Lithium battery single crystal positive electrode material and preparation method and application thereof

The preparation of lithium battery single crystal positive electrode material is simplified by segmented spray pyrolysis, and the stress and cyclic performance problems of the cathode material in the prior art are solved, and the efficient and low-cost preparation of lithium battery single crystal positive electrode material is achieved, which significantly improves the electrical power of the material Chemical properties and preparation efficiency.

CN118957753APending Publication Date: 2024-11-15CHINA ELECTRONIC TECH GRP CORP NO 18 RES INST
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411068565.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing lithium battery positive electrode materials are prone to stress during charging and discharging, resulting in increased cracking, powdering and side reactions, attenuation of cycling performance, and complex preparation process and high cost.

Method used

The mixed liquid is subjected to temperature control treatment by segmented spray pyrolysis method, and the powdered lithium battery single crystal positive electrode material with uniform particle size dispersion is directly obtained, the process flow is simplified, the consumption of auxiliary materials and wastewater treatment is reduced, and complex processes are avoided.

Benefits of technology

It significantly reduces preparation time, improves efficiency, basically has no by-products, improves the cyclic and electrochemical properties of single-crystal positive electrode materials, and is suitable for large-scale preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957753A_ABST
    Figure CN118957753A_ABST
Patent Text Reader

Abstract

The invention provides a lithium battery single-crystal positive electrode material and a preparation method and application thereof, and the preparation method comprises the following steps: carrying out segmented spray pyrolysis treatment on a mixed solution to obtain the lithium battery single-crystal positive electrode material, wherein the mixed solution at least comprises a raw material solution containing a lithium source, a nickel source, a cobalt source and a manganese source; the segmented spray pyrolysis at least comprises a first treatment stage and a second treatment stage, the temperature of the first treatment stage is 450-600 DEG C, and the temperature of the second treatment stage is 750-1200 DEG C. The method has the beneficial effects that the mixed solution is subjected to spray pyrolysis by adopting a segmented spray pyrolysis method to obtain the powdery lithium battery single-crystal positive electrode material with uniformly dispersed particle sizes, so that the preparation time can be remarkably shortened, the efficiency is improved, almost no by-product is generated, large-scale preparation of the lithium battery single-crystal positive electrode material is facilitated, and the production cost is reduced. And the single-crystal particles prepared by the method are good in dispersion uniformity, so that the electrical performance of the single-crystal positive electrode material is favorably exerted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery positive electrode materials, and in particular to a lithium battery single crystal positive electrode material, a preparation method and application thereof. Background Art

[0002] With the development of science and technology, lithium-ion batteries have been widely used in various fields. The rapid development of electric vehicles, mobile devices and other fields has put higher and higher requirements on battery energy density, charging speed, cycle life and other performance. As a key component of the battery, the performance of the positive electrode material directly affects the various indicators of the battery. For example, the ternary positive electrode material currently on the market can increase the specific capacity of the positive electrode material by increasing the nickel content in its components, thereby increasing the energy density of the prepared battery. However, with the increase of nickel content, the crystal structure of the ternary positive electrode material changes more during the charging and discharging process, which is easy to generate stress, causing cracking and pulverization of the positive electrode material particles, increased side reactions and other problems, resulting in the attenuation of the positive electrode material cycle performance. However, by making the positive electrode material particles single crystal, the generation and concentration of stress can be suppressed, thereby improving the cycle performance of the positive electrode material.

[0003] Chinese patent with publication number CN116730405A discloses a single crystal positive electrode material precursor and its preparation method and application. Chinese patent with publication number CN116435499A discloses a single crystal positive electrode material and its preparation method and lithium ion battery. Both adopt liquid phase co-precipitation method to prepare ternary precursor, and then sinter with lithium and air flow pulverize to prepare positive electrode material. This method has complicated process, and liquid phase co-precipitation reaction requires the use of precipitant, complexing agent, etc. To obtain a relatively pure ternary precursor, a large amount of washing, filter pressing and other operations are required, which consumes a large amount of auxiliary materials and wastewater treatment, and the cost is relatively high.

[0004] Therefore, it is of great significance to develop a low-cost and efficient method for preparing lithium battery single crystal positive electrode materials. Summary of the invention

[0005] The purpose of the present invention is to provide a lithium battery single crystal positive electrode material, a preparation method and application thereof, and to directly obtain a powdered lithium battery single crystal positive electrode material with uniform particle size dispersion by performing segmented temperature-controlled spray pyrolysis on the raw materials by spray pyrolysis method, without the need to first prepare a precursor, then sinter with lithium, and perform air flow crushing and other complex steps. While simplifying the process flow and improving the preparation efficiency, it can also avoid the problems of large auxiliary material consumption, large wastewater treatment volume, and high cost in the prior art.

[0006] The first object of the present invention is to provide: a method for preparing a lithium battery single crystal positive electrode material, the steps of which include: performing a segmented spray pyrolysis treatment on a mixed solution to obtain a lithium battery single crystal positive electrode material;

[0007] in:

[0008] The mixed solution at least includes a raw material solution containing a lithium source, a nickel source, a cobalt source and a manganese source;

[0009] The staged spray pyrolysis comprises at least a first processing stage and a second processing stage, wherein the temperature of the first processing stage is 450-600°C, and the temperature of the second processing stage is 750-1200°C.

[0010] Preferably, the molar ratio of the substances in the raw material solution satisfies: lithium source: (nickel source + cobalt source + manganese source) = (1.0-1.1): 1, and the total concentration of nickel ions, cobalt ions and manganese ions in the raw material solution is 0.5-3M.

[0011] Preferably, the lithium source includes one or more of lithium hydroxide, lithium carbonate and lithium chloride.

[0012] Preferably, the nickel source, the cobalt source and the manganese source are soluble sulfates or chlorides.

[0013] Preferably, the mixed solution further comprises an additive accounting for 0-5wt% of the raw material solution, and the additive comprises one or more of nano-scale zirconium dihydrogen phosphate sol, nano-ammonium tungstate sol, nano-aluminum hydroxide sol, nano-titanium dioxide sol, and nano-antimony trioxide sol.

[0014] Preferably, during the staged spray pyrolysis, the mixed liquid is placed in an oxygen atmosphere with an oxygen concentration of more than 90%.

[0015] Preferably, during staged spray pyrolysis, the flow rate of adding the mixed liquid is 0.1 to 1 L / h.

[0016] Preferably, the treatment time of the first treatment stage is 1 to 3 hours, and the treatment time of the second treatment stage is 7 to 12 hours.

[0017] Another object of the present invention is to provide: a lithium battery single crystal positive electrode material, which is prepared by the preparation method of the lithium battery single crystal positive electrode material as described above.

[0018] Another object of the present invention is to provide: a lithium-ion battery, which is made from the lithium battery single crystal positive electrode material as described above.

[0019] The beneficial effects of the present invention are as follows: the preparation method adopts a segmented spray pyrolysis method to spray pyrolyze the mixed liquid to obtain a powdered lithium battery single crystal positive electrode material with uniform particle size dispersion, which can significantly reduce the preparation time and improve efficiency, has basically no by-products, and is conducive to the large-scale preparation of lithium battery single crystal positive electrode materials. In addition, the single crystal particles prepared by this method have good dispersion uniformity, which is conducive to the performance of the electrical properties of the single crystal positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1is a SEM image of the lithium nickel cobalt manganese oxide single crystal particles prepared in Example 1 of the present invention;

[0021] Figure 2 is an XRD diagram of the lithium nickel cobalt manganese oxide single crystal particles prepared in Example 1 of the present invention;

[0022] Figure 3 This is a SEM image of the nickel-cobalt-manganese-oxide lithium single crystal positive electrode material prepared in Comparative Example 1 of the present invention;

[0023] Figure 4 This is the XRD diagram of the nickel cobalt manganese oxide single crystal positive electrode material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with embodiments and drawings:

[0025] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and comparative examples, and are not intended to limit the scope of protection of the present invention. It should be particularly noted that there may be multiple names for the same organic structure, as long as the structure is within the scope of this patent, it belongs to the protection object of this patent.

[0026] Unless otherwise defined, the raw materials, reagents, etc. in the following examples can be purchased from the market or prepared according to reported methods.

[0027] The present embodiment provides a method for preparing a lithium battery single crystal positive electrode material, a lithium battery single crystal positive electrode material prepared by the method, and an application of the lithium battery single crystal positive electrode material in a lithium-ion battery.

[0028] The process of preparing a lithium battery single crystal positive electrode material using the preparation method comprises the following steps:

[0029] (1) A raw material solution containing a lithium source, a nickel source, a cobalt source and a manganese source is mixed with an additive to obtain a mixed solution.

[0030] In this step, the lithium source is selected from one or more of lithium hydroxide, lithium carbonate and lithium chloride, preferably lithium hydroxide and lithium carbonate. Among the three, lithium hydroxide has higher reactivity and is more beneficial to the formation of lithium battery single crystal positive electrode materials. In addition, the byproducts after the reaction of lithium hydroxide and lithium carbonate are only water and carbon dioxide, which is environmentally friendly, does not require additional treatment, and reduces costs. The nickel source, cobalt source and manganese source are selected from soluble sulfates or chlorides of Ni, Co and Mn, respectively.

[0031] In this step, the additive is selected from one or more of nano-scale zirconium dihydrogen phosphate sol, nano-ammonium tungstate sol, nano-aluminum hydroxide sol, nano-titanium dioxide sol, and nano-antimony trioxide sol, which is used to enhance the structural stability of lithium battery single crystal positive electrode materials and improve the electrochemical properties of the materials.

[0032] (2) adding the mixed liquid into a spray pyrolysis device, creating an oxygen atmosphere with a concentration of more than 90% in the spray pyrolysis device, adding the mixed liquid at a flow rate of 0.1 to 1 L / h, and performing segmented spray pyrolysis treatment on the mixed liquid using the spray pyrolysis device to obtain a powdered lithium battery single crystal positive electrode material.

[0033] In this step, the segmented spray pyrolysis includes a first treatment stage and a second treatment stage. The temperature of the first treatment stage is 450-600°C, and the treatment time is 1-3 hours. This treatment stage is a process of dehydrating the mixed solution and forming a eutectic body with the lithium source and other metal ions; the temperature of the second treatment stage is 750-1200°C, and the treatment time is 7-12 hours. This treatment stage is a process of crystallizing the eutectic body, undergoing an oxidation reaction in an oxygen atmosphere to generate a target metal oxide, and forming a lithium battery single crystal positive electrode material with uniform single crystal particle distribution. The specific reaction process of the two stages is as follows:

[0034] The first treatment stage: LiOH·H2O+aNiCl2+bCoCl2+cMnCl2+0.5O2→2HCl+0.5H2O+0.5Li2O·Ni a Co b Mn c O(a+b+c=1);

[0035] Second processing stage: 0.5Li2O·Ni a Co b Mn c O+0.25O2→LiNi a Co b Mn c O2.

[0036] When the mixed liquid is added at a flow rate of 0.1 to 1 L / h, the positive electrode material formed after the segmented spray pyrolysis treatment has better performance. If the flow rate is too high, the spray pyrolysis temperature will increase and the spray pyrolysis time will be prolonged, thereby reducing production efficiency.

[0037] Preferably, the molar ratio of the substances in the raw material solution in step (1) satisfies: In the raw material solution, the molar ratio of the substances satisfies: lithium source: (nickel source + cobalt source + manganese source) = (1.0-1.1): 1, so as to obtain a lithium battery single crystal positive electrode material with good morphology and good quality. If the total amount of the nickel source, cobalt source and manganese source accounts for too high a proportion, the capacity of the material is relatively high, but the cycle performance of the material is reduced. If the total amount of the nickel source, cobalt source and manganese source accounts for too low a proportion, the cycle performance of the material will be improved, but the capacity is not the highest. Moreover, when the total amount of the nickel source, cobalt source and manganese source accounts for too low a proportion, the residual alkali on the surface of the material will increase, thereby affecting its performance. The total concentration of nickel ions, cobalt ions and manganese ions in the raw material solution is 0.5-3M, so as to generate the target metal oxide (LiNi a Co b Mn c O2), if the total concentration of the above ions is too high, some metal ions may not undergo oxidation reaction within the preset spray pyrolysis temperature range and time range, resulting in poor performance of the final single crystal; if the concentration is too low, it may cause low production capacity and reduced efficiency.

[0038] The amount of additive added to the mixed liquid is preferably: 0-5wt% of the raw material liquid. The main function of the additive is to enhance the structural stability of the lithium battery single crystal positive electrode material and improve the electrochemical properties of the lithium battery single crystal positive electrode material. Do not add too much, otherwise it will cause the capacity of the lithium battery single crystal positive electrode material to decrease and affect the material performance.

[0039] The preparation method adopts a segmented spray pyrolysis method to spray pyrolyze the mixed liquid to obtain a powdered lithium battery single crystal positive electrode material with uniform particle size dispersion, which can significantly reduce the preparation time and improve efficiency, has basically no by-products, and is conducive to the large-scale preparation of lithium battery single crystal positive electrode materials. In addition, the single crystal particles prepared by this method have good dispersion uniformity, which is conducive to the performance of the electrical properties of the single crystal positive electrode material.

[0040] Some specific embodiments are listed below.

[0041] Embodiment 1:

[0042] Nickel chloride, cobalt chloride and manganese chloride were added into deionized water at a molar ratio of Ni:Co:Mn=0.8:0.1:0.1, and dissolved and mixed; lithium hydroxide monohydrate was added at a molar ratio of lithium source:(nickel source+cobalt source+manganese source)=1.05:1 to obtain a raw material solution with a total concentration of nickel ions, cobalt ions and manganese ions of 1.5M;

[0043] Adding 0.5 wt % of nano aluminum hydroxide sol and 1 wt % of nano zirconium hydrogen phosphate sol into the raw material liquid, and mixing them evenly by ultrasonic stirring to obtain a uniformly dispersed mixed liquid;

[0044] The mixed liquid is added into the spray pyrolysis device at a flow rate of 0.5 L / h, and oxygen with a concentration of more than 90% is introduced to perform segmented spray pyrolysis treatment;

[0045] During the staged spray pyrolysis, the temperature of the first treatment stage is controlled to be 550°C and the duration is 1 to 3 hours, and the temperature of the second treatment stage is controlled to be 810°C and the duration is 7 to 12 hours, so as to obtain powdered lithium nickel cobalt manganese oxide single crystal particles (i.e., lithium battery single crystal positive electrode material) with uniform particle size distribution.

[0046] The electron microscope image of the lithium nickel cobalt manganese oxide single crystal particles prepared in this embodiment is as follows: Figure 1 As shown in the figure, it can be seen that the particle size of the prepared lithium battery single crystal positive electrode material is uniformly dispersed; its XRD Figure 2 As shown in the figure, it can be seen that lithium nickel cobalt manganese oxide single crystal particles were successfully prepared by segmented spray pyrolysis.

[0047] Embodiment 2:

[0048] Nickel chloride, cobalt chloride and manganese chloride were added into deionized water at a molar ratio of Ni:Co:Mn=0.9:0.07:0.03, and dissolved and mixed; lithium hydroxide monohydrate was added at a molar ratio of lithium source:(nickel source+cobalt source+manganese source)=1.05:1 to obtain a raw material solution with a total concentration of nickel ions, cobalt ions and manganese ions of 1.5M;

[0049] Adding 0.5 wt % of nano aluminum hydroxide sol and 1 wt % of nano zirconium hydrogen phosphate sol into the raw material liquid, and mixing them evenly by ultrasonic stirring to obtain a uniformly dispersed mixed liquid;

[0050] The mixed liquid is added into the spray pyrolysis device at a flow rate of 0.5 L / h, and oxygen with a concentration of more than 90% is introduced to perform segmented spray pyrolysis treatment;

[0051] During the staged spray pyrolysis, the temperature of the first treatment stage is controlled to be 550°C and the duration is 1 to 3 hours, and the temperature of the second treatment stage is controlled to be 760°C and the duration is 7 to 12 hours, so as to obtain powdered lithium nickel cobalt manganese oxide single crystal particles (i.e., lithium battery single crystal positive electrode material) with uniform particle size distribution.

[0052] Embodiment 3:

[0053] Nickel chloride, cobalt chloride and manganese chloride were added into deionized water at a molar ratio of Ni:Co:Mn=0.6:0.1:0.3, and dissolved and mixed; lithium hydroxide monohydrate was added at a molar ratio of lithium source:(nickel source+cobalt source+manganese source)=1.05:1 to obtain a raw material solution with a total concentration of nickel ions, cobalt ions and manganese ions of 1.5M;

[0054] Adding 0.5 wt % of nano aluminum hydroxide sol and 1 wt % of nano zirconium hydrogen phosphate sol into the raw material liquid, and mixing them evenly by ultrasonic stirring to obtain a uniformly dispersed mixed liquid;

[0055] The mixed liquid is added into the spray pyrolysis device at a flow rate of 0.5 L / h, and oxygen with a concentration of more than 90% is introduced to perform segmented spray pyrolysis treatment;

[0056] During the staged spray pyrolysis, the temperature of the first treatment stage is controlled to be 550°C and the duration is 1 to 3 hours, and the temperature of the second treatment stage is controlled to be 920°C and the duration is 7 to 12 hours, so as to obtain powdered lithium nickel cobalt manganese oxide single crystal particles (i.e., lithium battery single crystal positive electrode material) with uniform particle size distribution.

[0057] Comparative Example 1:

[0058] (1) Preparation of precursor:

[0059] Nickel sulfate, cobalt sulfate and manganese sulfate are prepared into a ternary solution with a total metal ion concentration of 2M according to a molar ratio of Ni:Co:Mn=8:1:1, 4M industrial liquid alkali is used as a precipitant solution, and 20% ammonia water is used as a complexing agent solution;

[0060] Add 90L of deionized water to the reactor, control the stirring speed at 500rpm, heat to 65°C, replace with nitrogen for 2h, and then add 20% ammonia water to adjust the pH of the bottom liquid to 11.0;

[0061] The ternary solution was added into the reactor at a rate of 15 L / h, the precipitant solution was added at a rate of 8 L / h, and the complexing agent solution was added at a rate of 2 L / h for 13 hours. When the particle size D50 was greater than 3.5 μm, the feeding was stopped and the stirring and aging were continued for 2 hours.

[0062] The aged slurry was transferred to a filter press, and washed and filtered for multiple times until the pH of the final filtrate was less than 10, and the filter cake was transferred to a vacuum oven and dried at 120° C. for 12 h, and the magnetic substances introduced in the reaction were sieved to remove them, thereby obtaining a precursor;

[0063] (2) Preparation of lithium battery single crystal positive electrode materials:

[0064] Lithium hydroxide and the precursor obtained in step (1) are mixed in a molar ratio of lithium: (nickel + cobalt + manganese) = 1.05:1, sintered at 850° C. in a pure oxygen atmosphere for 10 h, and then subjected to a gas flow pulverization operation to obtain a pulverized nickel-cobalt-manganese single crystal positive electrode material.

[0065] The electron microscope image of the nickel-cobalt-manganese single crystal positive electrode material prepared in this comparative example is as follows: Figure 3 As shown in the figure, it can be seen that the prepared single crystal positive electrode material particles are unevenly dispersed and there is adhesion between the particles; its XRD Figure 4As shown in the figure, it can be seen that the nickel cobalt manganese oxide lithium single crystal positive electrode material was successfully prepared by liquid phase co-precipitation method.

[0066] Application Example 1:

[0067] The nickel cobalt manganese oxide single crystal particles obtained in Example 1 and the nickel cobalt manganese oxide single crystal positive electrode material obtained in Comparative Example 1 were respectively used as positive electrode materials for lithium ion batteries, and button-type lithium ion batteries were assembled with lithium sheets as negative electrodes, 1M LiPF6 / (EC+EMC+DMC) as electrolytes, and polypropylene microporous diaphragms. The electrical properties were tested, and the results are shown in Table 1.

[0068]

[0069] It can be seen from Table 1 that the electrical properties of the lithium battery single crystal positive electrode material prepared by segmented spray pyrolysis through the present preparation method are better.

[0070] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing a lithium battery single crystal positive electrode material, characterized in that: The mixed solution is subjected to a staged spray pyrolysis treatment to obtain a lithium battery single crystal positive electrode material; in: The mixed solution at least includes a raw material solution containing a lithium source, a nickel source, a cobalt source and a manganese source; The staged spray pyrolysis comprises at least a first processing stage and a second processing stage, wherein the temperature of the first processing stage is 450-600°C, and the temperature of the second processing stage is 750-1200°C.

2. The method for preparing a lithium battery single crystal positive electrode material according to claim 1, characterized in that: The molar ratio of the substances in the raw material solution satisfies: lithium source: (nickel source + cobalt source + manganese source) = (1.0-1.1): 1, and the total concentration of nickel ions, cobalt ions and manganese ions in the raw material solution is 0.5-3M.

3. The method for preparing a lithium battery single crystal positive electrode material according to claim 2, characterized in that: The lithium source includes one or more of lithium hydroxide, lithium carbonate and lithium chloride.

4. The method for preparing a lithium battery single crystal positive electrode material according to claim 2, characterized in that: The nickel source, the cobalt source and the manganese source are soluble sulfates or chlorides.

5. The method for preparing a lithium battery single crystal positive electrode material according to any one of claims 1 to 4, characterized in that: The mixed solution also includes additives accounting for 0-5wt% of the raw material solution, and the additives include one or more of nano-level zirconium dihydrogen phosphate sol, nano-ammonium tungstate sol, nano-aluminum hydroxide sol, nano-titanium dioxide sol, and nano-antimony trioxide sol.

6. The method for preparing a lithium battery single crystal positive electrode material according to claim 1, characterized in that: During the staged spray pyrolysis, the mixed liquid is placed in an oxygen atmosphere with a concentration of more than 90%.

7. The method for preparing a lithium battery single crystal positive electrode material according to claim 1, characterized in that: During staged spray pyrolysis, the flow rate of adding the mixed liquid is 0.1-1 L / h.

8. The method for preparing a lithium battery single crystal positive electrode material according to claim 1, characterized in that: The treatment time of the first treatment stage is 1 to 3 hours, and the treatment time of the second treatment stage is 7 to 12 hours.

9. A lithium battery single crystal positive electrode material, characterized in that: The lithium battery single crystal positive electrode material is prepared by the preparation method of any one of claims 1 to 8.

10. A lithium ion battery, characterized in that: It is prepared by the lithium battery single crystal positive electrode material according to claim 9.

Citation Information

Cited By

  • Modified positive electrode precursor and preparation method and application thereof

    CN120698522A