Rare-earth-ion-doped lanthanum scandate laser single-crystal optical fiber and preparation method thereof

Through rare earth ion-doped lanthanum scandium laser single crystal fiber, the Re2xLa1-2xScO3 single crystal fiber is grown by laser heating base method, which solves the problem of difficulty in growing cubic rare earth sesquioxide crystals and achieves high-quality and low-cost High-temperature oxide crystal growth, with excellent thermal, optical and mechanical properties, is suitable for the generation of high-power pulsed lasers.

CN118957759APending Publication Date: 2024-11-15XUZHOU NORMAL UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411071465.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to grow high-quality large-size cubic rare earth sesquioxide crystals, especially in maintaining a stable thermal gradient and avoiding cracking, which makes crystal preparation very difficult under high temperature and high pressure conditions.

Method used

Re2xLa1-2xScO3 single crystal fibers are prepared by laser heating base method using rare earth ion-doped lanthanum scandium laser single crystal fibers. The single crystal fibers are grown at high temperatures using CO2 lasers and lifting devices, achieving rapid growth and reduced production. cost.

Benefits of technology

The Re2xLa1-2xScO3 single crystal fiber with glass fiber characteristics and excellent performance in block crystals was successfully grown, which has high thermal conductivity, mechanical properties and optical properties. It is suitable for the generation of pulsed lasers in different bands and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957759A_ABST
    Figure CN118957759A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth element doped lanthanum scandate laser single crystal optical fiber and a preparation method thereof, the chemical formula of the single crystal optical fiber is Re2xLa1-2xScO3, and Re is a rare earth ion; when Re is Yb < 3 + >, x is more than or equal to 0.005 and less than or equal to 0.05; when Re is Nd < 3 + >, x is not less than 0.005 and not more than 0.02; when Re is Er < 3 + >, x is not less than 0.01 and not more than 0.07, and when Re is Tm < 3 + >, x is not less than 0.005 and not more than 0.05; and when Re is Ho < 3 + >, x is not less than 0.005 and not more than 0.015. The method comprises the following steps: preparing a source rod by adopting molding packaging layering, cold isostatic pressing and sintering, growing a single crystal optical fiber by a laser heating base method, and growing in the air. The method is simple in process, the production cost can be effectively reduced, and the single crystal optical fiber with high optical quality can be grown; the prepared lanthanum scandate single crystal optical fiber has the characteristic of high length-diameter ratio, and can be applied to an intermediate infrared laser and a novel high-temperature sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of laser materials and preparation thereof, and specifically relates to visible and near-infrared band laser single crystal optical fibers and preparation methods thereof, and particularly relates to a rare earth ion-doped lanthanum scandate laser single crystal optical fiber and preparation method thereof. Background Art

[0002] Laser crystal materials have the characteristics of excellent thermal properties, good optical quality and low threshold, and are one of the most widely used laser gain materials at present. They have important application prospects in high-power pump sources, lidar, medical treatment and scientific research.

[0003] In scientific research and industry, light in the visible and near-infrared bands is commonly produced using solid-state lasers and other light sources. The visible light band roughly ranges between 380 and 780 nanometers. Electromagnetic waves in this range can be perceived by the human eye as different colors. Visible light is very important in everyday life and is the basis of many visual processes and optical technologies. The near-infrared light band generally refers to electromagnetic waves with wavelengths between 780 nanometers and about 2.5 microns. Light in this band is invisible to the human eye, but is very important in many scientific and technological applications. Near-infrared light can penetrate some materials, such as skin, clouds, and certain types of plastics, and therefore has applications in remote sensing, medical imaging, communications, and many other fields.

[0004] According to the matrix material, the mainstream laser crystal materials widely used in the laser field can be divided into fluoride matrix materials, sesquioxide matrix materials and garnet matrix materials. Among them, sesquioxide has high thermal conductivity, small maximum phonon energy, and stable physical and chemical properties, which has attracted much attention in recent years. High thermal conductivity is conducive to the evacuation of crystal heat, reducing the thermal effect of the crystal during the operation of the laser; low phonon energy can reduce the probability of non-radiative transitions and multi-phonon relaxation, and effectively improve the fluorescence emission efficiency. At the same time, sesquioxide has moderate hardness, stable physical and chemical properties, good mechanical properties, and convenient processing and storage of crystals. However, the melting point of cubic rare earth sesquioxide is very high, about 500℃ higher than the melting point of the mainstream laser medium YAG. Therefore, the preparation of sesquioxide crystals is very difficult, especially large-sized high-quality sesquioxide crystals. It is difficult to maintain a stable thermal gradient during the growth process and it is easy to crack.

[0005] Therefore, by selecting rare earth ion-doped lanthanum scandate single crystal optical fiber, high-efficiency and high-power laser output can be obtained in the near- and mid-infrared bands of 1 to 3 μm. Summary of the invention

[0006] The purpose of the present invention is to provide a rare earth ion doped lanthanum scandate laser single crystal optical fiber and a preparation method thereof, which has a simple process, can effectively reduce the production cost, and can grow high-quality Re 2x La1-2x ScO3 single crystal optical fiber; the prepared Re 2x La 1-2x ScO3 single crystal fiber has the advantages of both glass fiber and crystal, which is conducive to obtaining pulsed lasers in different bands.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A rare earth ion doped lanthanum scandate laser single crystal optical fiber, the chemical formula of the single crystal optical fiber is Re 2x La 1- 2x ScO3, where Re is Yb 3+ 、Nd 3+ , 3+ 、Tm 3+ 、Ho 3+ One of the rare earth ions, x is a rare earth ion replacing La 3+ The molar percentage of the lattice site; when Re is Yb 3+ When Re is Nd 3+ When 0.005≤x≤0.02; when Re is Er 3+ When Re is Tm 3+ When 0.005≤x≤0.05; when Re is Ho 3+ When 0.005≤x≤0.015.

[0009] Preferably, the single crystal optical fiber belongs to an orthorhombic crystal system, and has a diameter of 0.4 to 1 mm and a length of 20 to 150 mm.

[0010] The present invention also provides a method for preparing the above-mentioned rare earth ion-doped lanthanum scandate laser single crystal optical fiber, which adopts a laser heating base method and specifically comprises the following steps:

[0011] (1) Using Yb2O3 powder / Nd2O3 powder / Er2O3 powder / Tm2O3 powder / Ho2O3 powder La2O3 powder and Sc2O3 powder with a purity of 99.99% as raw materials, according to the molecular formula Re 2x La 1-2x Weigh each raw material according to the stoichiometric ratio of the corresponding elements in ScO3; where x is the rare earth ion replacing La 3+ The molar percentage of the lattice site is 3+ When Re is Nd 3+ When 0.005≤x≤0.02; when Re is Er 3+ When Re is Tm 3+When 0.005≤x≤0.05; when Re is Ho 3+ When 0.005≤x≤0.015.

[0012] (2) The weighed raw materials are mixed uniformly, pressed into cylindrical rods by a cold isostatic press at 200-300 MPa for 180-300 s, sintered in a muffle furnace in an air atmosphere to obtain ceramic rods, the sintering temperature is 1600-1650° C., the sintering time is 15-24 h, cut into ceramic rods with a diameter of 1-2 mm by a wire cutting machine, and dried at room temperature for 4-8 h to obtain material rods, which are used as seed crystals and source rods respectively;

[0013] (3) Clean the cavity of the laser substrate heating furnace for crystal growth and the reflective conical mirror, annular plane reflective mirror and focusing mirror in the optical system, and adjust the optical path to be uniform; fix the prepared source rod on the seed crystal rod of the feeding device below, and fix the prepared seed crystal on the pulling device above;

[0014] (4) Turn on the CO2 laser, adjust the center of the source rod to the center of the laser focus, melt the top of the source rod into a hemispherical melt, adjust the position of the seed crystal so that the seed crystal contacts the melt and is located in the center of the hemispherical melt, and then slowly contact the seed crystal with the hemispherical melt. Keep the state for at least 2 minutes to allow the molten zone to stabilize, then start to pull the seed crystal through the pulling device and start the feeding device to raise the source rod. After the shoulder release and equal diameter growth, when the grown crystal reaches the required length, close the feeding device and lift the crystal off;

[0015] (5) The obtained crystal is fixed on the feeding device as a source rod again, and secondary growth is performed according to the above steps (3) and (4) to obtain a longer and thinner single crystal optical fiber;

[0016] (6) After the single crystal fiber is pulled off, the laser power is reduced at a rate of 0.02-0.05 W / s. After turning off the CO2 laser, flowing air is passed through. After 5-15 minutes, the crystal growth furnace is opened and the crystal is removed to obtain Re 2x La 1-2x ScO3 single crystal optical fiber.

[0017] Preferably, in step (2), the cross section of the source rod is (1-2)×(1-2) mm 2 , length is 50~120mm.

[0018] Preferably, in steps (4) and (5), the cross section of the prepared single crystal optical fiber is (0.3-1)×(0.3-1) mm 2 , length is 20~120mm.

[0019] Preferably, in step (4), the power at the center of the laser heating source rod is 25 to 50 W, and the heating time is 2 to 5 minutes.

[0020] Preferably, in step (5), the power at the center of the laser heating source rod is 10 to 25 W, and the heating time is 1 to 3 minutes.

[0021] Preferably, in step (4), the parameters of the equal-diameter growth include: a pulling speed of 10 to 20 mm / h; a feeding speed of 10 to 20 mm / h; a power at the center of the laser being maintained at 25 to 50 W; and a growth time of 2 to 6 hours.

[0022] Preferably, in step (5), the parameters of the equal-diameter growth include: a pulling speed of 30 to 60 mm / h; a feeding speed of 10 to 20 mm / h; a power at the laser center of 10 to 25 W; and a growth time of 2 to 6 hours.

[0023] Furthermore, in step (6), the crystal is taken out and then placed in a muffle furnace for high temperature annealing at 1450-1500° C. for 24 hours in a hydrogen atmosphere.

[0024] The chemical composition of the present invention is Re 2x La 1-2x ScO3 single crystal optical fiber is a typical perovskite crystal with a space group of Pnma (no.62). In LaScO3 crystal, each La ion is coordinated by 6 oxygen ions and 3 Sc ions to form an octahedral coordination structure, while each Sc ion is coordinated by 6 oxygen ions and 3 La ions to form an octahedral coordination configuration. This coordination configuration helps to stabilize the crystal structure and improve the stability of the material. They are chemically stable, have optical bandgap, high thermal conductivity and excellent mechanical properties. Due to La 3+ and Sc 3+ The random distribution of cation sites forms a disordered structure. Their disordered crystal structure produces a wider and smoother spectrum due to the inhomogeneous spectral broadening effect. This broadening helps to generate ultrashort pulses. Ideally, disordered crystals should have good thermal, thermo-optical and thermo-mechanical properties to support power expansion and generate high peak power pulse output. Therefore, this material is promising for ultrafast lasers.

[0025] Compared with the prior art solutions, the present invention has the following advantages:

[0026] (1) Re prepared by the present invention 2x La 1-2xScO3 single crystal optical fiber has the characteristics of high specific surface area and optical waveguide of glass optical fiber, and also has the physical and chemical properties of excellent thermal conductivity, high hardness, excellent optical properties, corrosion resistance and other physical and chemical properties of bulk crystal materials. It combines the excellent physical and chemical properties of single crystal with the unique size advantage of optical fiber.

[0027] (2) The present invention adopts the laser heating base method to prepare Re 2x La 1-2x ScO3 single crystal optical fiber, this method has a fast growth speed, short growth cycle, does not require a crucible container, saves costs to a great extent, avoids the influence of the crucible material on the single crystal optical fiber, and the growth of crystals is no longer limited by the melting point of the crucible material. It can easily grow high-temperature crystals exceeding 2000℃, which is very suitable for growing Re 2x La 1-2x High temperature oxide crystals such as ScO3;

[0028] (3) Since the lanthanum scandate crystal of the present invention is an oxide crystal, it has better physical and chemical properties than fluoride crystals and other ceramics or optical fibers. The crystal fiber has the advantages of high thermal conductivity, high laser damage threshold, small nonlinear effect, etc., making it possible for single crystal optical fibers to produce higher power output and transmit higher energy lasers.

[0029] (4) The present invention uses the secondary growth technology to reduce the ion segregation, stress and bubble defects inside the optical fiber, and grows a longer and thinner single crystal optical fiber. 2x La 1-2x ScO3 crystal growth method, the first time to grow high-quality Re by LHPG technology 2x La 1-2x ScO3 single crystal optical fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a photo of a sample prepared in Example 1 of the present invention;

[0031] Figure 2 The fluorescence spectrum of the sample prepared in Example 1 of the present invention;

[0032] Figure 3 The fluorescence lifetime decay curve of the sample prepared in Example 1 of the present invention;

[0033] Figure 4 It is a schematic diagram of a crystal growth device in the present invention;

[0034] In the figure: 1. CO2 laser, 2. beam expander, 3. optical attenuator, 4. reflecting conical mirror, 5. annular plane reflecting mirror, 6. feeding device, 7. pulling device, 8. focusing mirror, 9. grown crystal, 10. hemispherical melt, 11. source rod, 12. furnace wall. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0036] Example 1

[0037] Laser Heating Base Method to Produce Yb 0.01 La 0.99 The specific implementation steps of ScO3 (x is 0.005) single crystal optical fiber are as follows:

[0038] (1) According to the chemical reaction equation, the stoichiometric ratio is 0.005Yb2O3+0.495La2O3+0.5Sc2O3→Yb 0.01 La 0.99 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Yb2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g;

[0039] (2) The weighed raw materials were mixed evenly, filled into a balloon, and pressed by a cold isostatic press at 200 MPa for 180 seconds to form a cylindrical powder rod with a length of 100 mm and a diameter of 10 mm; the cylindrical powder rod was sintered in air to obtain a ceramic rod at a sintering temperature of 1600°C and a sintering time of 24 hours, and processed by a wire cutting machine to obtain a cross-section of 1.5×1.5 mm 2 , a square ceramic rod with a length of 90 mm, which is dried at room temperature for 6 hours to obtain a material rod, which is used as a seed crystal and a source rod 11 respectively;

[0040] (3) Clean the cavity of the laser substrate heating furnace for crystal growth and the reflective conical mirror 4, annular plane reflective mirror 5 and focusing mirror 8 in the optical system, and adjust the optical system of the equipment to make the focused heating spot heat evenly; fix the prepared source rod 11 on the lower feeding device 6, fix the prepared seed crystal on the upper pulling device 7, and adjust the position of the source rod and seed crystal through the camera to ensure that the subsequent growth molten zone is not skewed;

[0041] like Figure 4 As shown, the optical system includes a CO2 laser 1, a beam expander 2, an optical attenuator 3, a reflective conical mirror 4, an annular plane reflector 5, a feeding device 6, a pulling device 7, and a focusing mirror 8. The beam expander 2 is arranged between the CO2 laser 1 and the optical attenuator 3, the optical attenuator 3 is arranged on the furnace cavity wall 12, and the reflective conical mirror 4, the annular plane reflector 5, the feeding device 6, the pulling device 7 and the focusing mirror 8 are all arranged in the furnace cavity;

[0042] (4) Turn on the CO2 laser 1, adjust the center of the source rod 11 to be placed at the focal center of the laser so that the source rod 11 is evenly heated, and the top of the source rod 11 is melted into a hemispherical melt 10. Increase the power of the laser to 35W to melt the source rod 11, adjust the position of the seed crystal so that it is in contact with the melt 10 and located in the center of the hemispherical melt 10, and then slowly contact the seed crystal with the hemispherical melt 10. Keep the state for at least 2 minutes until the hemispherical melt 10 (growth interface melting zone) is stable, and gradually increase the power of the laser to 45W, start the pulling device 7, and neck at a pulling speed of 10mm / h; when the diameter of the seed crystal is reduced to about 0.5mm, adjust the power to 42W to release the shoulder and grow in equal diameter; during the equal diameter growth process, the pulling speed is 15mm / h, and the feeding speed is 13mm / h; when the grown crystal 9 reaches the required length, close the feeding device 6 and lift the crystal;

[0043] (5) The obtained crystal is fixed on the feeding device 6 as a source rod again, and secondary growth is performed according to the above steps (3) and (4) to obtain a longer and thinner single crystal optical fiber; the CO2 laser 1 is turned on, and the center of the source rod 11 is adjusted to be placed at the center of the laser focus so that the source rod 11 is evenly heated, and the top of the source rod 11 is melted into a hemispherical melt 10, and the power of the laser is increased to 20W to melt the source rod 11, and the position of the seed crystal is adjusted so that it is in contact with the melt 10 and is located at the center of the hemispherical melt 10, and then the seed crystal is slowly Contact the hemispherical melt 10, maintain the state for at least 2 minutes, wait for the hemispherical melt 10 (growth interface melting zone) to stabilize, and gradually increase the laser power to 22W, start the pulling device 7, and neck at a pulling speed of 10mm / h; when the seed crystal diameter is reduced to about 0.3mm, adjust the power to 18W for shoulder release and equal diameter growth; during the equal diameter growth process, the pulling speed is 40mm / h, and the feeding speed is 10mm / h; when the grown crystal 9 reaches the required length, close the feeding device 6 and lift the crystal;

[0044] (6) After the single crystal fiber is pulled off, the laser power is reduced at a rate of 0.05 W / s, and after turning off the CO2 laser 1, flowing air is passed through. After 15 minutes, the furnace chamber is opened and the crystal with a diameter of 1 mm is removed and is transparent and colorless;

[0045] (7) In order to eliminate the thermal stress in the crystal, prevent cracking, and improve the crystal quality, the crystal was annealed at 1400°C in a muffle furnace for 24 h to obtain transparent, colorless, high optical quality Yb 0.01 La 0.99 ScO3 single crystal optical fiber.

[0046] After measurement, the Yb 0.01 La 0.99The diameter of the ScO3 single crystal fiber is 0.5 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, and the length is 22 mm. The single crystal fiber is transparent and colorless with good optical quality.

[0047] See attached Figure 1 , the prepared Yb 0.01 La 0.99 ScO3 single crystal optical fiber material is transparent and has no cracking effect.

[0048] See attached Figure 2 ,As can be seen from the figure, the emission half peak width is wider, which is conducive to the tunable operation of the laser.

[0049] See attached Figure 3 , it can be seen from the figure that Yb 0.01 La 0.99 The fluorescence lifetime of ScO3 single crystal fiber is long, which can make the crystal easy to store energy and achieve efficient laser output.

[0050] Example 2

[0051] Growth of Nd by Laser Heating Susceptor 0.01 La 0.99 ScO3 (x is 0.005) single crystal optical fiber

[0052] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1) and step (7). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.005Nd2O3+0.495La2O3+0.5Sc2O3→Nd 0.01 La 0.99 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Nd2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The difference in step (5) of this embodiment is that the pulling speed during the equal diameter growth process is 28mm / h and the feeding speed is 10mm / h; the other steps are kept consistent with the embodiment, and finally a blue transparent Nd2O3 with good optical quality is obtained. 0.005 La 0.995 ScO3 single crystal optical fiber.

[0053] After measurement, the obtained Nd 0.01 La 0.99 The diameter of the ScO3 single crystal fiber is 0.6 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, the length is 30 mm, the single crystal fiber is transparent and blue and has good optical quality.

[0054] Example 3

[0055] Growth of Er by Laser Heating Substrate 0.02 La0.98 ScO3 (x is 0.01) single crystal optical fiber

[0056] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.01Er2O3+0.495La2O3+0.5Sc2O3→Er 0.02 La 0.98 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Nd2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The other steps are kept consistent with the embodiment, and finally pink transparent Er with good optical quality is obtained. 0.01 La 0.995 ScO3 single crystal optical fiber.

[0057] After measurement, the obtained Er 0.02 La 0.98 The diameter of the ScO3 single crystal fiber is 0.5 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, the length is 40 mm, the single crystal fiber is pink and transparent and has good optical quality.

[0058] Example 4

[0059] Growth of Tm by Laser Heating Susceptor 0.01 La 0.99 ScO3 (x is 0.005) single crystal optical fiber

[0060] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.005Tm2O3+0.495La2O3+0.5Sc2O3→Tm 0.01 La 0.99 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Nd2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The other steps are kept consistent with the embodiment, and finally a transparent, colorless, optically good Tm 0.005 La 0.995 ScO3 single crystal optical fiber.

[0061] After measurement, the obtained Tm 0.01 La 0.99 The diameter of the ScO3 single crystal fiber is 0.5 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, and the length is 26 mm. The single crystal fiber is transparent and colorless with good optical quality.

[0062] Example 5

[0063] Growth of Ho by Laser Heating Substrate0.01 La 0.99 ScO3 (x is 0.005) single crystal optical fiber

[0064] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.005Ho2O3+0.495La2O3+0.5Sc2O3→Ho 0.01 La 0.99 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Nd2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The difference in step (5) of this embodiment is that the pulling speed during the equal diameter growth process is 14mm / h and the feeding speed is 10mm / h; the other steps are kept consistent with the embodiment, and finally a yellow transparent Ho 0.01 La 0.99 ScO3 single crystal optical fiber.

[0065] After measurement, the Ho 0.01 La 0.99 The diameter of the ScO3 single crystal fiber is 0.8 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, the length is 30 mm, the single crystal fiber is yellow and transparent and has good optical quality.

[0066] Example 6

[0067] Growth of Yb by Laser Heating Susceptor 0.1 La 0.9 ScO3 (x is 0.05) single crystal optical fiber

[0068] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1). Step (1) in this embodiment is: According to the stoichiometric ratio in the chemical reaction equation 0.05Yb2O3+0.45La2O3+0.5Sc2O3→Yb 0.1 La 0.9 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Nd2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The other steps are consistent with the embodiment, and finally a transparent, colorless, optically good Yb 0.1 La 0.9 ScO3 single crystal optical fiber.

[0069] After measurement, the Yb 0.1 La 0.9 The diameter of the ScO3 single crystal fiber is 0.5 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, and the length is 80 mm. The single crystal fiber is transparent and colorless with good optical quality.

[0070] Example 7

[0071] Growth of Nd by Laser Heating Susceptor 0.04 La 0.96 ScO3 (x is 0.02) single crystal optical fiber

[0072] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1) and step (7). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.02Nd2O3+0.48La2O3+0.5Sc2O3→Nd 0.04 La 0.96 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Nd2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The difference in step (5) of this embodiment is that the pulling speed during the equal diameter growth process is 20mm / h and the feeding speed is 10mm / h; the other steps are kept consistent with the embodiment, and finally a blue transparent Nd2O3 with good optical quality is obtained. 0.04 La 0.96 ScO3 single crystal optical fiber.

[0073] After measurement, the obtained Nd 0.04 La 0.96 The diameter of the ScO3 single crystal fiber is 0.7 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, the length is 35 mm, the single crystal fiber is blue and transparent and has good optical quality.

[0074] Example 8

[0075] Growth of Er by Laser Heating Substrate 0.14 La 0.86 ScO3 (x is 0.07) single crystal optical fiber

[0076] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.07Er2O3+0.43La2O3+0.5Sc2O3→Er 0.14 La 0.86 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Er2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The other steps are kept consistent with the embodiment, and finally a pink transparent Er2O3 with good optical quality is obtained. 0.14 La 0.86 ScO3 single crystal optical fiber.

[0077] After measurement, the obtained Er 0.14 La 0.86The diameter of the ScO3 single crystal fiber is 0.5 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, the length is 70 mm, the single crystal fiber is pink and transparent and has good optical quality.

[0078] Example 9

[0079] Growth of Tm by Laser Heating Susceptor 0.1 La 0.9 ScO3 (x is 0.05) single crystal optical fiber

[0080] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.05Tm2O3+0.45La2O3+0.5Sc2O3→Tm 0.1 La 0.9 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Tm2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The other steps are consistent with the embodiment, and finally a transparent, colorless, optically good Tm 0.1 La 0.9 ScO3 single crystal optical fiber.

[0081] After measurement, the obtained Tm 0.1 La 0.9 The diameter of the ScO3 single crystal fiber is 0.5 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, and the length is 90 mm. The single crystal fiber is transparent and colorless with good optical quality.

[0082] Example 10

[0083] Growth of Ho by Laser Heating Substrate 0.03 La 0.97 SCO3 0.015 La 0.985 ScO3 (x is 0.015) single crystal optical fiber

[0084] The preparation of the single crystal optical fiber in this embodiment refers to that in embodiment 1, except for step (1). Step (1) in this embodiment is: according to the stoichiometric ratio in the chemical reaction equation 0.015Ho2O3+0.485La2O3+0.5Sc2O3→Ho 0.03 La 0.97 ScO3 accurately weighs Sc2O3 powder, La2O3 powder and Ho2O3 powder with a purity of 99.99% as raw materials, and the total weight weighed is 20g. The other steps are consistent with the embodiment, and finally yellow transparent Ho2O3 with good optical quality is obtained. 0.03 La 0.97 ScO3 single crystal optical fiber.

[0085] After measurement, the Ho 0.03 La 0.97 The diameter of the ScO3 single crystal fiber is 0.5 mm, the crystal diameter fluctuation of the equal diameter part is less than 5%, the length is 110 mm, the single crystal fiber is yellow and transparent and has good optical quality.

Claims

1. A rare earth ion-doped lanthanum scandate laser single crystal fiber, characterized in that: The chemical formula of the single crystal optical fiber is Re 2x La 1-2x ScO3, where Re is Yb 3+ 、Nd 3+ , Er 3+ 、Tm 3+ 、Ho 3+ One of the rare earth ions, x is a rare earth ion replacing La 3+ The molar percentage of the lattice site; when Re is Yb 3+ When Re is Nd 3+ When 0.005≤x≤0.02; when Re is Er 3+ When Re is Tm 3+ When 0.005≤x≤0.05, Ho 3+ When 0.005≤x≤0.

015.

2. The rare earth ion-doped magnesium lanthanum strontium aluminate laser single crystal fiber according to claim 1, characterized in that: The single crystal optical fiber belongs to the orthorhombic crystal system, and has a diameter of 0.4 to 1 mm and a length of 10 to 120 mm.

3. A method for preparing the rare earth ion-doped lanthanum scandate laser single crystal fiber as claimed in claim 1 or 2, characterized in that: The laser heating base method is adopted, which specifically includes the following steps: (1) Using Yb2O3 powder / Nd2O3 powder / Er2O3 powder / Tm2O3 powder / Ho2O3 powder, La2O3 powder, and Sc2O3 powder with a purity of 99.99% as raw materials, according to the molecular formula Re 2x La 1-2x Weigh each raw material according to the stoichiometric ratio of the corresponding elements in ScO3; where x is the rare earth ion replacing La 3+ The molar percentage of the lattice site is 3+ When 0.005≤x≤0.05; Re is Nd 3+ When 0.005≤x≤0.02; Re is Er 3+ When 0.01≤x≤0.07; Re is Tm 3+ When 0.005≤x≤0.05, Ho 3 + When 0.005≤x≤0.015; (2) The weighed raw materials are mixed uniformly, pressed into cylindrical rods by cold isostatic pressing at 200-300 MPa for 180-300 seconds, sintered in a muffle furnace in an air atmosphere to obtain ceramic rods, the sintering temperature is 1600-1650° C., the sintering time is 15-24 hours, cut into ceramic rods with a diameter of 1-2 mm by wire cutting, and dried at room temperature for 4-8 hours to obtain material rods, which are used as seed crystals and source rods (11) respectively; (3) Cleaning the cavity of the laser substrate heating furnace for crystal growth and the reflective conical mirror (4), the annular plane reflective mirror (5) and the focusing mirror (8) in the optical system, and adjusting the optical path to be uniform; fixing the prepared source rod (11) on the lower feeding device (6), and fixing the prepared seed crystal on the upper pulling device (7); (4) Turn on the CO2 laser (1), adjust the center of the source rod (11) to be placed at the focal center of the laser, melt the top of the source rod (11) into a hemispherical melt (10), adjust the position of the seed crystal so that the seed crystal contacts the melt (10) and is located at the center of the hemispherical melt (10), then slowly contact the seed crystal with the hemispherical melt (10), maintain the state for at least 2 minutes to allow the molten zone to reach stability, start pulling the seed crystal through the pulling device (7) and start the feeding device (6) to raise the source rod (11), and after sequentially going through shoulder release and equal diameter growth, when the grown crystal (9) reaches the required length, close the feeding device (6) and lift the crystal off; (5) The obtained crystal is fixed on the feeding device (6) as a source rod again, and secondary growth is performed according to the above steps (3) and (4) to obtain a longer and thinner single crystal optical fiber; (6) After the single crystal fiber is pulled off, the laser power is reduced at a rate of 0.02-0.05 W / s. After turning off the CO2 laser (1), flowing air is allowed to flow. After 5-15 minutes, the crystal growth chamber is opened and the crystal is removed to obtain Re 2x La 1-2x ScO3 single crystal optical fiber.

4. The method for preparing a rare earth ion-doped lanthanum scandate laser single crystal fiber according to claim 3, characterized in that: In step (2), the cross section of the source rod (11) is (1-2)×(1-2) mm. 2 , length is 50~120mm.

5. The method for preparing a rare earth ion-doped lanthanum scandate laser single crystal fiber according to claim 3 or 4, characterized in that: In steps (4) and (5), the cross section of the prepared single crystal optical fiber is (0.4-1)×(0.4-1) mm 2 , length is 20~120mm.

6. The method for preparing a rare earth ion-doped lanthanum scandate laser single crystal fiber according to claim 3 or 4, characterized in that: In step (4), the power at the center of the laser heating source rod (11) is 25 to 50 W, and the heating time is 2 to 5 minutes.

7. The method for preparing a rare earth ion-doped lanthanum scandate laser single crystal fiber according to claim 3 or 4, characterized in that: In step (5), the power at the center of the laser heating source rod (11) is 10 to 25 W, and the heating time is 1 to 3 minutes.

8. The method for preparing a rare earth ion-doped lanthanum scandate laser single crystal fiber according to claim 3 or 4, characterized in that: In step (4), the parameters of the equal-diameter growth include: a pulling speed of 10 to 20 mm / h; a feeding speed of 10 to 20 mm / h; a power at the laser center of 25 to 50 W; and a growth time of 2 to 6 hours.

9. The method for preparing a rare earth ion-doped lanthanum scandate laser single crystal fiber according to claim 3 or 4, characterized in that: In step (5), the parameters of the equal-diameter growth include: a pulling speed of 30 to 60 mm / h; a feeding speed of 10 to 20 mm / h; a power at the laser center of 10 to 25 W; and a growth time of 2 to 6 hours.

10. The method for preparing a rare earth ion-doped lanthanum scandate laser single crystal fiber according to claim 3 or 4, characterized in that: In step (6), the crystal is taken out and then placed in a muffle furnace for high temperature annealing at 1450-1500° C. for 24 hours in a hydrogen atmosphere.

Citation Information

Cited By

  • Lanthanum-aluminum single crystal as well as preparation method and application thereof

    CN119843367A