Mildew-proof antibacterial packaging paper and preparation method thereof

By coating anti-mold coatings with tetrachloroisophthalene, composite quaternary ammonium salt and varnish on the wrapping paper, the problem of mold in the packaging paper in high humidity environment is solved, and stable anti-mold and anti-bacterial effects are achieved. Improves waterproof performance and simplifies the production process.

CN118958034APending Publication Date: 2024-11-15BOA SHEN PAPER & PLASTIC PROD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411202626.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing packaging papers are prone to mold in high humidity environments, and existing anti-mold agents such as salicylic acid aniline, 8-hydroxyquinoline copper and chitosan quaternary ammonium salts have problems with poor stability, solubility or reduced waterproofing ability.

Method used

Using anti-mold coatings including tetrachloroisophthalene, composite quaternary ammonium salt and varnish, an anti-mold coating is formed on the surface of the wrapping paper, and tetrachloroisophthalene destroys the metabolism and composite quaternary of fungal cells. Ammonium salt destroys the cell membrane and combines varnish to form a hydrophobic layer to improve mildew resistance.

Benefits of technology

It achieves long-term and stable anti-mold effect under normal temperature and light environment, enhances the waterproofness and antibacterial ability of the packaging paper, and simplifies the preparation process and facilitates large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118958034A_ABST
    Figure CN118958034A_ABST
Patent Text Reader

Abstract

The invention discloses mildewproof antibacterial packaging paper which comprises raw paper, and a mildewproof coating is formed on the surface of the raw paper by coating a mildewproof coating. The mildew-proof coating comprises the following raw materials in parts by mass: 20-30 parts of a first solvent, 10-20 parts of gloss oil, 3-10 parts of a TPN mildew-proof agent and 0.1-3 parts of composite quaternary ammonium salt, the TPN mildew preventive comprises a second solvent and tetrachloroisophthalonitrile, and the mass ratio of the second solvent to the tetrachloroisophthalonitrile is 100: (1-5). The packaging paper has excellent mildew-proof and antibacterial effects, and the mildew-proof coating is stable and not prone to decomposition and deterioration. The invention further discloses a preparation method of the mildewproof and antibacterial packaging paper, the preparation period is short, and mass production of the mildewproof and antibacterial packaging paper is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of packaging paper, and in particular to mildew-proof and antibacterial packaging paper and a preparation method thereof. Background Art

[0002] In the packaging industry, packaging paper is a widely used material, and its performance stability and durability are directly related to the protection and display effect of products. However, the problem of packaging paper mold has always been a technical challenge faced by this field.

[0003] Wrapping paper includes kraft paper, parchment paper, cellophane and other types. During production and storage, it is easily affected by ambient temperature and humidity. Especially when the ambient humidity exceeds a certain threshold (such as 12% humidity), the wrapping paper will face the risk of mold, so anti-mold agents are usually added to the wrapping paper to prevent mold.

[0004] The mold inhibitors in the prior art mainly include the following: salicylic acid aniline, 8-hydroxyquinoline copper, chitosan quaternary ammonium salt, etc. Among them, salicylic acid aniline will deteriorate or become ineffective in a high temperature environment, and its color will turn yellow and brown under long-term light exposure, and its stability is poor. 8-Hydroxyquinoline copper has a high solubility in strong acids, but a low solubility in other organic solvents and water, making it difficult to apply to packaging paper in the form of a coating. Chitosan quaternary ammonium salt is hygroscopic, and adding it to packaging paper will reduce its waterproof ability.

[0005] In view of this, the present invention provides a mildew-proof and antibacterial packaging paper and a preparation method thereof to solve the above problems. Summary of the invention

[0006] In order to overcome the shortcomings of the above-mentioned technology, the present invention provides a mildew-proof and antibacterial packaging paper, comprising base paper, wherein the surface of the base paper is coated with a mildew-proof coating to form a mildew-proof coating; the mildew-proof coating comprises the following raw materials in parts by mass: 20 to 30 parts of a first solvent, 10 to 20 parts of varnish, 3 to 10 parts of a TPN mildew-proof agent, and 0.1 to 3 parts of a composite quaternary ammonium salt; the TPN mildew-proof agent comprises a second solvent and tetrachloroisophthalonitrile, and the mass ratio of the second solvent to tetrachloroisophthalonitrile is 100:1 to 5.

[0007] Preferably, the anti-mildew paint comprises the following raw materials in parts by mass: 23 to 26 parts of a first solvent, 13 to 16 parts of varnish, 5 to 8 parts of a TPN anti-mildew agent, and 0.8 to 1.5 parts of a complex quaternary ammonium salt.

[0008] Preferably, the first solvent is dry water.

[0009] Preferably, the first solvent comprises the following raw materials in parts by mass: 16 to 40 parts of isopropanol, 20 to 40 parts of ethyl acetate, 20 to 30 parts of ethanol, and 10 to 30 parts of n-butyl acetate.

[0010] Preferably, the second solvent is ethanol.

[0011] Preferably, the mass ratio of the second solvent to tetrachloroisophthalonitrile is 100:1.5-3.

[0012] Preferably, the base paper is coated with 5 to 8 g of anti-mildew coating per square meter.

[0013] Preferably, the varnish is UV varnish.

[0014] To achieve the above object, the present invention further provides a method for preparing mildew-proof and antibacterial packaging paper, which is characterized by comprising the following steps:

[0015] Step 1: prepare a composite quaternary ammonium salt solution;

[0016] Step 2: sequentially adding TPN mildew preventer, composite quaternary ammonium salt solution and the first solvent into the reactor;

[0017] Step 3: Slowly add varnish to the reactor;

[0018] Step 4: stirring the composition in the reactor for 3 to 6 minutes to obtain an anti-mildew coating;

[0019] Step 5: Apply the anti-mildew coating on the surface of the base paper and dry it to obtain the anti-mildew and antibacterial packaging paper.

[0020] Preferably, in step five, the anti-mildew coating base paper is dried by hot air.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The mildew-proof coating of the present invention comprises tetrachloroisophthalonitrile, composite quaternary ammonium salt and varnish. Tetrachloroisophthalonitrile can react with glyceraldehyde-3-phosphate dehydrogenase in fungal cells and combine with protein containing cysteine ​​in the enzyme, thereby destroying the activity of the enzyme, causing the metabolism of the fungal cells to be damaged and lose vitality, thereby achieving the effect of inhibiting mold. Moreover, tetrachloroisophthalonitrile is stable at room temperature, weakly alkaline or weakly acidic medium and in light environment, and can ensure the long-term mildew-proof effect of packaging paper.

[0023] The compound quaternary ammonium salt acts on the cell membrane through the ionic structure, destroying the integrity of the cell membrane, causing the cell to shrink and die, thereby achieving a bactericidal effect. It has a good inhibitory effect on mold and bacteria. In addition, the compound quaternary ammonium salt is stable, non-volatile, and resistant to inorganic salts. At the same time, the compound quaternary ammonium salt is a cationic surfactant. Adding it to the packaging paper can resist static electricity and improve the waterproofness of the packaging paper.

[0024] The varnish is coated on the wrapping paper to form a thin film, making the surface of the wrapping paper smooth and hydrophobic, preventing water vapor from penetrating into the wrapping paper, and further improving the anti-mildew performance of the wrapping paper.

[0025] 2. The first reagent of the present invention is medium dry water, which can make varnish, TPN mildew preventer and composite quaternary ammonium salt evenly dispersed in the medium dry water, and the medium dry water has a certain polarity and can penetrate the wrapping paper, so that tetrachloroisophthalonitrile and composite quaternary ammonium salt penetrate into the wrapping paper, so that the inside of the wrapping paper has mildew-proof effect.

[0026] 3. The preparation method of the mildew-proof and antibacterial packaging paper of the present invention is simple and has a short preparation cycle, which is convenient for mass production of mildew-proof and antibacterial packaging paper. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a graph showing the ASTM G21 mildew resistance test results of Example 1 of the present invention;

[0028] Figure 2 is a graph showing the results of the ASTM G21 mildew resistance test of the base paper of the present invention;

[0029] The implementation, functional features and advantages of the present invention will be further described in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0030] The features of the present invention and other related features are further described in detail below through embodiments to facilitate understanding by those skilled in the art:

[0031] An embodiment of the present invention provides a mildew-proof and antibacterial packaging paper, comprising base paper, wherein a mildew-proof coating is formed on the surface of the base paper by coating a mildew-proof coating; the mildew-proof coating comprises the following raw materials in parts by mass: 20 to 30 parts of a first solvent, 10 to 20 parts of varnish, 3 to 10 parts of a TPN mildew-proof agent, and 0.1 to 3 parts of a composite quaternary ammonium salt; the TPN mildew-proof agent comprises a second solvent and tetrachloroisophthalonitrile, and the mass ratio of the second solvent to tetrachloroisophthalonitrile is 100:1 to 5.

[0032] In some embodiments, the anti-mildew paint comprises the following raw materials in parts by weight: 23 to 26 parts of a first solvent, 13 to 16 parts of varnish, 5 to 8 parts of a TPN anti-mildew agent, and 0.8 to 1.5 parts of a complex quaternary ammonium salt.

[0033] In some embodiments, the first solvent is medium-dry water.

[0034] In some embodiments, the first solvent includes the following raw materials in parts by weight: 16 to 40 parts of isopropanol, 20 to 40 parts of ethyl acetate, 20 to 30 parts of ethanol, and 10 to 30 parts of n-butyl acetate.

[0035] In some embodiments, the second solvent is ethanol.

[0036] In some embodiments, the mass ratio of the second solvent to tetrachloroisophthalonitrile is 100:1.5-3.

[0037] In some embodiments, the base paper is coated with 5 to 8 g of anti-mildew coating per square meter.

[0038] In some embodiments, the varnish is UV varnish.

[0039] The embodiment of the present invention further provides a method for preparing mildew-proof and antibacterial packaging paper, which is characterized by comprising the following steps:

[0040] Step 1: prepare a composite quaternary ammonium salt solution;

[0041] Step 2: sequentially adding TPN mildew preventer, composite quaternary ammonium salt solution and the first solvent into the reactor;

[0042] Step 3: Slowly add varnish to the reactor;

[0043] Step 4: stirring the composition in the reactor for 3 to 6 minutes to obtain an anti-mildew coating;

[0044] Step 5: Apply the anti-mildew coating on the surface of the base paper and dry it to obtain the anti-mildew and antibacterial packaging paper.

[0045] In some embodiments, the anti-mildew coating base paper is dried by hot air.

[0046] Embodiment 1 of the present invention provides a mildew-proof and antibacterial packaging paper, which comprises the following steps:

[0047] Step 1: Add 4 kg of composite quaternary ammonium salt to 6 kg of ethanol to form a composite quaternary ammonium salt solution, numbered AEM3388. Add 0.2 kg of tetrachloroisophthalonitrile to 9.8 kg of ethanol to form a TPN mildew inhibitor.

[0048] Step 2: Add 7.2kg TPN mildew inhibitor, 2.4kg AEM3388 and 24.4kg medium dry water into the mixing barrel in sequence.

[0049] Step 3: Slowly add 14.4kg of varnish into the mixing barrel;

[0050] Step 4: Stir the composition in the mixing bucket for 5 minutes to obtain a mildew-proof coating;

[0051] Step 5: In 1m 2 7g of anti-mildew paint is applied to the base paper, and the base paper is heated with 50-degree hot air to form an anti-mildew coating on the surface of the base paper.

[0052] In Examples 2 to 4 and Comparative Examples 1 to 4, the raw material formula is changed according to Table 2, and the mildew-proof and antibacterial packaging paper of Examples 2 to 10 is prepared according to the preparation method of Example 1. Preparation method of salicylic acid aniline mildew inhibitor: 0.2 kg of salicylic acid aniline is dissolved in 9.8 kg of ethanol. In Comparative Example 1, salicylic acid aniline mildew inhibitor replaces TPN mildew inhibitor in step 2. In Comparative Example 2, chitosan quaternary ammonium salt replaces TPN mildew inhibitor in step 2.

[0053] Table 1 Formulations of Examples and Comparative Examples

[0054]

[0055]

[0056] 1. ASTM G21 mildew resistance test, the test process is as follows.

[0057] 1. Prepare 50mm×50mm square pieces of mildew-proof and antibacterial packaging paper and 50mm×50mm square piece base paper of Examples 1 to 4 and Comparative Examples 1 to 4.

[0058] 2. Prepare a mixed fungal spore suspension of Aspergillus niger, Penicillium pinephilum, Chaetomium globosum, Trichoderma viride and Aureobasidium pullulans.

[0059] 3. Place the packaging paper and base paper on different culture media respectively, and spray the mixed fungal spore suspension evenly on the surface of the packaging paper and culture media. Keep the temperature at 28-30℃ and the relative humidity not less than 85% for 72 hours, and observe the growth of mold on the sample surface.

[0060] 4. Result evaluation: Common mildew prevention grades include: Grade 0: No obvious mildew growth at a magnification of about 50 times. Grade 1: Mildew growth is invisible or difficult to see with the naked eye, but mildew growth can be clearly seen under a magnifying glass and the coverage area is less than 10%. Grade 2: Mildew growth is clearly visible to the naked eye, with a coverage area of ​​10% to 30%. Grade 3: Mildew growth is clearly visible to the naked eye, with a coverage area of ​​30% to 60%. Grade 4: Mildew growth is clearly visible to the naked eye, with a coverage area greater than 60%.

[0061] 2. Water vapor transmission rate test: Water vapor transmission rate is determined by the electrolytic sensor method of GB / T21529-2008 "Plastic film and sheet water vapor transmission rate".

[0062] III. Stability test: 50 mm×50 mm square pieces of mildew-proof and antibacterial packaging paper prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were placed in 40°C air and irradiated with a 300W xenon lamp to simulate visible light for 5 days, and the appearance of the packaging paper was observed. The ASTM G21 mildew-proof test was repeated.

[0063] Table 2 Test results of embodiments and comparative examples

[0064]

[0065] (1) By comparing Examples 1 to 2 with Comparative Example 1, it can be seen that the mildew-proof coating does not contain a composite quaternary ammonium salt, which will significantly affect the mildew-proof and antibacterial effect of the packaging paper. This is because the composite quaternary ammonium salt can act on the cell membrane through the ionic structure, destroy the integrity of the cell membrane, and cause the cells to shrink and die, thereby achieving a bactericidal effect, and has a good inhibitory effect on molds and bacteria. The water vapor permeability of Example 1, Example 2, and Comparative Example 1 increases in turn, which is because the composite quaternary ammonium salt is a cationic surfactant that can improve the waterproofness of the packaging paper.

[0066] (2) By comparing Examples 1 and 3, it can be seen that the reduction of tetrachloroisophthalonitrile in the mildew-proof coating will affect the mildew-proof and antibacterial effect of the packaging paper. This is because tetrachloroisophthalonitrile can react with glyceraldehyde-3-phosphate dehydrogenase in fungal cells and combine with the protein containing cysteine ​​in the enzyme, thereby destroying the activity of the enzyme, causing the metabolism of the fungal cells to be damaged and lose vitality, thereby achieving the effect of inhibiting mold. However, tetrachloroisophthalonitrile has a certain irritation. Although the mildew-proof grade of Example 1 is consistent with that of Comparative Example 4, the irritation of Comparative Example 4 is greater.

[0067] (3) By comparing Examples 1 and 4 with Comparative Example 1, it can be seen that the reduction of the varnish content in the anti-mildew coating will affect the anti-mildew and antibacterial effect of the packaging paper. This is because the varnish is coated on the packaging paper to form a thin film, which makes the surface of the packaging paper smooth and hydrophobic, preventing water vapor from penetrating into the packaging paper, and further improving the anti-mildew performance of the packaging paper. If the anti-mildew coating does not contain varnish, the anti-mildew and antibacterial effect of the packaging paper will be significantly reduced. The water vapor permeability of Example 1, Example 2, and Comparative Example 1 increases successively, further indicating that varnish can improve the performance of the packaging paper in blocking water vapor.

[0068] (4) By comparing Examples 1 to 4, it can be seen that the mass ratio of dry water: varnish: PN mildew inhibitor: composite quaternary ammonium salt in the mildew-proof coating is 6:10:3:0.4, and the packaging paper has the best mildew-proof, antibacterial and water vapor barrier properties.

[0069] (5) By comparing Example 1 with Comparative Examples 1 to 2, it can be seen that the packaging paper of the present invention has good stability and does not turn yellow after long-term exposure to light. Moreover, the packaging paper after exposure to light still has excellent anti-mildew properties.

[0070] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention description and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A mildew-proof and antibacterial packaging paper, It is characterized in that The invention comprises base paper, wherein a mildew-proof coating is formed on the surface of the base paper by coating mildew-proof coating; the mildew-proof coating comprises the following raw materials in parts by mass: 20 to 30 parts of a first solvent, 10 to 20 parts of varnish, 3 to 10 parts of a TPN mildew-proof agent, and 0.1 to 3 parts of a composite quaternary ammonium salt; the TPN mildew-proof agent comprises a second solvent and tetrachloroisophthalonitrile, and the mass ratio of the second solvent to tetrachloroisophthalonitrile is 100:1 to 5.

2. The mildew-proof and antibacterial packaging paper according to claim 1, It is characterized in that The anti-mildew paint comprises the following raw materials in parts by mass: 23 to 26 parts of a first solvent, 13 to 16 parts of varnish, 5 to 8 parts of a TPN anti-mildew agent, and 0.8 to 1.5 parts of a composite quaternary ammonium salt.

3. The mildew-proof and antibacterial packaging paper according to claim 1, It is characterized in that The first solvent is medium-dry water.

4. The mildew-proof and antibacterial packaging paper according to claim 3, It is characterized in that The first solvent comprises the following raw materials in parts by mass: 16 to 40 parts of isopropanol, 20 to 40 parts of ethyl acetate, 20 to 30 parts of ethanol, and 10 to 30 parts of n-butyl acetate.

5. The mildew-proof and antibacterial packaging paper according to claim 1, It is characterized in that The second solvent is ethanol.

6. The mildew-proof and antibacterial packaging paper according to claim 1, It is characterized in that The mass ratio of the second solvent to tetrachloroisophthalonitrile is 100:1.5-3.

7. The mildew-proof and antibacterial packaging paper according to claim 1, It is characterized in that The base paper is coated with 5 to 8 grams of anti-mildew paint per square meter.

8. The mildew-proof and antibacterial packaging paper according to claim 1, It is characterized in that The varnish is UV varnish.

9. A method for preparing mildew-proof and antibacterial packaging paper, used for preparing the mildew-proof and environmentally friendly packaging paper according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Step 1: prepare a composite quaternary ammonium salt solution; Step 2: sequentially adding TPN mildew preventer, composite quaternary ammonium salt solution and the first solvent into the reactor; Step 3: Slowly add varnish to the reactor; Step 4: stirring the composition in the reactor for 3 to 6 minutes to obtain an anti-mildew coating; Step 5: Apply the anti-mildew coating on the surface of the base paper and dry it to obtain the anti-mildew and antibacterial packaging paper.

10. The method for preparing the mildew-proof and antibacterial packaging paper according to claim 9, It is characterized in that In the step 5, the anti-mildew coating base paper is dried by hot air.

Citation Information

Patent Citations

  • Paper substrates and articles containing antimicrobial components as well as methods of making and using the same

    CN101107398A

  • Gloss oil for IMD (In-Mold Decoration) printing ink, IMD printing ink, IMD film and preparation method of gloss oil

    CN102719139A

  • Curable composite quaternary ammonium salt, preparation method thereof, and application thereof in disinfection and sterilization

    CN103535372A

  • Fungus-resistant-treated coatings of printed wrapping paper and production method thereof