Nylon 66 industrial filament for automobile air bag and preparation method of nylon 66 industrial filament
By introducing modified silane coupling agents and silicon carbide micro powder into nylon 66 industrial filaments, the problems of insufficient flame retardancy, oxidation resistance and wear resistance were solved, and high-performance nylon 66 industrial filaments for automotive airbags were prepared.
Patent Information
- Application Number
- CN202411286762.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-15
AI Technical Summary
Existing nylon 66 industrial filaments have insufficient flame retardancy, oxidation resistance, and abrasion resistance in automotive airbags, failing to meet customers' diverse needs.
Using nylon 66 and polyester as base raw materials, modified silane coupling agents and silicon carbide micro powders are introduced to prepare nylon 66 industrial filaments through a specific process. The modified silane coupling agent reacts with catechin and phosphoric acid to form modified phosphoric acid, which improves the antioxidant properties. The phosphoric acid groups decompose at high temperatures to produce flame-retardant gases. The modified silane coupling agent forms a chemical bond with the silicon carbide micro powder, which enhances the adhesion and improves the flame retardant properties and wear resistance.
The prepared nylon 66 industrial filament has excellent antioxidant properties, flame retardant properties and wear resistance, which meet the application requirements of automotive airbags.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthetic fiber production, and specifically relates to nylon 66 industrial filament for automobile airbags and a preparation method thereof. Background Art
[0002] Nylon 66, commonly known as nylon 66, is an industrial nylon 66 filament mainly used in the field of automotive airbags. With the rapid development of the automotive industry in recent years, the demand for airbag yarns has also been expanding. Conventional nylon 66 industrial filaments cannot meet the differentiated needs of customers due to their limited functions.
[0003] The patent with application number CN201510071908.6 provides a production process of nylon yarn, including raw material processing, drying, POY yarn manufacturing, DTY yarn manufacturing, network processing and graded packaging. Antioxidants, antistatic agents and antibacterial agents are added to the raw materials of the invention to improve the performance of nylon 66 finished products, so that the produced nylon yarn has antibacterial and antistatic effects. Dyeing agents are also added to the raw materials to improve the dyeing performance of the finished products. However, various raw materials are prepared into nylon yarn by simple mixing, melting and spinning. Various functional raw materials are not well combined with nylon 66. Nylon yarn is easy to fail and has no flame retardancy, which poses a safety hazard when used in automobile airbags; The patent with application number CN201210079670.8 provides a coated fabric for airbags and a production method thereof. The filaments constituting the fabric of the invention are circular cross-section nylon 66 filaments with a fineness between 280-420dtex, the tensile strength of the filaments is above 9.5cN / dtex, and the fabric has a coating layer with a coating amount of 5-10g / m 2 The resin of the invention has the characteristics of light weight, high tensile strength, good flame retardancy and low air permeability. However, it lacks wear resistance when used for airbags and is easily oxidized when waiting to be used, causing the performance of the airbag to deteriorate and affecting the use effect.
[0004] Therefore, it is necessary to develop a nylon 66 industrial filament for automobile airbags that is flame retardant, antioxidant, wear-resistant, and has excellent mechanical properties. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a nylon 66 industrial filament for automobile airbags. Compared with the traditional process, the nylon 66 industrial filament for automobile airbags provided by the present invention has the characteristics of flame retardancy, oxidation resistance, wear resistance, excellent mechanical properties, etc., and can meet its application requirements in automobile airbags. The present invention also provides a preparation method of the nylon 66 industrial filament for automobile airbags.
[0006] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0007] A nylon 66 industrial filament for automobile airbags comprises the following raw materials in parts by weight: 90-95 parts of nylon 66, 80-85 parts of polyester, 10-15 parts of modified silane coupling agent, 8-12 parts of silicon carbide micropowder, 5-10 parts of catalyst, and 5-10 parts of dispersant; the preparation method of the modified silane coupling agent is as follows:
[0008] Step S1, dissolving catechin, phosphoric acid and sodium acetate in N,N-dimethylformamide at 70-80° C. with stirring, reacting for 8-10 hours, cooling to room temperature, and removing the solvent to obtain modified phosphoric acid;
[0009] Step S2, dissolving the silane coupling agent KH-550 in tetrahydrofuran under stirring conditions, adding triethylamine in an ice-water bath at -3-5°C, mixing evenly, then adding modified phosphoric acid, stirring evenly and reacting for 4-8 hours, naturally returning to room temperature, and removing the solvent to obtain a modified silane coupling agent.
[0010] Furthermore, the dispersant is vinyl bisstearamide and the catalyst is sodium silicate.
[0011] Furthermore, in step S1, the mass ratio of catechin, phosphoric acid and sodium acetate is 10:3-6:0.5-2, and the amount of catechin added to N,N-dimethylformamide is 5-10 g / 100 mL.
[0012] Furthermore, in step S2, the amount of silane coupling agent KH-550 added to tetrahydrofuran is 40-50 g / 100 mL, and the mass ratio of silane coupling agent KH-550, modified phosphoric acid and triethylamine is 20:4-8:3-10.
[0013] The present invention also provides a method for preparing nylon 66 industrial filament for automobile airbags, comprising the following steps:
[0014] (1) Prepare the following components by weight: 90-95 parts of nylon 66, 80-85 parts of polyester, 10-15 parts of modified silane coupling agent, 8-12 parts of silicon carbide powder, 5-10 parts of catalyst, and 5-10 parts of dispersant;
[0015] (2) adding toluene, silicon carbide powder and modified silane coupling agent into a reactor, heating to 80-90° C. under N2 atmosphere and stirring, reacting for 5-7 hours, and obtaining silane-modified silicon carbide after vacuum filtration, ultrasonic dispersion, centrifugal washing, drying, crushing and sieving;
[0016] (3) adding nylon 66, polyester, silane-modified silicon carbide, a catalyst, and a dispersant into a heating device of a spinning machine according to a proportion, and heating and melting them;
[0017] (4) spinning the product obtained in step (3) through a spinning machine at 0.2-0.5 MPa to form filaments;
[0018] (5) The filaments obtained in step (4) are stretched in a stretching machine, cooled, and naturally solidified to obtain a filament.
[0019] Furthermore, the particle size of the silicon carbide powder in step (1) is ≤10.0 μm.
[0020] Furthermore, the cooling in step (5) adopts side-blowing cooling, the blowing air temperature is 20-30° C., and the cooling air speed is 0.3-0.5 m / s.
[0021] The present invention has the following beneficial effects:
[0022] The present invention uses nylon 66 and polyester as basic raw materials, and introduces silane-modified silicon carbide and other raw materials to prepare nylon 66 industrial filaments with excellent performance. The preparation of the modified silane coupling agent in the present invention is firstly to obtain modified phosphoric acid by esterification reaction of hydroxyl groups in catechins with phosphoric acid. The modified phosphoric acid structure contains catechin groups and phosphoric acid groups, wherein the catechin groups have multiple phenolic hydroxyl groups, which are easily oxidized to quinones to provide H + Therefore, the modified phosphoric acid containing catechin groups has significant antioxidant activity; wherein the phosphoric acid group is decomposed by heat to produce strong acids with water absorption or dehydration effects, such as polyphosphoric acid, pyrophosphoric acid, etc., which promote the dehydration and carbonization of the polymer to form a non-flammable carbon layer with a certain thickness, which separates the polymer from oxygen and heat sources, prevents the transfer of heat, and blocks the combustion. In addition, the phosphoric acid group decomposes at high temperature to produce flame-retardant or non-flammable gas, which can dilute the concentration of combustible gas and oxygen content around the polymer, form a gas protection layer around the polymer, and take away a large amount of heat at the same time, thereby inhibiting combustion and further improving the flame retardant properties of the polymer material; and then the modified phosphoric acid is introduced into the structure of the silane coupling agent KH-550 through the reaction of hydroxyl and amino groups to obtain a modified silane coupling agent, which contains two different active groups, amino and ethoxy, and can be used to couple the polymer and the inorganic filler, enhance the adhesion between the polymer and the inorganic filler, give full play to the reinforcing effect of the inorganic filler, and thus significantly improve the wear resistance and mechanical properties of the composite material. The present invention utilizes a modified silane coupling agent to modify silicon carbide powder to obtain silane-modified silicon carbide, and then uses nylon 66, polyester, silane-modified silicon carbide and the like as raw materials, controls the process, forms a chemical bond between the silicon carbide powder and other raw materials, realizes uniform dispersion of the silicon carbide powder in the composite material, and the components of the raw materials interact with each other and synergize to enhance the effect. The prepared nylon 66 industrial filament has excellent antioxidant properties, flame retardant properties, mechanical properties and wear resistance, meets the application requirements of automobile airbags, and has broad prospects. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0024] Nylon 66 was purchased from Ningbo Xinmin Import and Export Co., Ltd., with a brand name of A3WG7; polyester was purchased from Yuyao Kaimaigao Plastic Technology Co., Ltd., with a brand name of Kaimaigao; silicon carbide micropowder was purchased from Hebei Wenlun Metal Materials Co., Ltd., with a particle size of ≤10 μm and a brand name of 66556; sodium silicate was purchased from Shandong No. 1 Chemical Group Co., Ltd., with a particle size of 80 mesh and a brand name of No. 1. The raw materials used in the following examples are all common commercially available products.
[0025] Example 1
[0026] A nylon 66 industrial filament for automobile airbags, comprising the following raw materials in parts by weight: 90 parts of nylon 66, 80 parts of polyester, 10 parts of modified silane coupling agent, 8 parts of silicon carbide micropowder, 5 parts of catalyst, and 5 parts of dispersant;
[0027] The preparation method of the modified silane coupling agent is as follows:
[0028] Step S1, dissolving 10 g of catechin, 3 g of phosphoric acid and 0.5 g of sodium acetate in 200 mL of N,N-dimethylformamide at 70° C. with stirring, reacting for 8 h, and naturally cooling to room temperature to obtain a mixed solution, and removing N,N-dimethylformamide from the mixed solution by rotary evaporation at 80° C. to obtain modified phosphoric acid;
[0029] Step S2, dissolving 20 g of silane coupling agent KH-550 in 50 mL of tetrahydrofuran under stirring, adding 3 g of triethylamine in an ice-water bath at -3-5°C, mixing evenly, then adding 4 g of modified phosphoric acid, stirring evenly and reacting for 4 h, naturally returning to room temperature, and removing tetrahydrofuran by reduced pressure distillation to obtain a modified silane coupling agent;
[0030] The dispersant is vinyl bisstearamide and the catalyst is sodium silicate.
[0031] A method for preparing nylon 66 industrial filament for automobile airbags comprises the following steps:
[0032] (1) Prepare the following components by weight: 6690 parts of nylon, 80 parts of polyester, 10 parts of modified silane coupling agent, 8 parts of silicon carbide powder, 5 parts of catalyst, and 5 parts of dispersant;
[0033] (2) Add toluene (the mass ratio of toluene to silicon carbide powder is 90:8), silicon carbide powder and modified silane coupling agent into the reactor, heat to 80°C under N2 atmosphere and stirring conditions, react for 5 hours, vacuum filter, use acetone and deionized water for ultrasonic dispersion and centrifugal washing, then dry in an oven at 100°C for 10 hours, cool to room temperature, crush and sieve to obtain silane-modified silicon carbide, the particle size of silane-modified silicon carbide is ≤14.1 μm; wherein, the ultrasonic frequency is 40 kHz, the ultrasonic time is 30 min, the centrifugal speed is 12000 rpm, and the centrifugal time is 10 min;
[0034] (3) adding nylon 66, polyester, silane-modified silicon carbide, a catalyst, and a dispersant into a heating device of a spinning machine according to a proportion, and heating and melting them at 250° C.;
[0035] (4) the product obtained in step (3) is passed through a spinning machine with a spinneret number of ≤150 holes under a condition of 0.2-0.5 MPa to form filaments;
[0036] (5) The filament obtained in step (4) is stretched in a stretching machine with a stretching multiple of 2 and a stretching speed of 800 rpm, cooled by side blowing, the blowing air temperature is 20° C., the cooling air speed is 0.3 m / s, and naturally solidified to obtain a nylon 66 industrial filament with a single yarn density of ≤20 dtex.
[0037] Example 2
[0038] A nylon 66 industrial filament for automobile airbags, comprising the following raw materials in parts by weight: 95 parts of nylon 66, 85 parts of polyester, 15 parts of modified silane coupling agent, 12 parts of silicon carbide micropowder, 10 parts of catalyst, and 10 parts of dispersant;
[0039] The preparation method of the modified silane coupling agent is as follows:
[0040] Step S1, dissolving 10 g of catechin, 6 g of phosphoric acid and 2 g of sodium acetate in 100 mL of N,N-dimethylformamide at 80° C. with stirring, reacting for 10 h, and naturally cooling to room temperature to obtain a mixed solution, and removing N,N-dimethylformamide from the mixed solution by rotary evaporation at 80° C. to obtain modified phosphoric acid;
[0041] Step S2, dissolving 20 g of silane coupling agent KH-550 in 40 mL of tetrahydrofuran under stirring conditions, adding 10 g of triethylamine in an ice-water bath at -3-5°C, mixing evenly, then adding 8 g of modified phosphoric acid, stirring evenly and reacting for 8 h, naturally returning to room temperature, and removing tetrahydrofuran by reduced pressure distillation to obtain a modified silane coupling agent;
[0042] The dispersant is vinyl bisstearamide and the catalyst is sodium silicate.
[0043] A method for preparing nylon 66 industrial filament for automobile airbags comprises the following steps:
[0044] (1) Prepare the following components by weight: 6695 parts of nylon, 85 parts of polyester, 15 parts of modified silane coupling agent, 12 parts of silicon carbide powder, 10 parts of catalyst, and 10 parts of dispersant;
[0045] (2) Add toluene (the mass ratio of toluene to silicon carbide powder is 90:8), silicon carbide powder and modified silane coupling agent into the reactor, heat to 90°C under N2 atmosphere and stirring conditions, react for 7 hours, vacuum filter, use acetone and deionized water for ultrasonic dispersion and centrifugal washing, and then dry in an oven at 110°C for 14 hours, cool to room temperature, crush and sieve to obtain silane-modified silicon carbide, the particle size of silane-modified silicon carbide is ≤12.3 μm; wherein, the ultrasonic frequency is 40 kHz, the ultrasonic time is 30 min, the centrifugal speed is 12000 rpm, and the centrifugal time is 10 min;
[0046] (3) adding nylon 66, polyester, silane-modified silicon carbide, a catalyst, and a dispersant into a heating device of a spinning machine according to a proportion, and heating and melting them at 290° C.;
[0047] (4) the product obtained in step (3) is passed through a spinning machine with a spinneret number of ≤150 holes under a condition of 0.2-0.5 MPa to form filaments;
[0048] (5) The filament obtained in step (4) is stretched in a stretching machine with a stretching multiple of 2 and a stretching speed of 800 rpm, cooled by side blowing, the blowing air temperature is 30° C., the cooling air speed is 0.5 m / s, and naturally solidified to obtain a nylon 66 industrial filament with a single yarn density of ≤20 dtex.
[0049] Example 3
[0050] A nylon 66 industrial filament for automobile airbags, comprising the following raw materials in parts by weight: 92 parts of nylon 66, 83 parts of polyester, 12 parts of modified silane coupling agent, 10 parts of silicon carbide micropowder, 8 parts of catalyst, and 7 parts of dispersant;
[0051] The preparation method of the modified silane coupling agent is as follows:
[0052] Step S1, dissolving 10 g of catechin, 5 g of phosphoric acid and 1 g of sodium acetate in 150 mL of N,N-dimethylformamide at 75° C. with stirring, reacting for 9 h, and naturally cooling to room temperature to obtain a mixed solution, and removing N,N-dimethylformamide from the mixed solution by rotary evaporation at 80° C. to obtain modified phosphoric acid;
[0053] Step S2, dissolving 20 g of silane coupling agent KH-550 in 44.44 mL of tetrahydrofuran under stirring conditions, adding 5 g of triethylamine in an ice-water bath at -3-5°C, mixing evenly, then adding 6 g of modified phosphoric acid, stirring evenly and reacting for 6 h, naturally returning to room temperature, and removing tetrahydrofuran by reduced pressure distillation to obtain a modified silane coupling agent;
[0054] The dispersant is vinyl bisstearamide and the catalyst is sodium silicate.
[0055] A method for preparing nylon 66 industrial filament for automobile airbags comprises the following steps:
[0056] (1) Prepare the following components by weight: 6692 parts of nylon, 83 parts of polyester, 12 parts of modified silane coupling agent, 10 parts of silicon carbide powder, 8 parts of catalyst, and 7 parts of dispersant;
[0057] (2) Add toluene (the mass ratio of toluene to silicon carbide powder is 90:8), silicon carbide powder and modified silane coupling agent into the reactor, heat to 85°C under N2 atmosphere and stirring conditions, react for 6 hours, vacuum filter, use acetone and deionized water for ultrasonic dispersion and centrifugal washing, and then dry in an oven at 105°C for 12 hours, cool to room temperature, crush and sieve to obtain silane-modified silicon carbide, the particle size of silane-modified silicon carbide is ≤13.5 μm; wherein, the ultrasonic frequency is 40 kHz, the ultrasonic time is 30 min, the centrifugal speed is 12000 rpm, and the centrifugal time is 10 min;
[0058] (3) adding nylon 66, polyester, modified silane coupling agent, catalyst, and dispersant into a heating device of a spinning machine according to a proportion, and heating and melting at 270° C.;
[0059] (4) the product obtained in step (3) is passed through a spinning machine with a spinneret number of ≤150 holes under a condition of 0.2-0.5 MPa to form filaments;
[0060] (5) The filament obtained in step (4) is stretched in a stretching machine with a stretching multiple of 2 and a stretching speed of 800 rpm, cooled by side blowing, the blowing air temperature is 25° C., the cooling air speed is 0.4 m / s, and naturally solidified to obtain a nylon 66 industrial filament with a single yarn linear density of ≤20 dtex.
[0061] Comparative Example 1
[0062] A nylon 66 industrial filament for automobile airbags, comprising the following raw materials in parts by weight: 80 parts of nylon 66, 83 parts of polyester, 5 parts of flame retardant modified silane coupling agent, 10 parts of silicon carbide, 5 parts of catalyst, and 5 parts of dispersant;
[0063] The preparation method of the flame retardant modified silane coupling agent is as follows: 20g of silane coupling agent KH-550 is dissolved in 50mL of tetrahydrofuran under stirring, 3g of triethylamine is first added in an ice water bath at -3-5°C, mixed evenly, and then 6g of phosphoric acid is added, stirred evenly and reacted for 6h, naturally restored to room temperature, and tetrahydrofuran is removed by reduced pressure distillation to obtain a flame retardant modified silane coupling agent;
[0064] The dispersant is vinyl bisstearamide and the catalyst is sodium silicate.
[0065] A method for preparing nylon 66 industrial filament for automobile airbags comprises the following steps:
[0066] (1) Prepare the following components by weight: 6680 parts of nylon, 83 parts of polyester, 5 parts of flame retardant modified silane coupling agent, 10 parts of silicon carbide, 5 parts of catalyst, and 5 parts of dispersant;
[0067] (2) Add toluene (the mass ratio of toluene to silicon carbide powder is 90:8), silicon carbide powder and modified silane coupling agent into the reactor, heat to 70°C under N2 atmosphere and stirring conditions, react for 3 hours, vacuum filter, use acetone and deionized water for ultrasonic dispersion and centrifugal washing, then dry in an oven at 80°C for 12 hours, cool to room temperature, crush and sieve to obtain silane-modified silicon carbide, the particle size of silane-modified silicon carbide is ≤11.6 μm; wherein, the ultrasonic frequency is 40 kHz, the ultrasonic time is 30 min, the centrifugal speed is 12000 rpm, and the centrifugal time is 10 min;
[0068] (3) adding nylon 66, polyester, modified silicon carbide, catalyst, and dispersant into a heating device of a spinning machine according to a certain ratio, and heating and melting them at 290° C.;
[0069] (4) the product obtained in step (3) is passed through a spinning machine with a spinneret number of ≤150 holes under a condition of 0.2-0.5 MPa to form filaments;
[0070] (5) The filament obtained in step (4) is stretched in a stretching machine with a stretching multiple of 2 and a stretching speed of 800 rpm, cooled by side blowing, the blowing air temperature is 20° C., the cooling air speed is 0.3 m / s, and naturally solidified to obtain a nylon 66 industrial filament with a single yarn density of ≤20 dtex.
[0071] Comparative Example 2
[0072] A nylon 66 industrial filament for automobile airbags, comprising the following raw materials in parts by weight: 80 parts of nylon 66, 80 parts of polyester, 20 parts of silane coupling agent, 5 parts of silicon carbide micropowder, 6 parts of catalyst, and 5 parts of dispersant;
[0073] The dispersant is vinyl bisstearamide and the catalyst is sodium silicate.
[0074] A method for preparing nylon 66 industrial filament for automobile airbags comprises the following steps:
[0075] (1) Prepare the following components by weight: 6680 parts of nylon, 80 parts of polyester, 20 parts of silane coupling agent, 5 parts of silicon carbide powder, 6 parts of catalyst, and 5 parts of dispersant;
[0076] (2) adding nylon 66, polyester, silane coupling agent, silicon carbide powder, catalyst, and dispersant into a heating device of a spinning machine according to a certain ratio, and heating and melting them at 230° C.;
[0077] (3) the product obtained in step (2) is passed through a spinning machine with a spinneret number of ≤150 holes under a condition of 0.2-0.5 MPa to form filaments;
[0078] (4) The filament obtained in step (3) is stretched in a stretching machine with a stretching multiple of 2 and a stretching speed of 800 rpm, cooled by side blowing, the blowing air temperature is 20° C., the cooling air speed is 0.3 m / s, and naturally solidified to obtain a nylon 66 industrial filament with a single yarn density of ≤20 dtex.
[0079] The properties of the nylon 66 industrial filaments for automobile airbags prepared in Examples 1-3 and Comparative Examples 1-2 were tested. The test method is as follows. The test results are shown in Table 1 below.
[0080] (1) Mechanical properties
[0081] The YG023B-III single yarn strength machine was used for testing in accordance with GB / T14344-2022 “Test method for tensile properties of chemical fiber filaments”.
[0082] (2) Oxygen index value
[0083] The oxygen index value is the minimum oxygen concentration for the filament sample to maintain combustion in a mixed atmosphere of O2 and N2, expressed as volume percentage. According to the international standard ASTMD2863, the calculation formula is oxygen concentration % = oxygen flow rate / (oxygen flow rate + nitrogen flow rate) × 100%.
[0084] (3) Antioxidant
[0085] First, weigh 2.5 mg of 2,2-diphenyl-1-picrylhydrazyl (DPPH), dissolve it in an appropriate amount of anhydrous ethanol, and make up to 100 mL to obtain a DPPH ethanol solution with a concentration of 25.0 mg / L. Mix 1 g of the filament sample with 2 mL of the DPPH solution and let it stand in the dark for 10 min to obtain the test group; mix 1 g of the filament sample with 2 mL of anhydrous ethanol to obtain the control group 1; mix 2 mL of the DPPH ethanol solution with 1.0 mL of the ethanol solution to obtain the control group 2. Use a spectrophotometer to measure the absorbance of the test solution and calculate the antioxidant capacity of the fiber.
[0086] The calculation formula is as follows: P = [A0 - (A1 - A2)] / A0 × 100%, where P is the free radical scavenging rate, A0 is the absorbance value of the control group 2, A1 is the absorbance value of the test group, and A2 is the absorbance of the control group 1.
[0087] (4) Wear resistance
[0088] With reference to FZ / T01058-1999, the filament samples were tested for wear resistance by a reciprocating wear tester. The tension weight used was 35g, the water sandpaper was No. 400, and it was rotated continuously at a speed of 75m / min. The number of frictions when it broke was recorded to evaluate its wear resistance.
[0089] Table 1 Mechanical properties, oxygen index, oxidation resistance and wear resistance test of nylon 66 industrial filament used for automobile airbags
[0090] sample Breaking strength (cN / dtex) Elongation at break (%) Oxygen index value (%) Antioxidant activity (%) Wear resistance (times) Example 1 9.6 58 38 30.5 8600 Example 2 10.3 60 38 33.8 8500 Example 3 9.5 53 36 33.7 8500 Comparative Example 1 7.6 43 30 23 8000 Comparative Example 2 6.6 41 25 23.6 7900
[0091] As can be seen from Table 1, compared with Comparative Examples 1-2, the nylon 66 industrial filaments for automobile airbags prepared in Examples 1-3 have excellent mechanical properties and wear resistance, high oxygen index value and good antioxidant performance, among which Example 2 has the best comprehensive performance; compared with Comparative Example 2, the use of flame retardant modified silane coupling agent in Comparative Example 1 improves the oxygen index value of nylon 66 industrial filaments for automobile airbags; Comparative Example 2 only adds silane coupling agent KH-550, and the mechanical properties, oxygen index value, antioxidant and wear resistance are not ideal.
[0092] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0093] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A nylon 66 industrial filament for automobile airbags, characterized in that: The invention comprises the following raw materials in parts by weight: 90-95 parts of nylon 66, 80-85 parts of polyester, 10-15 parts of modified silane coupling agent, 8-12 parts of silicon carbide micropowder, 5-10 parts of catalyst, and 5-10 parts of dispersant; the preparation method of the modified silane coupling agent is as follows: Step S1, dissolving catechin, phosphoric acid and sodium acetate in N,N-dimethylformamide at 70-80° C. with stirring, reacting for 8-10 hours, cooling to room temperature, and removing the solvent to obtain modified phosphoric acid; Step S2, dissolving the silane coupling agent KH-550 in tetrahydrofuran under stirring conditions, adding triethylamine in an ice-water bath at -3-5°C, mixing evenly, then adding modified phosphoric acid, stirring evenly and reacting for 4-8 hours, naturally returning to room temperature, and removing the solvent to obtain a modified silane coupling agent.
2. The nylon 66 industrial filament for automobile airbags according to claim 1, characterized in that: The dispersant is vinyl bisstearamide, and the catalyst is sodium silicate.
3. The nylon 66 industrial filament for automobile airbags according to claim 1, characterized in that: In step S1, the mass ratio of catechin, phosphoric acid and sodium acetate is 10:3-6:0.5-2, and the amount of catechin added to N,N-dimethylformamide is 5-10 g / 100 mL.
4. The nylon 66 industrial filament for automobile airbags according to claim 1, characterized in that: The amount of silane coupling agent KH-550 added to tetrahydrofuran in step S2 is 40-50 g / 100 mL, and the mass ratio of silane coupling agent KH-550, modified phosphoric acid and triethylamine is 20:4-8:3-10.
5. The method for preparing nylon 66 industrial filament for automobile airbags according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Prepare the following components by weight: 90-95 parts of nylon 66, 80-85 parts of polyester, 10-15 parts of modified silane coupling agent, 8-12 parts of silicon carbide powder, 5-10 parts of catalyst, and 5-10 parts of dispersant; (2) adding toluene, silicon carbide powder and modified silane coupling agent into a reactor, heating to 80-90° C. under N2 atmosphere and stirring, reacting for 5-7 hours, and obtaining silane-modified silicon carbide after vacuum filtration, ultrasonic dispersion, centrifugal washing, drying, crushing and sieving; (3) adding nylon 66, polyester, silane-modified silicon carbide, a catalyst, and a dispersant into a heating device of a spinning machine according to a proportion, and heating and melting them; (4) the product obtained in step (3) is passed through a spinning machine under a condition of 0.2-0.5 MPa to form filaments; (5) The filaments obtained in step (4) are stretched in a stretching machine, cooled, and naturally solidified to obtain a filament.
6. The method for preparing nylon 66 industrial filament for automobile airbags according to claim 5, characterized in that: The particle size of the silicon carbide powder in step (1) is ≤10.0 μm.
7. The method for preparing nylon 66 industrial filament for automobile airbags according to claim 5, characterized in that: The cooling in step (5) is performed by side-blowing cooling, the blowing air temperature is 20-30° C., and the cooling air speed is 0.3-0.5 m / s.
Citation Information
Patent Citations
Coated fabric for safety airbag and production method thereof
CN103321052A
Polyamide yarn production technology
CN104674366A