Method for growing continuous organic single crystal by polymer-assisted two-phase dip-coating and application

Through the polymer-assisted biphase impregnation and lifting method, the hydrogen bond interaction between polyvinyl alcohol and organic semiconductors is used to induce the formation of a small number of crystal nuclei and promote the adhesion of semiconductor molecules, which solves the high nucleation density and growth in traditional single-phase impregnation and lifting. The problem of discontinuity has achieved high-quality organic single crystal growth and improved performance of organic field effect transistor devices.

CN118957730APending Publication Date: 2024-11-15SICHUAN INNOVATION RES INST OF TIANJIN UNIV +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411100146.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

There is random homogeneous nucleation in the traditional single-phase impregnation and lifting technology, with high nucleation density, making it difficult to obtain large-area single crystal domains, and it is difficult to form crystal nuclei and achieve continuous growth at low concentrations.

Method used

Using polymer-assisted biphasic impregnation and lifting method, polyvinyl alcohol aqueous solution is used as the base phase, combined with low-concentration organic semiconductor solution, the substrate is immersed vertically at room temperature and pulled from the biphasic solution, and polyvinyl alcohol is used with The hydrogen bond interaction between semiconductors induces the formation of a small number of crystal nuclei, and promotes the adhesion of semiconductor molecules on the substrate through sticky polyvinyl alcohol, achieving continuous growth.

Benefits of technology

It effectively avoids the problems of polycrystalline accumulation and growth discontinuity caused by high concentration homogeneous nucleation, reduces the nucleation barrier, realizes low-density heteronucleation, promotes high-quality continuous growth of organic single crystals, and Improves the mobility of organic field effect transistor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957730A_ABST
    Figure CN118957730A_ABST
Patent Text Reader

Abstract

The invention discloses a method for growing a continuous organic single crystal by polymer-assisted double-phase dip-coating and application, and the method comprises the following steps: at room temperature, vertically immersing a clean substrate into a double-phase solution, when the substrate is completely immersed into the double-phase solution, vertically moving the substrate out of a dip-coating solution at a speed of 5-20 [mu] m / s, and when the substrate is completely pulled out of the dip-coating solution, taking out the substrate from the dip-coating solution; the lower layer of the biphase solution is a polyvinyl alcohol aqueous solution, the upper layer of the biphase solution is an organic semiconductor solution, the upper layer of the biphase solution and the lower layer of the biphase solution are immiscible, the concentration of polyvinyl alcohol is 0.1-10 mg / mL, and the concentration of the organic semiconductor is 0.1-1 mg / mL. According to the method, negative effects caused by high-concentration homogeneous nucleation in traditional single-phase dip-coating are successfully avoided, adhesion of semiconductor molecules on a substrate is facilitated due to introduction of PVA, fluid instability and mass transfer disorder are reduced, and high-quality continuous growth of organic single crystals is effectively promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic semiconductors, and in particular to a method and application of polymer-assisted two-phase immersion pulling growth of continuous organic single crystals. Background Art

[0002] Organic semiconductors have the advantages of molecular diversity, low-cost large-area preparation, low-temperature solution processing, and inherent compatibility with flexible substrates, and have attracted widespread attention from academia and industry. Among them, organic single crystals are a new type of functional materials. Due to their advantages such as long-range order, no grain boundaries, low defect density, and long exciton lifetime, they are an ideal platform for exploring the basic physical properties of materials and realizing functional applications. In order to prepare continuous high-quality organic semiconductor single crystal films, people have studied and developed a variety of solution processing methods. The immersion pulling technology has a high tolerance for the material type and shape of the substrate, simple equipment, and can be quickly prepared on a large scale, so it is widely used. In order to achieve the matching of the solution retreat rate and the evaporation rate, the traditional single-phase immersion pulling technology requires a high solution concentration, which inevitably has random homogeneous nucleation and high nucleation density. It is difficult to obtain large-area single crystal domains. At low concentrations, it is difficult to form nuclei and achieve continuous growth. At the same time, the film morphology is extremely sensitive to the environment such as fluid flow, temperature, substrate surface, and pulling speed. Summary of the invention

[0003] The purpose of the present invention is to provide a method and application of polymer-assisted two-phase impregnation pulling to grow continuous organic single crystals, so as to solve the technical problems in the prior art of single-phase impregnation pulling, such as random homogeneous nucleation, high nucleation density, difficulty in obtaining large-area single crystal domains, and difficulty in forming crystal nuclei and achieving continuous growth at low concentrations.

[0004] To achieve the above object, the present invention provides the following technical solutions: The present invention provides a method for growing continuous organic single crystals by polymer-assisted two-phase immersion pulling, comprising the following steps: vertically immersing a clean substrate into a two-phase solution at room temperature, and when the substrate is completely immersed in the two-phase solution, vertically removing the substrate from the pulling solution at a speed of 5-20 μm / s, and when the substrate is completely pulled out, continuously growing organic single crystals are obtained on the substrate, the lower layer of the two-phase solution is a polyvinyl alcohol aqueous solution, and the upper layer is an organic semiconductor solution, the upper and lower layers of the solution are immiscible, the concentration of the polyvinyl alcohol is 0.1-10 mg / mL, and the concentration of the organic semiconductor is 0.1-1 mg / mL.

[0005] Furthermore, the crystal growth temperature is 25°C.

[0006] Furthermore, the substrate is a silicon wafer, and the substrate is cleaned by the following steps: first, the substrate is placed in deionized water and ultrasonically treated at 40% power for 15 minutes, then placed in acetone and ultrasonically treated at 40% power for 15 minutes, then placed in isopropanol and ultrasonically treated at 40% power for 15 minutes, and finally, the substrate is blown dry with nitrogen or inert gas.

[0007] Furthermore, the polyvinyl alcohol is of 0588 low-viscosity type, and the alcoholysis degree is 87.0-89.0 mol / mol.

[0008] Furthermore, the water in the polyvinyl alcohol aqueous solution is ultrapure water with an electrical conductivity of 18.2 MΩ cm -1 The organic semiconductor in the organic semiconductor solution is C6-DPA or TIPS-PEN, and the solvent in the organic semiconductor solution is chlorobenzene.

[0009] Furthermore, the volume of the lower layer polyvinyl alcohol aqueous solution is 10 mL, and the volume of the upper layer organic semiconductor solution is 30 μL.

[0010] Furthermore, the biphasic solution is contained in a clean glass container, and the glass container is cleaned by the following steps: first, an alkaline solution is used to remove surface dust and oil stains, then it is washed with clean water, and then it is immersed in anhydrous ethanol and ultrasonically immersed for 30 minutes, and then it is placed in deionized water and soaked for 10 minutes, and finally it is placed in an oven at 65°C for drying.

[0011] The present invention also provides an application of the method for growing continuous organic single crystals by polymer-assisted dual-phase immersion pulling in the preparation of organic single crystals or organic single crystal films.

[0012] Furthermore, the thickness of the organic single crystal film is 10-20 nm.

[0013] The present invention also provides an application of an organic single crystal or an organic single crystal film prepared by a method for growing continuous organic single crystals by polymer-assisted two-phase immersion pulling in an organic field effect transistor device.

[0014] Furthermore, the average mobility of the organic field effect transistor device is 1.47 cm 2 / (Vs), the maximum mobility of the organic field effect transistor device is 2.1cm 2 / (Vs).

[0015] Based on the above technical solution, the embodiments of the present invention can at least produce the following technical effects: The present invention uses polyvinyl alcohol (PVA) aqueous solution as the bottom phase. Due to the presence of a large number of hydroxyl groups on PVA, hydrogen bonds can be generated between the PVA and the semiconductor. In a low-concentration semiconductor solution, a small amount of crystal nuclei can be induced to form on the curved liquid surface, thereby avoiding the random high-density homogeneous nucleation and subsequent polymorphic accumulation caused by the high-concentration solution in the single-phase immersion pulling method. At the same time, during the pulling process, the viscous polyvinyl alcohol (PVA) will be uniformly attached to the substrate, promoting the attachment of semiconductor molecules at the front of the curved liquid surface to the viscous substrate, thereby reducing the negative effects caused by fluid instability and mass transfer disorder, and then inducing the molecules to grow into continuous organic single crystals on the substrate surface.

[0016] The use of polyvinyl alcohol (PVA) aqueous solution as the bottom phase solution successfully circumvents the negative effects of polymorphic stacking and discontinuous growth caused by high-concentration homogeneous nucleation in traditional single-phase immersion pulling. The introduction of PVA effectively reduces the nucleation barrier, allowing low-density heterogeneous nucleation to be achieved in low-concentration solutions. At the same time, the introduction of PVA helps the adhesion of semiconductor molecules to the substrate, reduces fluid instability and mass transfer disorder, and effectively promotes the high-quality continuous growth of organic single crystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0018] Figure 1 Schematic diagram of single-phase impregnation pulling and dual-phase impregnation pulling; Figure 2 Schematic diagram of the working principle of polyvinyl alcohol (PVA) in two-phase immersion pulling; Figure 3 Microscope images of C6-DPA crystals obtained by dual-phase immersion pulling with polyvinyl alcohol (PVA) aqueous solutions of different concentrations; Figure 3 Middle: a3 is the morphology of Example 1, where the experimental conditions are that no polyvinyl alcohol (PVA) is added, the pulling speed is 10 μm / s, and the concentration of C6-DPA solution is 0.1 mg / mL, and b3 and c3 are the corresponding polarizing microscope images; Figure 3 In the figure: d3 is the morphology of Example 2, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.01 mg / mL, a pulling speed of 10 μm / s, and a C6-DPA solution concentration of 0.1 mg / mL, and e3 and f3 are the corresponding polarizing microscope images; Figure 3 In the figure: g3 is the morphology of Example 3, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.1 mg / mL, a pulling speed of 10 μm / s, and a C6-DPA solution concentration of 0.1 mg / mL, and h3 and i3 are the corresponding polarizing microscope images; Figure 3 In: j3 is the morphology of Example 4, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 1.0 mg / mL, a pulling speed of 10 μm / s, and a C6-DPA solution concentration of 0.1 mg / mL, and k3 and l3 are the corresponding polarizing microscope images; Figure 4 Microscope images of C6-DPA crystal morphology at different pulling speeds; Figure 4 Middle: a4, b4, c4 are morphological images of Examples 5, 1, and 6, respectively, where the experimental conditions are that no polyvinyl alcohol (PVA) is added, the concentration of C6-DPA solution is 0.1 mg / mL, and the pulling speeds are 5 μm / s, 10 μm / s, and 30 μm / s, respectively; Figure 4 Middle: d4, e4, f4 are morphological images of Examples 7, 4, and 8, respectively. The experimental conditions are that the concentration of polyvinyl alcohol (PVA) is 1.0 mg / mL, the concentration of C6-DPA solution is 0.1 mg / mL, and the pulling speeds are 5 μm / s, 10 μm / s, and 30 μm / s, respectively; Figure 5 Low-magnification microscope images of C6-DPA crystals obtained by pulling with and without the addition of polyvinyl alcohol (PVA); Figure 6 The microscope images of TIPS-PEN crystals obtained by two-phase immersion pulling with polyvinyl alcohol (PVA) aqueous solutions of different concentrations; a6 is a morphology image of Example 9, where the experimental conditions are no polyvinyl alcohol (PVA) added, the pulling speed is 10 μm / s, and the concentration of TIPS-PEN solution is 1.0 mg / mL; b6 and c6 are the corresponding polarizing microscope images; d6 is a morphology image of Example 10, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.01 mg / mL, a pulling speed of 10 μm / s, and a TIPS-PEN solution concentration of 1.0 mg / mL, and e6 and f6 are corresponding polarizing microscope images; g6 is a morphology image of Example 11, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.1 mg / mL, a pulling speed of 10 μm / s, and a TIPS-PEN solution concentration of 1.0 mg / mL. h6 and i6 are corresponding polarizing microscope images; j6 is a morphology image of Example 12, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 1.0 mg / mL, a pulling speed of 10 μm / s, and a TIPS-PEN solution concentration of 1.0 mg / mL, and k6 and l6 are corresponding polarizing microscope images; Figure 7 Microscope images of TIPS-PEN crystals at different pulling speeds; Figure 7 In the middle: a7, b7, c7 are examples 13, 9, and 14, respectively, and are morphology images under the experimental conditions of no addition of polyvinyl alcohol (PVA), a TIPS-PEN solution concentration of 1.0 mg / mL, and a pulling speed of 5 μm / s, 10 μm / s, and 30 μm / s, respectively; Figure 7 In the middle: d7, e7, f7 are the morphology images of Examples 14, 12, and 16, respectively, where the experimental conditions are that the concentration of polyvinyl alcohol (PVA) is 1.0 mg / mL, the concentration of TIPS-PEN solution is 1.0 mg / mL, and the pulling speeds are 5 μm / s, 10 μm / s, and 30 μm / s, respectively; Figure 8 Microscope image of polyvinyl alcohol (PVA)-induced crystal nucleation in semiconductor solution; Fig. 9 Atomic force microscopy image of single crystal grown by polyvinyl alcohol (PVA) assisted dual-phase immersion pulling; Fig. 9 Middle: a9 and b9 are atomic force microscope images of Example 4 and Example 12 respectively; Fig.10 This is the XRD test diagram of the single crystal grown by polyvinyl alcohol (PVA) assisted dual-phase immersion pulling; Fig.10 Middle: a10 and b10 are XRD spectra of Example 4 and Example 12 respectively; Fig.11 This is the transfer curve diagram measured based on Keithley 4200 in the device performance test; Fig.12 This is the output curve graph measured based on Keithley 4200 in the device performance test; Fig.13 Mobility diagram for device testing. DETAILED DESCRIPTION

[0019] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0020] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0021] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0022] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0023] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0024] The sources of drug purchase in the following embodiments are as follows: 2,6-Bis(4-hexylphenyl)anthracene (C6-DPA), purity>99%, purchased from: TCI Chemicals Co., Ltd.

[0025] 6,13-Bis(triisopropylsilylethynyl)pentacene (TIPS-PEN), purity>99%, purchased from: Sigma-Aldrich

[0026] Polyvinyl alcohol 0588 low viscosity type (PVA-205), alcoholysis degree: 87.0~89.0 (mol / mol), purchased from: Macklin

[0027] Chlorobenzene, purity: >99%, purchased from: Sigma-Aldrich Acetone, purity: analytical grade, purchased from: Tianjin Jiangtian Chemical Co., Ltd. Isopropanol, purity: analytical grade, purchased from: Tianjin Komiou Chemical Reagent Co., Ltd. Ultrapure water, conductivity: 18.2 MΩ cm -1 , Tianjin University Assets Silicon wafer, N-type phosphorus doped, with 300 nm SiO2 loaded on the silicon wafer, purchased from: China Electronics Technology Group Corporation 46th Research Institute The main test equipment in the embodiment is as follows: Polarizing microscope, model: Nikon OptiPlex 3046, origin: Japan Atomic force microscope, model: Dimension Icon, origin: Beijing, China X-ray diffractometer, model: PANalytical / Empyrean, origin: Netherlands Probe station, model: Keithley 4200, origin: Beijing, China Constant temperature immersion coating machine, model: SYDC-100H, origin: Shanghai, China CNC ultrasonic cleaner, model: KQ5200DE, origin: Kunshan, China Electric heating blast drying oven, model: DH-101, origin: Tianjin, China The silicon wafers and glass containers used in the following examples were cleaned before use. The steps for cleaning the silicon wafers were as follows: first, the silicon wafers were placed in deionized water and ultrasonically treated at 40% power for 15 min, then placed in acetone and ultrasonically treated at 40% power for 15 min, then placed in isopropanol and ultrasonically treated at 40% power for 15 min, and finally dried with nitrogen or inert gas. The steps for cleaning the glass container were as follows: first, an alkaline solution was used to remove surface dust and oil stains, then the glass container was cleaned with clean water, then the glass container was immersed in anhydrous ethanol and ultrasonically treated for 30 min, then the glass container was placed in deionized water and soaked for 10 min, and finally dried in an oven at 65°C.

[0028] Examples 1 to 8 Configuration concentration ( C ) was a 0.1 mg / mL C6-DPA chlorobenzene solution, which was fully dissolved by ultrasonication at 100% power for 30 min at room temperature.

[0029] Configure the concentration ( C ) in aqueous polyvinyl alcohol (PVA) solutions of 0 mg / mL, 0.01 mg / mL, 0.1 mg / mL, and 1.0 mg / mL were fully dissolved by ultrasonication at 100% power for 60 min at room temperature.

[0030] The ambient temperature of the constant temperature immersion coating machine chamber is regulated to 25±1℃ and the humidity is 45±3%.

[0031] Use a pipette to take 10 mL of C 0 (0mg / mL, 0.01mg / mL, 0.1mg / mL, 1.0mg / mL) of polyvinyl alcohol (PVA) aqueous solution was placed in a glass container, and then 30 mL of C6-DPA solution was dripped onto the surface of the polyvinyl alcohol (PVA) aqueous solution with a pipette to form a two-phase solution. The weighing bottle containing the two-phase solution was placed in a lifting machine and allowed to stand. The silicon wafer was clamped with tweezers and placed on the retractable cantilever in the lifting machine. The stepper motor was controlled to immerse the silicon wafer vertically in the two-phase solution. When the silicon wafer was completely immersed in the lifting solution, the silicon wafer was pulled with a v The sample was moved vertically out of the pulling solution at a speed of 1 μm / s.

[0032] C 0 and v 1As shown in Table 1.

[0033] Table 1

[0034] Examples 9-16 verify the universality of the invention for other semiconductor molecules.

[0035] Configuration concentration ( C ) was a 1.0 mg / mL TIPS-PEN chlorobenzene solution, which was fully dissolved by ultrasonication at 100% power for 30 min at room temperature.

[0036] Configure the concentration ( C ) in aqueous polyvinyl alcohol (PVA) solutions of 0 mg / mL, 0.01 mg / mL, 0.1 mg / mL, and 1.0 mg / mL were fully dissolved by ultrasonication at 100% power for 60 min at room temperature.

[0037] The ambient temperature of the constant temperature immersion coating machine chamber is regulated to 25±1℃ and the humidity is 45±3%.

[0038] Use a pipette to take 10 mL of C 0 (0 mg / mL, 0.01 mg / mL, 0.1 mg / mL, 1.0 mg / mL) of polyvinyl alcohol (PVA) aqueous solution was placed in a glass container, and then 30 μL of TIPS-PEN solution was dripped onto the surface of the polyvinyl alcohol (PVA) aqueous solution with a pipette to form a two-phase solution. The weighing bottle containing the two-phase solution was placed in a puller and allowed to stand. The silicon wafer was clamped with tweezers and placed on the retractable cantilever in the puller. The stepper motor was controlled to immerse the silicon wafer vertically in the two-phase solution. When the silicon wafer was completely immersed in the pull solution, the silicon wafer was pulled with a vThe sample was moved vertically out of the pulling solution at a speed of 1 μm / s.

[0039] C 0 and v 1As shown in Table 2.

[0040] Table 2

[0041] Figure 1 This is a schematic diagram of single-phase immersion pulling and two-phase immersion pulling. Single-phase refers to only organic semiconductor solution phase, and two-phase refers to water phase and organic semiconductor solution phase, which are immiscible with each other. The water phase is in the lower layer and the organic phase is in the upper layer.

[0042] Figure 2 This is a schematic diagram of the working principle of polyvinyl alcohol (PVA) in two-phase immersion pulling. Due to the presence of a large number of hydroxyl groups on PVA, hydrogen bonding interactions can occur between PVA and semiconductors. In a low-concentration semiconductor solution, a small amount of crystal nuclei can be induced to form. At the same time, during the pulling process, the viscous polyvinyl alcohol (PVA) will adhere to the substrate evenly, prompting the semiconductor molecules at the front of the curved liquid surface to adhere to the viscous substrate, thereby reducing the negative impact of fluid instability and mass transfer disorder.

[0043] Figure 3 In the figure: a3 is a morphology image of Example 1, where the experimental conditions are that no polyvinyl alcohol (PVA) is added, the pulling speed is 10 μm / s, and the concentration of C6-DPA solution is 0.1 mg / mL; b3 and c3 are corresponding polarizing microscope images; the image shows a discontinuous and scattered organic film.

[0044] Figure 3 In the figure: d3 is the morphology of Example 2, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.01 mg / mL, a pulling speed of 10 μm / s, and a C6-DPA solution concentration of 0.1 mg / mL; e3 and f3 are corresponding polarizing microscope images; the figure shows neat stripes.

[0045] Figure 3 In the figure: g3 is the morphology of Example 3, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.1 mg / mL, a pulling speed of 10 μm / s, and a C6-DPA solution concentration of 0.1 mg / mL; h3 and i3 are the corresponding polarizing microscope images; the figure shows a continuous large-area film with a small amount of grain boundaries.

[0046] Figure 3In the figure: j3 is the morphology of Example 4, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 1.0 mg / mL, a pulling speed of 10 μm / s, and a C6-DPA solution concentration of 0.1 mg / mL; k3 and l3 are corresponding polarizing microscope images; the figure shows a continuous large-area single crystal with no grain boundaries.

[0047] Figure 4 Middle: a4, b4, c4 are morphological images of Examples 5, 1, and 6, respectively, where the experimental conditions are that no polyvinyl alcohol (PVA) is added, the concentration of C6-DPA solution is 0.1 mg / mL, and the pulling speeds are 5 μm / s, 10 μm / s, and 30 μm / s, respectively; Figure 4 In the middle: d4, e4, f4 are morphology pictures of Examples 7, 4, and 8, respectively. The experimental conditions are that the concentration of polyvinyl alcohol (PVA) is 1.0 mg / mL, the concentration of C6-DPA solution is 0.1 mg / mL, and the pulling speeds are 5 μm / s, 10 μm / s, and 30 μm / s, respectively.

[0048] Figure 5 The microscope images of Example 4 and Example 1 under low magnification. In Example 4, a uniform and continuous crystal film was observed in the range of >1*1cm, and in Example 1, a uniform and continuous crystal film was observed in the range of >1*1cm. 2 The range shows a non-uniform and discontinuous crystal film.

[0049] Figure 6 Middle: a6 is a morphology image of Example 9, where the experimental conditions are that no polyvinyl alcohol (PVA) is added, the pulling speed is 10 μm / s, and the concentration of the TIPS-PEN solution is 1.0 mg / mL; b6 and c6 are corresponding polarizing microscope images, which show scattered black spherulites; d6 is a morphology image of Example 10, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.01 mg / mL, a pulling speed of 10 μm / s, and a TIPS-PEN solution concentration of 1.0 mg / mL. e6 and f6 are corresponding polarizing microscope images, which show stripes, but with branches and discontinuity. g6 is a morphology image of Example 11, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 0.1 mg / mL, a pulling speed of 10 μm / s, and a TIPS-PEN solution concentration of 1.0 mg / mL. h6 and i6 are corresponding polarizing microscope images, which are displayed as continuous strips. j6 is the morphology of Example 12, where the experimental conditions are a polyvinyl alcohol (PVA) concentration of 1.0 mg / mL, a pulling speed of 10 μm / s, and a TIPS-PEN solution concentration of 1.0 mg / mL. k6 and l6 are corresponding polarizing microscope images, which appear as continuous dense strips.

[0050] Figure 7 In the middle: a7, b7, c7 are examples 13, 9, and 14, respectively, and are morphology images under the experimental conditions of no addition of polyvinyl alcohol (PVA), a TIPS-PEN solution concentration of 1.0 mg / mL, and a pulling speed of 5 μm / s, 10 μm / s, and 30 μm / s, respectively. No crystals appear in a7, b7, and c7; Figure 7 In the figure: d7, e7, f7 are morphology images of Examples 14, 12, and 16, respectively. The experimental conditions are that the concentration of polyvinyl alcohol (PVA) is 1.0 mg / mL, the concentration of TIPS-PEN solution is 1.0 mg / mL, and the pulling speeds are 5 μm / s, 10 μm / s, and 30 μm / s, respectively; Figures d7 and e7 are both dense, continuous, and uniformly oriented single crystal strips, and Figure 7f is a loose, discontinuous strip with branches.

[0051] From the above results, it can be seen that when polyvinyl alcohol (PVA) is not added to the aqueous phase, it is difficult to reach the supersaturation point when pulling to the solid-liquid-gas three-phase junction under the condition of low semiconductor solution concentration. Especially when the pulling speed is increased, most of the solute in the solution will return to the solution along with the solution, and discontinuous crystals or even spherulites often appear on the substrate after pulling. When polyvinyl alcohol (PVA) is added to the aqueous phase, the addition of PVA will induce the organic phase and the polymer solution phase to produce crystal nuclei. At the moment of substrate insertion, the crystal nuclei adhere to the substrate, and the entanglement of polymer chains leads to strong interchain forces, which is conducive to stable solute transport and is conducive to crystallization. And under high-speed pulling, good crystal morphology can still be obtained. In addition, due to the low concentration of the semiconductor solution, random homogeneous nucleation will not occur, avoiding the accumulation of polymorphs.

[0052] Figure 8 This is a microscope image of polyvinyl alcohol (PVA) inducing the formation of crystal nuclei in semiconductor solutions. From the real-time microscope observation image, it can be seen that tiny crystal nuclei are observed 10 seconds after the semiconductor solution is dropped on the water phase with PVA added, and they grow as time goes by. When the semiconductor solution is dropped on the water phase without PVA added, crystal nuclei appear only after the solution evaporates for 6 minutes.

[0053] Fig. 9 a9 and b9 are the atomic force microscope images of Example 4 and Example 12, respectively, scanning 50*50 μm 2In the range of , Example 4 shows a large area of ​​uniform thickness, the thickness is 11.1 nm, corresponding to 4 molecular layers, R q Example 12 shows a uniform strip thickness of 19.7 nm, corresponding to 12 molecular layers, R q The thickness of the nanostructured carbon fiber is 0.27 nm, showing atomic-level flatness, which is crucial for preparing high-quality optoelectronic devices.

[0054] Fig.10 a10 and b10 are the XRD spectra of Example 4 and Example 12, respectively. The XRD spectrum of Example 4 has a flat baseline, and sharp diffraction peaks appear at 2θ=2.7° and 13.7°, which is consistent with the peak position of C6-DPA single crystal reported in the previous literature. The calculated interplanar spacing is 3.2 nm. The XRD spectrum of Example 12 also has a flat baseline, and sharp diffraction peaks are measured at 2θ=5.41°, 10.74° and 16.10°, corresponding to the (001), (002) and (003) crystal planes of TIPS-PEN, respectively. The interplanar spacing of TIPS-PEN calculated by the Bragg equation is 1.63 nm, which is consistent with the c-axis in its crystal data. XRD characterization further proves that the C6-DPA and TIPS-PEN single crystals grown by dual-phase immersion pulling assisted by polyvinyl alcohol (PVA) have excellent crystallinity.

[0055] Figure 11-13 For device performance testing, a pair of gold films prepared in advance were picked up with a probe and attached in parallel to the C6-DPA organic single crystal film prepared in Example 4 to prepare an organic field effect transistor device, such as Fig.11 As shown in Figure 1, the ratio of the channel distance (L) to the channel width (W) is 3:4. The transfer curve and output curve measured by Keithley 4200 are shown in Figures 11 and 12. The mobility extracted from the transfer curve is 2.1 cm 2 / (Vs), the on / off ratio is 10 6 . 15 devices were counted, such as Fig.13 As shown, the average migration rate is 1.57 cm 2 / (Vs), showing a higher mobility, which further indicates the high quality of organic single crystals grown by polymer-assisted dual-phase immersion pulling.

[0056] Finally, it should be noted that: The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may still be modified, or some or all of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for growing continuous organic single crystals by polymer-assisted dual-phase impregnation and pulling, characterized in that: The method comprises the following steps: vertically immersing a clean substrate into a two-phase solution at room temperature; when the substrate is completely immersed in the two-phase solution, vertically moving the substrate out of the pulling solution at a speed of 5-20 μm / s; when the substrate is completely pulled out, continuously growing organic single crystals on the substrate; the lower layer of the two-phase solution is a polyvinyl alcohol aqueous solution, and the upper layer is an organic semiconductor solution; the upper and lower layers of the solution are immiscible; the concentration of the polyvinyl alcohol is 0.1-10 mg / mL, and the concentration of the organic semiconductor is 0.1-1 mg / mL.

2. The method for growing continuous organic single crystals by polymer-assisted dual-phase impregnation pulling according to claim 1, characterized in that: The substrate is a silicon wafer, and the substrate is cleaned by the following steps: first, the substrate is placed in deionized water and ultrasonically treated at 40% power for 15 minutes, then placed in acetone and ultrasonically treated at 40% power for 15 minutes, then placed in isopropanol and ultrasonically treated at 40% power for 15 minutes, and finally, the substrate is blown dry with nitrogen or inert gas.

3. The method for growing continuous organic single crystals by polymer-assisted dual-phase impregnation pulling according to claim 1, characterized in that: The polyvinyl alcohol is of 0588 low viscosity type, and has an alcoholysis degree of 87.0-89.0 mol / mol.

4. The method for growing continuous organic single crystals by polymer-assisted dual-phase impregnation pulling according to claim 1, characterized in that: The water in the polyvinyl alcohol aqueous solution is ultrapure water with an electrical conductivity of 18.2 MΩ cm -1 The organic semiconductor in the organic semiconductor solution is C6-DPA or TIPS-PEN, and the solvent in the organic semiconductor solution is chlorobenzene.

5. The method for growing continuous organic single crystals by polymer-assisted dual-phase impregnation pulling according to claim 1, characterized in that: The volume of the lower layer polyvinyl alcohol aqueous solution is 10 mL, and the volume of the upper layer organic semiconductor solution is 30 μL.

6. The method for growing continuous organic single crystals by polymer-assisted dual-phase impregnation pulling according to claim 1, characterized in that: The biphasic solution was placed in a clean glass container, which was cleaned by the following steps: first, an alkaline solution was used to remove surface dust and oil stains, then the glass container was cleaned with clean water, then the glass container was immersed in anhydrous ethanol for 30 minutes, then the glass container was immersed in deionized water for 10 minutes, and finally dried in an oven at 65°C.

7. Use of the method for growing continuous organic single crystals by polymer-assisted dual-phase impregnation pulling according to any one of claims 1 to 6 in preparing organic single crystals or organic single crystal films.

8. Use of an organic single crystal or an organic single crystal film prepared by the method for growing continuous organic single crystals by polymer-assisted dual-phase immersion pulling according to any one of claims 1 to 6 in an organic field effect transistor device.