and adding current during chemical formation to obtain a primary chemically formed foil; chemically forming the primary chemically formed foil in the ammonium dioxide solution to obtain a secondary chemically formed foil; chemically forming the secondary chemically formed foil in the ammonium dioxide solution, and adding current during chemical formation to obtain a tertiary chemically formed foil; chemically forming the tertiary chemically formed foil in the ammonium dioxide solution, repeating the multi-stage chemical formation to obtain a six-stage chemically formed foil; depolarizing the obtained six-stage chemically formed foil; performing post-chemical treatment on the depolarized anode foil to obtain a final chemically formed foil product. This method accelerates the dissolution of bubbles in the pores of the aluminum foil during the reaction process by adding ultrasonic treatment during energization, thereby increasing the quality of oxide film formation and reducing the defects of the oxide film; improving the uniformity and density of the oxide film through six-stage formation; and improving the hydration resistance and moisture resistance of the oxide film and the service life of the electrode foil during passivation treatment. However, this method is only applicable to low-voltage foils because low-voltage foils are hard foils with high tensile strength, and the ultrasonic process will not affect the shape of the foil; however, medium and high voltage foils are soft foils, and the shape of the foil will change during the ultrasonic process. Although the hardness of the aluminum foil increases after the oxide film is formed, its brittleness also increases, and it is easy to be affected by the ultrasonic treatment, and even the aluminum foil breaks. Therefore, this method is not applicable to medium and high voltage formed foils. Summary of the invention
[0011] The present invention conducts in-depth research on the pretreatment process of medium and high voltage electrode foils in order to simultaneously improve the specific capacity of medium and high voltage electrode foils, reduce leakage current, boost time and boost time after boiling, and improve the comprehensive performance of high voltage electrode foils.
[0012] To achieve the above object, the present invention provides a medium and high voltage electrode foil pretreatment method for improving specific capacity, reducing boost time and leakage current, which comprises the following steps:
[0013] A. Pretreatment: Place the corroded foil in water for ultrasonic treatment;
[0014] B. Boiling treatment: Boil the corroded foil after pre-treatment in water;
[0015] C. Pretreatment liquid treatment: the boiled corroded foil is placed in the pretreatment liquid for ultrasonic treatment, and then cleaned to obtain the pretreated foil;
[0016] Wherein, in step A, the temperature of the ultrasonic treatment is 45-60°C, the frequency is 30-100kHz, and the time is 3-6min;
[0017] In step C, the pretreatment liquid is an aqueous solution of hypophosphorous acids and their salts and phosphoric acids and their ammonium salts, the total concentration of the hypophosphorous acids and their salts and phosphoric acids and their ammonium salts is 0.4-3wt%, and the mass concentration ratio of the hypophosphorous acids and their salts to the phosphoric acids and their ammonium salts is 4-9:1; or the pretreatment liquid is an aqueous solution of olefin polycarboxylic acids and their ammonium salts, and the concentration of the olefin polycarboxylic acids and their ammonium salts is 0.5-3wt%;
[0018] In step C, the temperature of the ultrasonic treatment is 50-85° C., the frequency is 30-100 kHz, and the ultrasonic time is 3-10 minutes.
[0019] Preferably, in the above-mentioned medium- and high-voltage electrode foil pretreatment method, in step A, the temperature of the ultrasonic treatment is 50-55° C., the frequency is 50 kHz, and the time is 4-5 min.
[0020] Wherein, in the above-mentioned medium and high voltage electrode foil pretreatment method, in step A, the corroded foil is corroded aluminum foil with a purity of 99.99wt%.
[0021] Wherein, in the above-mentioned medium and high voltage electrode foil pretreatment method, in step B, the boiling temperature is 85-100° C., and the time is 3-20 minutes.
[0022] Among them, in the above-mentioned medium and high voltage electrode foil pretreatment method, in step C, the hypophosphorous acids and their salts are at least one of hypophosphorous acid, sodium hypophosphite, potassium hypophosphite or ammonium hypophosphite, and the phosphoric acids and their ammonium salts are at least one of phosphoric acid, ammonium hydrogen phosphate or diammonium phosphate.
[0023] Preferably, in the above-mentioned medium- and high-voltage electrode foil pretreatment method, in step C, the hypophosphorous acid and its salt are ammonium hypophosphite, and the phosphoric acid and its ammonium salt are diammonium phosphate.
[0024] Preferably, in the above-mentioned medium and high voltage electrode foil pretreatment method, in step C, the total concentration of the hypophosphorous acids and their salts and the phosphoric acids and their ammonium salts is 0.5-0.6wt%, and the mass concentration ratio of the hypophosphorous acids and their salts and the phosphoric acids and their ammonium salts is 5-7:1.
[0025] Wherein, in the above-mentioned medium and high voltage electrode foil pretreatment method, in step C, the olefin polycarbon carboxylic acid and its ammonium salt are at least one of maleic acid, fumaric acid or ammonium hydrogen maleate.
[0026] Preferably, in the above-mentioned medium- and high-voltage electrode foil pretreatment method, in step C, the olefin polycarboxylic acid and its ammonium salt are maleic acid.
[0027] Preferably, in the above-mentioned medium- and high-voltage electrode foil pretreatment method, in step C, the temperature of the ultrasonic treatment is 55-65° C., the frequency is 50 kHz, and the ultrasonic treatment time is 5-8 minutes.
[0028] Among them, in the above-mentioned medium and high voltage electrode foil pretreatment method, during continuous production, the corroded foil can be directly cleaned after the pretreatment process and continue the chemical process, and no drying is required at this time; if the production process is non-continuous, the pretreatment process can be used as a separate production process, and the foil treated with the pretreatment liquid is cleaned and dried, and the drying temperature of the drying step is 60-200°C, and the time is 1-10 minutes.
[0029] In the present invention, the pretreated aluminum foil can be chemically formed according to conventional chemical forming processes in the art to obtain medium-high voltage chemically formed foil, for example, the medium-high voltage chemically formed foil forming method in CN114197004B can be used, or the chemical forming process in the embodiment of the present invention can be used. Due to the influence of the pretreatment of the present invention, the amount of boric acid used in the chemical forming process is reduced. In the embodiment of the present invention, the chemical forming process is specifically as follows:
[0030] Primary chemical treatment: The pretreated aluminum foil is taken out and placed in an aqueous solution of 0.1-2wt% ammonium citrate, 0.1-0.5wt% boric acid, 0.001-0.1wt% hypophosphite and 0.1-2wt% citric acid, and then heated at a current density of 20-100 mA / cm 2 , under the condition of the forming temperature of 80-95°C, when the medium pressure is formed, the voltage is 70-130V, and the forming time is 3-5 minutes, a primary formed aluminum foil is obtained; when the high pressure is formed, the voltage is 150-230V, and the forming time is 4-7 minutes, a primary formed aluminum foil is obtained;
[0031] Secondary chemical treatment: the primary chemical aluminum foil is placed in an aqueous solution of 0.05-1wt% ammonium citrate, 0.2-0.8wt% boric acid, 0.001-0.1wt% hypophosphite and 0.05-1wt% citric acid, and then heated at a current density of 20-100 mA / cm 2 , under the condition of the forming temperature of 80-95°C, when the medium pressure is formed, the voltage is 120-190V, and the forming time is 3-5 minutes to obtain the secondary formed aluminum foil; when the high pressure is formed, the voltage is 220-340V, and the forming time is 4-7 minutes to obtain the secondary formed aluminum foil;
[0032] The secondary chemical treatment: the secondary chemical aluminum foil is placed in an aqueous solution of 0.01-1wt% ammonium citrate, 1.5-2.8wt% boric acid, 0.01-1wt% azelaic acid ammonium salt and 0.01-1wt% citric acid, and then the current density is 20-100mA / cm 2 , under the condition of the forming temperature of 80-95°C, when the medium pressure is formed, the voltage is 180-250V, the forming time is 4.5-7.5 minutes, and the three-level formed aluminum foil is obtained; when the high pressure is formed, the voltage is 350-450V, the forming time is 6-10 minutes, and the three-level formed aluminum foil is obtained;
[0033] First-stage feed tank liquid feed: Place the third-stage aluminum foil in an aqueous solution of 2-4wt% ammonium citrate and 0.01-0.5vol% ammonia, and then at a formation voltage of <25V and a current density of 20-100mA / cm 2 , under the condition of forming temperature <35°C, reverse power is applied, when forming at medium voltage, forming for 1.5 to 3 minutes, and a first-level feed forming aluminum foil is obtained; when forming at high voltage, forming for 2 to 4 minutes, and a first-level feed forming aluminum foil is obtained;
[0034] Four-stage chemical treatment: the first-stage feed-type aluminum foil is placed in an aqueous solution of 0.01-1wt% ammonium citrate, 0.6-1.5wt% boric acid, 0.01-1wt% azelaic acid ammonium salt and 0.005-1wt% citric acid, and then the current density is 20-100mA / cm 2 , under the condition of the forming temperature of 80-95°C, when the medium pressure is formed, the voltage is 210-300V, the forming time is 4.5-7.5 minutes, and the four-level formed aluminum foil is obtained; when the high pressure is formed, the voltage is 400-520V, the forming time is 6-10 minutes, and the four-level formed aluminum foil is obtained;
[0035] Five-stage chemical treatment: The four-stage chemical aluminum foil is placed in an aqueous solution of 0.01-1wt% ammonium citrate, 0.6-1.5wt% boric acid, 0.005-1wt% azelaic acid ammonium salt and 0.005-1wt% citric acid, and then heated at a current density of 20-100 mA / cm 2 , under the condition of the forming temperature of 80-95°C, when the medium pressure is formed, the voltage is 210-350V, the forming time is 6-10 minutes, and the five-level formed aluminum foil is obtained; when the high pressure is formed, the voltage is 500-580V, the forming time is 8-14 minutes, and the five-level formed aluminum foil is obtained;
[0036] Secondary feeding tank liquid feeding: the five-level aluminum foil is placed in an aqueous solution of 2-4wt% ammonium citrate and 0.01-0.5vol% ammonia, and then the formation voltage is less than 25V and the current density is 20-100mA / cm 2 , under the condition of forming temperature <35°C, reverse power is applied, when forming at medium voltage, forming for 1.5 to 3 minutes, and a secondary feed forming aluminum foil is obtained; when forming at high voltage, forming for 2 to 4 minutes, and a secondary feed forming aluminum foil is obtained;
[0037] Six-stage chemical treatment: The secondary feed-type aluminum foil is placed in an aqueous solution of 0.01-1wt% ammonium citrate, 0.6-1.5wt% boric acid, 0.005-1wt% azelaic acid ammonium salt and 0.005-1wt% citric acid, and then heated at a current density of 20-100 mA / cm 2, under the condition of the forming temperature of 80-95°C, when the medium pressure is formed, the voltage is 210-380V, the forming time is 9-15 minutes, and the six-level formed aluminum foil is obtained; when the high pressure is formed, the voltage is 500-630V, the forming time is 12-21 minutes, and the six-level formed aluminum foil is obtained;
[0038] Primary phosphoric acid treatment: the six-stage phosphoric acid treatment solution is placed in a 0.5-3 vol% phosphoric acid treatment solution without electricity. When the medium pressure is formed, the aluminum foil is immersed at a temperature of 45-60°C for 0.5-2 minutes to obtain a primary phosphoric acid-treated aluminum foil; when the high pressure is formed, the aluminum foil is immersed at a temperature of 45-60°C for 1-3 minutes to obtain a primary phosphoric acid-treated aluminum foil;
[0039] Primary high temperature treatment: Take out the primary phosphated aluminum foil, and heat treat it at a high temperature of 450-550°C for 1-3 minutes when it is medium pressure-type, and obtain the primary high temperature-type aluminum foil; when it is high pressure-type, heat treat it for 1.5-4 minutes to obtain the primary high temperature-type aluminum foil;
[0040] Primary repair treatment: The primary high temperature aluminum foil is placed in an aqueous solution of 0.001-1wt% ammonium carbonate, 0.6-1.5wt% boric acid, 0.002-1wt% azelaic acid ammonium salt and 0.001-1wt% citric acid, and then heated at a current density of 20-100 mA / cm 2 , under the condition of forming temperature of 80-95°C, when forming at medium pressure, the voltage is 210-380V, forming for 3-5 minutes, and a first-level repaired aluminum foil is obtained; when forming at high pressure, the voltage is 500-630V, forming for 4-7 minutes, and a first-level repaired aluminum foil is obtained;
[0041] Secondary phosphoric acid treatment: the primary repaired aluminum foil is placed in a 3-8 vol% phosphoric acid treatment solution without electricity. When the medium pressure is formed, it is immersed at a temperature of 55-65°C for 3.5-8 minutes to obtain a secondary phosphorylated aluminum foil; when the high pressure is formed, it is immersed at a temperature of 55-65°C for 6-12 minutes to obtain a secondary phosphorylated aluminum foil;
[0042] Secondary repair treatment: The secondary phosphorylated aluminum foil is placed in an aqueous solution of 0.001-1wt% ammonium carbonate, 0.6-1.5wt% boric acid, 0.002-1wt% azelaic acid ammonium salt and 0.001-1wt% citric acid, and then heated at a current density of 20-100 mA / cm 2 , under the condition of the forming temperature of 80-95°C, when the medium pressure forming is performed, the voltage is 210-380V, the forming time is 3-5 minutes, and the secondary repaired formed aluminum foil is obtained; when the high pressure forming is performed, the voltage is 500-630V, the forming time is 4-7 minutes, and the secondary repaired formed aluminum foil is obtained;
[0043] Secondary high temperature treatment: Take out the secondary repaired aluminum foil and heat treat it at a high temperature of 250-450°C for 0.5-2 minutes when it is formed under medium pressure to obtain a secondary high temperature aluminum foil; when it is formed under high pressure, heat treat it for 1-3 minutes to obtain a secondary high temperature aluminum foil;
[0044] The third-level repair treatment: the secondary high-temperature aluminum foil is placed in an aqueous solution of 0.001-1wt% ammonium carbonate, 0.6-1.5wt% boric acid, 0.002-1wt% azelaic acid ammonium salt and 0.001-1wt% citric acid, and then heated at a current density of 20-100 mA / cm 2 , under the condition of the forming temperature of 70-80°C, when the medium pressure forming, the voltage is 210-380V, the forming time is 3-5 minutes, and the medium treatment forming aluminum foil is obtained; when the high pressure forming, the voltage is 500-630V, the forming time is 4-7 minutes, and the medium treatment forming aluminum foil is obtained;
[0045] Finishing treatment: placing the medium-treated aluminum foil in an aqueous solution of 0.5-2 wt% ammonium hydrogen phosphate and 0.01-1 vol% phosphoric acid, and treating it at a temperature of 55-65° C. for 1-3 minutes during medium-pressure forming to obtain a fine-treated aluminum foil; and treating it at a temperature of 55-65° C. for 2-5 minutes during high-pressure forming to obtain a fine-treated aluminum foil;
[0046] Drying: After taking out the refined aluminum foil, dry it at 180-220°C for 1-4 minutes to obtain medium-high pressure aluminum foil.
[0047] In the above-mentioned chemical formation process of the present invention, the ammonium citrate salt is diammonium citrate or triammonium citrate.
[0048] The present invention adds multiple ultrasonic treatment operations during the pretreatment process, which has a better dissolution effect on the loose porous hydrated oxide layer with defects in the aluminum foil. At the same time, a pretreatment liquid is added to attach hypophosphite, phosphate or olefin polycarbon carboxylate to the surface of the hydrated oxide film of the aluminum foil and the surface of the hydrated oxide film in the tunnel-type holes. After the oxide film is covered in the subsequent formation step, the phosphorus content or the olefin polycarbon carboxylate content in the aluminum foil is increased, thereby improving the hydration resistance.
[0049] Beneficial effects of the present invention:
[0050] The present invention optimizes the pretreatment process and screens a large number of pretreatment means, ultrasonic temperature and time, pretreatment liquid and ultrasonic time in the pretreatment process, etc., thereby not only improving the specific volume, but also reducing the leakage current, boost time and boost time after boiling, and significantly improving the comprehensive performance of the high-voltage electrode foil. The method of the present invention is not only applicable to high-voltage chemical foil, but also to medium-voltage chemical foil. DETAILED DESCRIPTION
[0051] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.
[0052] The detection method in the embodiment of the present invention is: In the "China Electronic Components Industry Association Group Standard T / CECA 22-2017 Electrode Foil for Aluminum Electrolytic Capacitors", the hydration resistance test refers to washing the test piece that has been subjected to the oxide film withstand voltage test with pure water and then placing it in 500ml pure water above 95°C, water bathing for 60±1 min, and then measuring the oxide film withstand voltage and boost time. The time taken for the chemical foil to be boosted to 90% of the rated withstand voltage (Vf) according to the specified current is the boost time; the boost time after the hydration resistance test, that is, Tr(60)≤150s, is judged to be qualified. The hydration resistance test is a destructive test. The shorter the boost time after the hydration resistance test, the stronger the hydration resistance of the chemical foil and the better the quality of the chemical foil.
[0053] For details on the voltage rise time, withstand voltage, specific capacity (specific surface electrostatic capacitance), and voltage rise time after boiling (TR60, hydration resistance, and water boiling resistance), please refer to Appendix A of the China Electronic Components Industry Association Group Standard T / CECA 22-2017 Electrode Foil for Aluminum Electrolytic Capacitors: Test Methods for Withstand Voltage and Voltage Rise Time; Appendix B: Test Methods for Electrode Foil Electrostatic Capacitance.
[0054] Rising time, withstand voltage, and rising time after boiling tests, testing instrument: TV1000-3 aluminum foil characteristics intelligent testing system.
[0055] Specific capacitance test, testing instrument: TH2618B capacitance tester.
[0056] Leakage current test, detection instrument: TV-1000B aluminum foil characteristics intelligent test system.
[0057] The formation process in the embodiments, comparative examples and test examples of the present invention is as follows:
[0058] Primary chemical treatment: The pretreated aluminum foil was taken out and placed in an aqueous solution of 0.4wt% diammonium citrate, 0.2wt% boric acid, 0.002wt% hypophosphite and 0.1wt% citric acid, and then heated at a voltage of 150V and a current density of 80mA / cm 2 , under the condition of forming temperature of 85±3℃, forming for 5.4 minutes, a primary formed aluminum foil is obtained;
[0059] Secondary chemical treatment: The primary chemically treated aluminum foil was placed in an aqueous solution of 0.3wt% diammonium citrate, 0.5wt% boric acid, 0.001wt% hypophosphite and 0.08wt% citric acid, and then heated at a voltage of 280V and a current density of 80mA / cm 2, under the condition of forming temperature of 85±3℃, forming for 5.4 minutes, a secondary forming aluminum foil is obtained;
[0060] The secondary chemical treatment: the secondary chemical aluminum foil is placed in an aqueous solution of 0.1wt% diammonium citrate, 2.5wt% boric acid, 0.2wt% azelaic acid ammonium salt and 0.05wt% citric acid, and then the chemical treatment is carried out at a voltage of 390V and a current density of 80mA / cm 2 , forming at a temperature of 85±3°C for 8 minutes to obtain a three-stage formed aluminum foil;
[0061] Liquid feeding of the first-stage feeding tank: the third-stage aluminum foil is placed in an aqueous solution of 3.5wt% triammonium citrate and 0.1vol% ammonia water, and then the formation voltage is less than 25V and the current density is 80mA / cm 2 , under the condition of forming temperature <35°C, reverse power is applied and the forming time is 3 minutes to obtain a first-level feeding forming aluminum foil;
[0062] Four-stage chemical treatment: The first-stage feed-type aluminum foil is placed in an aqueous solution of 0.05wt% diammonium citrate, 1.1wt% boric acid, 0.01wt% azelaic acid ammonium salt and 0.01wt% citric acid, and then the formation voltage is 470V and the current density is 80mA / cm 2 , forming at a temperature of 85±3°C for 8 minutes to obtain a fourth-grade formed aluminum foil;
[0063] Five-stage chemical treatment: The four-stage chemically treated aluminum foil is placed in an aqueous solution of 0.03wt% diammonium citrate, 1.1wt% boric acid, 0.01wt% azelaic acid ammonium salt and 0.01wt% citric acid, and then heated at a voltage of 500V and a current density of 80mA / cm 2 , under the condition of forming temperature of 85±3℃, forming for 11 minutes to obtain five-level formed aluminum foil;
[0064] Secondary feeding tank liquid feeding: The five-level aluminum foil is placed in an aqueous solution of 3.5wt% triammonium citrate and 0.1vol% ammonia water, and then the formation voltage is less than 25V and the current density is 80mA / cm 2 , under the condition of forming temperature <35°C, reverse power is applied and the forming time is 3 minutes to obtain a secondary feeding formed aluminum foil;
[0065] Six-stage chemical treatment: The secondary feed-type aluminum foil is placed in an aqueous solution of 0.01wt% diammonium citrate, 1.0wt% boric acid, 0.005wt% azelaic acid ammonium salt and 0.01wt% citric acid, and then heated at a voltage of 520V and a current density of 80mA / cm 2 , under the condition of forming temperature of 85±3℃, forming for 16 minutes to obtain the sixth grade formed aluminum foil;
[0066] Primary phosphoric acid treatment: the sixth-grade aluminum foil is placed in a 1.5 vol% phosphoric acid treatment solution without adding electricity, and immersed at a temperature of 50° C. for 2 minutes to obtain a primary phosphoric acid-treated aluminum foil;
[0067] Primary high temperature treatment: Take out the primary phosphorylated aluminum foil and heat treat it at a high temperature of 500±20℃ for 2.4 minutes to obtain the primary high temperature phosphorylated aluminum foil;
[0068] Primary repair treatment: The primary high temperature aluminum foil is placed in an aqueous solution of 0.01wt% ammonium carbonate, 1.0wt% boric acid, 0.05wt% azelaic acid ammonium salt and 0.005wt% citric acid, and then heated at a voltage of 520V and a current density of 80mA / cm 2 , under the condition of forming temperature of 85±3℃, forming for 5.4 minutes, a first-grade repaired aluminum foil was obtained;
[0069] Secondary phosphoric acid treatment: the primary repaired aluminum foil is placed in a 6 vol% phosphoric acid treatment solution again, without electricity, and immersed at a temperature of 60° C. for 6.5 minutes to obtain a secondary phosphoric acid-treated aluminum foil;
[0070] Secondary repair treatment: The secondary phosphorylated aluminum foil was placed in an aqueous solution of 0.01wt% ammonium carbonate, 1.0wt% boric acid, 0.05wt% azelaic acid ammonium salt and 0.005wt% citric acid, and then heated at a voltage of 520V and a current density of 80mA / cm 2 , under the condition of forming temperature of 85±3℃, forming for 5.4 minutes, a secondary repaired formed aluminum foil was obtained;
[0071] Secondary high temperature treatment: Take out the secondary repaired aluminum foil and heat treat it at a high temperature of 300±20℃ for 1.8 minutes to obtain the secondary high temperature aluminum foil;
[0072] Level 3 repair treatment: The secondary high-temperature aluminum foil is placed in an aqueous solution of 0.01wt% ammonium carbonate, 1.0wt% boric acid, 0.05wt% azelaic acid ammonium salt and 0.005wt% citric acid, and then heated at a voltage of 520V and a current density of 80mA / cm 2 , under the condition of a forming temperature of 85±3°C, the forming time is 5.4 minutes to obtain a medium-treated formed aluminum foil.
[0073] Finishing treatment: the intermediate-treated aluminum foil is placed in an aqueous solution of 0.6 wt % ammonium hydrogen phosphate and 0.1 vol % phosphoric acid, and treated at a temperature of 55-65° C. for 2 minutes to obtain a finish-treated aluminum foil.
[0074] Drying: After taking out the finely treated aluminum foil, dry it at 180°C for 2 minutes to obtain the high-pressure aluminum foil.
[0075] Example 1
[0076] Pretreatment: Take the corroded aluminum foil with a purity of 99.99wt% and conduct ultrasonic treatment at a frequency of 50kHz for 5 minutes in pure water at 50°C;
[0077] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0078] Pretreatment liquid treatment: the boiled aluminum foil is subjected to ultrasonic treatment at an ultrasonic frequency of 50kHz for 6 minutes in a mixed aqueous solution of 0.45wt% ammonium hypophosphite and 0.1wt% ammonium dihydrogen phosphate at 60°C; the aluminum foil treated with the pretreatment liquid is cleaned, and then a subsequent chemical process is carried out to obtain a high-pressure chemically formed aluminum foil.
[0079] Example 2
[0080] Pretreatment: The corroded aluminum foil with a purity of 99.99 wt% was subjected to ultrasonic treatment at a frequency of 50 kHz for 5 minutes in pure water at 50°C;
[0081] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0082] Pretreatment liquid treatment: the boiled aluminum foil is subjected to ultrasonic treatment at an ultrasonic frequency of 50kHz for 6 minutes in a 0.5wt% maleic acid aqueous solution at 60°C; the aluminum foil treated with the pretreatment liquid is cleaned, and then subjected to a subsequent chemical process to obtain a high-pressure chemically formed aluminum foil.
[0083] Comparative Example 1
[0084] Boiling treatment: The corroded aluminum foil with a purity of 99.99 wt% is boiled in pure water at 93° C. for 10 minutes; the boiled aluminum foil is subjected to a subsequent chemical process to obtain a high-pressure chemically formed aluminum foil.
[0085] Comparative Example 2
[0086] Pre-treatment: None;
[0087] Boiling treatment: Take the corroded aluminum foil with a purity of 99.99wt% and boil it in pure water at 93℃ for 10 minutes;
[0088] Pretreatment liquid treatment: the boiled aluminum foil is subjected to ultrasonic treatment at an ultrasonic frequency of 50kHz for 6 minutes in a mixed aqueous solution of 0.45wt% ammonium hypophosphite and 0.1wt% ammonium dihydrogen phosphate at 60°C; the aluminum foil treated with the pretreatment liquid is cleaned, and then a subsequent chemical process is carried out to obtain a high-pressure chemically formed aluminum foil.
[0089] Comparative Example 3
[0090] Pretreatment: Take the corroded aluminum foil with a purity of 99.99wt% and soak it in pure water at 50℃;
[0091] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0092] Pretreatment liquid treatment: the boiled aluminum foil is subjected to ultrasonic treatment at an ultrasonic frequency of 50kHz for 6 minutes in a mixed aqueous solution of 0.45wt% ammonium hypophosphite and 0.1wt% ammonium dihydrogen phosphate at 60°C; the aluminum foil treated with the pretreatment liquid is cleaned, and then a subsequent chemical process is carried out to obtain a high-pressure chemically formed aluminum foil.
[0093] Table 1 Properties of the chemically formed foils obtained in Examples 1 to 2 and Comparative Examples 1 to 3
[0094]
[0095] It can be seen from the experimental results in the table that the use of the present invention significantly reduces the boost time, boost time Tr60 after boiling and leakage current, and improves the specific capacity compared with the prior art chemical foil.
[0096] Test Example 1
[0097] Pretreatment: Take the corroded aluminum foil with a purity of 99.99wt% and put it in pure water at 50℃ and perform ultrasonic treatment at a frequency of 50kHz for 5 minutes; detect the test data of the foil material before and after ultrasonic treatment; Corroded foil specific capacitance: 0.86μF / cm 2 , 520VF specification.
[0098] Weight test: before pure water ultrasonic treatment, the foil was dried at 300°C for 2 minutes, and the specific gravity was 5.243g; after pure water ultrasonic treatment, the foil was dried at 300°C for 2 minutes, and the specific gravity was 5.217g.
[0099] Pretreatment: Take the corroded aluminum foil with a purity of 99.99wt% and soak it in pure water at 50℃; test the test data of the foil material before and after pure water soaking treatment, the specific capacitance of the corroded foil is: 0.86μF / cm 2 , 520VF specification.
[0100] Weight test: before pure water infiltration treatment, the foil was dried at 300℃ for 2min, and the specific gravity was 5.372g; after pure water infiltration treatment, the foil was dried at 300℃ for 2min, and the specific gravity was 5.364g.
[0101] Remove dust, aluminum powder, impurities, etc. from the foil surface, which are factors that affect the performance of the foil and will affect the boost time, specific capacity, and leakage current. Physical tests show that ultrasonic treatment can better remove foreign matter from the foil surface.
[0102] Test Example 2: Ultrasonic treatment time before screening
[0103] Pretreatment: taking corroded aluminum foil with a purity of 99.99wt% and ultrasonically treating it in pure water at a certain temperature for a certain period of time;
[0104] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0105] Pretreatment liquid treatment: the boiled aluminum foil is subjected to ultrasonic treatment at an ultrasonic frequency of 50kHz for 6 minutes in a mixed aqueous solution of 0.5wt% ammonium hypophosphite and 0.1wt% diammonium phosphate at 60°C; the aluminum foil treated with the pretreatment liquid is cleaned, and then a subsequent chemical process is carried out to obtain a high-pressure chemically formed aluminum foil.
[0106] The results are shown in Table 2.
[0107] Table 2 Effect of pretreatment ultrasound time and temperature
[0108]
[0109] As shown in Table 2, considering the pressure rise time Tr and specific volume of the formed foil comprehensively, the ultrasonic time is controlled to be 3 to 6 minutes and the ultrasonic temperature is controlled to be 45 to 60°C.
[0110] Test Example 3
[0111] Pretreatment: Take the corroded aluminum foil with a purity of 99.99wt% and soak it in pure water at 50℃;
[0112] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0113] Pretreatment liquid treatment: the aluminum foil after boiling in water is immersed in the pretreatment liquid (without ultrasound), or subjected to ultrasound treatment at an ultrasonic frequency of 50 kHz (with ultrasound); the aluminum foil treated with the pretreatment liquid is cleaned, and then subjected to a subsequent chemical process to obtain a high-pressure chemically formed aluminum foil.
[0114] The specific parameters of the pretreatment liquid treatment steps and the properties of the formed foil are shown in Table 3.
[0115] Table 3 Effect of ultrasonic treatment on pretreatment liquid
[0116]
[0117] As shown in Table 3, the ultrasonic treatment in the pretreatment liquid treatment can significantly affect the pressure rise time and leakage current after boiling, especially the ultrasonic treatment can significantly reduce the pressure rise time after boiling.
[0118] Test Example 4
[0119] Pretreatment: The corroded aluminum foil with a purity of 99.99 wt% was subjected to ultrasonic treatment at a frequency of 50 kHz for 5 minutes in pure water at 50°C;
[0120] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0121] Pretreatment liquid treatment: the aluminum foil after boiling in water is immersed in the pretreatment liquid (without ultrasound), or subjected to ultrasound treatment at an ultrasonic frequency of 50 kHz (with ultrasound); the aluminum foil treated with the pretreatment liquid is cleaned, and then subjected to a subsequent chemical process to obtain a high-pressure chemically formed aluminum foil.
[0122] The specific parameters of the pretreatment liquid treatment step and the properties of the formed foil are shown in Table 4.
[0123] Table 4 Effect of ultrasonic treatment on pretreatment liquid
[0124]
[0125] It can be seen from Tables 3 and 4 that the leakage current and the pressure rise time after boiling can be further reduced by ultrasonic treatment and pretreatment liquid treatment in the pretreatment.
[0126] Test Example 5: Screening of pretreatment solution
[0127] Pretreatment: The corroded aluminum foil with a purity of 99.99 wt% was subjected to ultrasonic treatment at a frequency of 50 kHz for 5 minutes in pure water at 50°C;
[0128] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0129] Pretreatment liquid treatment: the boiled aluminum foil is subjected to ultrasonic treatment at a frequency of 50kHz for 6 minutes in a pretreatment liquid at 60°C, wherein the pretreatment liquid is a mixed aqueous solution of ammonium hypophosphite and ammonium dihydrogen phosphate with a mass concentration of 5:1; the aluminum foil treated with the pretreatment liquid is washed, and then a subsequent chemical process is carried out to obtain a high-pressure chemically formed aluminum foil.
[0130] The concentration of the pretreatment solution and the corresponding properties of the formed aluminum foil are shown in Table 5.
[0131] Table 5 Effect of pretreatment solution concentration
[0132]
[0133] A pretreatment solution with a concentration of 0.6 wt % was used. The mass concentration ratio of ammonium hypophosphite and ammonium dihydrogen phosphate in the pretreatment solution and the corresponding properties of the formed aluminum foil are shown in Table 6.
[0134] Table 6 Effect of the ratio of ammonium phosphite and diammonium phosphate
[0135]
[0136] It can be seen from Tables 5 and 6 that the concentration of the pretreatment solution and the ratio of hypophosphorous acid to phosphoric acid also affect the performance of the electrode foil. Their total concentration must be in the range of 0.4 to 3wt%, with hypophosphorous acid accounting for more than 80% to meet the requirements.
[0137] Test Example 7: Screening of ultrasonic treatment time and temperature of pretreatment liquid
[0138] Pretreatment: The corroded aluminum foil with a purity of 99.99 wt% was subjected to ultrasonic treatment at a frequency of 50 kHz for 5 minutes in pure water at 50°C;
[0139] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0140] Pretreatment liquid treatment: the aluminum foil after boiling in water is subjected to ultrasonic treatment at an ultrasonic frequency of 50kHz in a pretreatment liquid at 60°C, wherein the pretreatment liquid is a mixed aqueous solution of 0.5wt% ammonium hypophosphite and 0.1wt% diammonium phosphate; the aluminum foil treated with the pretreatment liquid is washed, and then a subsequent chemical process is carried out to obtain a high-pressure chemically formed aluminum foil.
[0141] The results are shown in Table 7.
[0142] Table 7 Effect of ultrasonic treatment time on pretreatment liquid
[0143]
[0144] It can be seen from Table 7 that, considering the forming foil boost time Tr, leakage current, specific volume enhancement effect and hydration boost time TR60 comprehensively, the ultrasonic time is controlled to be 3 to 10 minutes, and 5 to 8 minutes has the best effect.
[0145] Pretreatment: The corroded aluminum foil with a purity of 99.99 wt% was subjected to ultrasonic treatment at a frequency of 50 kHz for 5 minutes in pure water at 50°C;
[0146] Boiling treatment: Boil the pre-treated aluminum foil in pure water at 93°C for 10 minutes;
[0147] Pretreatment liquid treatment: the boiled aluminum foil is subjected to ultrasonic treatment at a certain temperature in a pretreatment liquid with an ultrasonic frequency of 50kHz for 6 minutes, and the pretreatment liquid is a mixed aqueous solution of 0.5wt% ammonium hypophosphite and 0.1wt% diammonium phosphate; the aluminum foil treated with the pretreatment liquid is washed, and then a subsequent chemical process is carried out to obtain a high-pressure chemically formed aluminum foil.
[0148] The results are shown in Table 8.
[0149] Table 8 Effect of ultrasonic temperature on pretreatment liquid treatment
[0150]
[0151]
[0152] It can be seen from Table 8 that the increase in pretreatment temperature is extremely beneficial to the formation foil boost time Tr, leakage current, specific volume increase and hydration boost time TR60. At the same time, due to the existence of ultrasonic treatment, when the pretreatment temperature is lowered to 50°C, the boost time Tr, leakage current, specific volume increase and hydration boost time TR60 can also be improved. Considering the electrode foil performance and energy consumption cost, the present invention controls the pretreatment ultrasonic temperature to 50-85°C, and 55-65°C has the best effect.
[0153] In summary, the present invention improves the leakage current performance and the boost time after boiling in order to improve the comprehensive performance of the formed foil while ensuring other properties of the high-voltage formed foil, optimizes the pretreatment process, and screens a large number of pretreatment means, ultrasonic temperature and time, pretreatment liquid and ultrasonic time in the pretreatment process, etc., which not only achieves an increase in specific volume, but also reduces the leakage current, boost time and boost time after boiling in order to significantly improve the comprehensive performance of the high-voltage electrode foil. The method of the present invention is not only applicable to high-voltage formed foil, but also to medium-voltage formed foil.
Claims
1. A medium and high voltage electrode foil pretreatment method for increasing specific capacity, reducing boost time and leakage current, characterized in that: The following steps are involved: A. Pretreatment: Place the corroded foil in water for ultrasonic treatment; B. Boiling treatment: Boil the corroded foil after pre-treatment in water; C. Pretreatment liquid treatment: the boiled corroded foil is placed in the pretreatment liquid for ultrasonic treatment, and then cleaned to obtain the pretreated foil; Wherein, in step A, the temperature of the ultrasonic treatment is 45-60°C, the frequency is 30-100kHz, and the time is 3-6min; In step C, the pretreatment liquid is an aqueous solution of hypophosphorous acids and their salts and phosphoric acids and their ammonium salts, the total concentration of the hypophosphorous acids and their salts and phosphoric acids and their ammonium salts is 0.4-3wt%, and the mass concentration ratio of the hypophosphorous acids and their salts to the phosphoric acids and their ammonium salts is 4-9:1; or the pretreatment liquid is an aqueous solution of olefin polycarboxylic acids and their ammonium salts, and the concentration of the olefin polycarboxylic acids and their ammonium salts is 0.5-3wt%; In step C, the temperature of the ultrasonic treatment is 50-85° C., the frequency is 30-100 kHz, and the ultrasonic time is 3-10 minutes.
2. The method for pretreating medium and high voltage electrode foil according to claim 1, characterized in that: In step A, the temperature of the ultrasonic treatment is 50-55° C., the frequency is 50 kHz, and the time is 4-5 min.
3. The method for pretreating medium and high voltage electrode foil according to claim 1, characterized in that: In step A, the corroded foil is corroded aluminum foil with a purity of 99.99 wt %.
4. The method for pretreating medium and high voltage electrode foil according to claim 1, characterized in that: In step B, the boiling temperature is 85-100° C. and the boiling time is 3-20 minutes.
5. The method for pretreating medium and high voltage electrode foil according to claim 1, characterized in that: In step C, the hypophosphorous acids and their salts are at least one of hypophosphorous acid, sodium hypophosphite, potassium hypophosphite or ammonium hypophosphite, and the phosphoric acids and their ammonium salts are at least one of phosphoric acid, ammonium hydrogen phosphate or diammonium phosphate; preferably, the hypophosphorous acids and their salts are ammonium hypophosphite, and the phosphoric acids and their ammonium salts are diammonium phosphate.
6. The method for pretreating medium and high voltage electrode foil according to claim 1, characterized in that: In step C, the total concentration of the hypophosphorous acids and their salts and the phosphoric acids and their ammonium salts is 0.5-0.6 wt %, and the mass concentration ratio of the hypophosphorous acids and their salts to the phosphoric acids and their ammonium salts is 5-7:
1.
7. The method for pretreating medium and high voltage electrode foil according to claim 1, characterized in that: In step C, the olefin polycarboxylic acid and its ammonium salt are at least one of maleic acid, fumaric acid or ammonium hydrogen maleate; preferably, the olefin polycarboxylic acid and its ammonium salt are maleic acid.
8. The method for pretreating medium and high voltage electrode foil according to claim 1, characterized in that: In step C, the temperature of the ultrasonic treatment is 55-65° C., the frequency is 50 kHz, and the ultrasonic time is 5-8 minutes.
9. The method for pretreating medium and high voltage electrode foil according to any one of claims 1 to 8, characterized in that: In step C, a drying operation is further performed after cleaning, and the drying temperature is 60 to 200° C. and the drying time is 1 to 10 minutes.
Citation Information
Cited By
Formed foil and preparation method thereof
CN120878466A
Amide-aluminum sulfate hydrated eutectic electrolyte for hydration treatment of high-voltage electrode foil and application of amide-aluminum sulfate hydrated eutectic electrolyte
CN121575462A