Antioxidant impregnated paper
By using antioxidant impregnation liquid in the impregnated paper to form an antioxidant film, the oxidation problem of impregnated paper under high temperature and light is solved, its antioxidant ability and durability are improved, and safety and environmental protection performance are ensured.
Patent Information
- Application Number
- CN202411290758.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
AI Technical Summary
Existing impregnated papers are prone to oxidation under high temperature and light conditions, resulting in damage to the fiber structure, reducing its strength, toughness and durability, and thus accelerating the aging process.
Using antioxidant impregnation liquid, containing a core antioxidant mixture (natural and synthetic antioxidant), auxiliary antioxidant, solvent, thickener, emulsifier, preservative and functional additives, the antioxidant film is formed through the impregnation and drying process. Improve the antioxidant ability of impregnated paper.
Maintain impregnated paper performance under different environmental conditions, alleviate oxidation problems, improve mechanical strength and water resistance, and ensure safety and environmental protection.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of impregnated paper, in particular to an anti-oxidation impregnated paper. Background Art
[0002] Impregnated paper is a porous material made of interwoven fibers with many gaps between the fibers and filled with air. The process of impregnating paper in glue is actually a process of exchanging air between the glue and the paper. Since the impregnated paper is easily damaged by light and friction in the natural environment during use, the service life of the impregnated paper is easily shortened. Therefore, the existing technology for the production of impregnated paper usually increases the service life of the impregnated paper by improving the process.
[0003] Chinese invention patent CN104775332A discloses a corrosion-resistant impregnated paper, which uses corrosion-resistant impregnated paper glue. The corrosion-resistant impregnated paper glue is made of polyethylene and melamine as raw materials. By using the corrosion-resistant impregnated paper glue to produce corrosion-resistant impregnated paper, the corrosion resistance of the impregnated paper is greatly improved, meeting people's needs.
[0004] Although the above process can improve the high temperature resistance and corrosion resistance of the impregnated paper to a certain extent, the high temperature may also cause oxidation of the impregnated paper during use. The oxidation will cause damage to the fiber structure of the paper, thereby reducing the strength, toughness and durability of the paper, making it more susceptible to other environmental factors such as humidity, light, etc., thereby accelerating the aging process of the paper. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In order to solve the problems existing in the above-mentioned background technology, the present invention adopts the following technical solutions.
[0007] An anti-oxidation impregnated paper comprises base paper, wherein the base paper is impregnated in an anti-oxidation impregnation liquid and then taken out and dried, wherein the anti-oxidation impregnation liquid adheres to the surface of the base paper to form at least one layer of anti-oxidation film,
[0008] Characterized in that the antioxidant impregnation solution comprises the following components in weight percentage:
[0009] Core Antioxidant Blend 20%-40%,
[0010] Auxiliary antioxidant 5%-15%,
[0011] Solvent 40%-60%,
[0012] Thickener 2%-8%,
[0013] Emulsifier 0.5%-2%,
[0014] Preservatives 0.1%-1%,
[0015] Functional additives 0%-10%.
[0016] Preferably, the core antioxidant mixture includes natural antioxidants and synthetic antioxidants, and the ratio of natural antioxidants to synthetic antioxidants is 1:1 to 2:1; the natural antioxidants are specifically flavonoids, and the synthetic antioxidant is tert-butylhydroquinone.
[0017] Preferably, the auxiliary antioxidants are propyl gallate and glucose oxidase.
[0018] Preferably, the solvent is a mixture of ethanol, isopropanol and water in a volume ratio of 1:1:1.
[0019] Preferably, the thickener is sodium carboxymethyl cellulose and the emulsifier is Tween 80.
[0020] Preferably, the functional additives include one or more of a moisture-proofing agent, an ultraviolet light absorber and an antibacterial agent.
[0021] Preferably, the base paper is prepared by using a fiber mixture to obtain pulp using an enzyme pulping method, and the fiber mixture is a mixture of bamboo fiber and hemp fiber in a mixing ratio of 2:1, and laccase is selected as a catalyst in the enzyme pulping method.
[0022] A method for anti-oxidation impregnated paper comprises the following steps:
[0023] Step 1: preparing an impregnation solution;
[0024] Step 2: Immerse the paper substrate in the solution;
[0025] Step 3: Drying and curing;
[0026] Step 4: Quality inspection.
[0027] Preferably, the solution preparation in step 1 requires the use of a stirrer.
[0028] Preferably, the drying and curing in step 3 is carried out in two steps, and the drying temperature ranges from 90° C. to 140° C., and the drying time ranges from 10 min to 60 min.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] (1) The impregnating liquid used for the impregnated paper in the present invention is a mixed liquid, and the mixed liquid contains a mixed antioxidant and an auxiliary antioxidant that can play an antioxidant role. The mixed antioxidant and the auxiliary antioxidant can form an antioxidant layer on the surface of the base paper of the impregnated paper, thereby improving the antioxidant ability of the impregnated paper. The antioxidant impregnated paper can maintain its performance under different environmental conditions, thereby slowing down the oxidation problem caused by the impregnated paper being exposed to light or high temperature during use.
[0031] (2) The impregnation liquid of the present invention contains a core antioxidant mixture, which is composed of natural antioxidants and synthetic antioxidants. The natural antioxidants are flavonoids, which can remove free radicals and prevent organic components such as cellulose in paper from decomposing due to oxidation. Flavonoids can also combine with cellulose in paper to improve the mechanical strength, flexibility and water resistance of paper. The tertiary butyl hydroquinone used in the synthetic antioxidant still maintains good antioxidant properties under high temperature conditions. This allows the production process of the impregnated paper to maintain its antioxidant effect even after high temperature treatment. At the same time, tertiary butyl hydroquinone is a food-grade synthetic agent. After combining with the natural antioxidant, the impregnated paper of the present invention is relatively safe. During use, the impregnated paper will not release a large amount of harmful substances, which is safer.
[0032] (3) The auxiliary antioxidants of the present invention are propyl gallate and glucose oxidase. Propyl gallate still maintains its antioxidant properties at high temperatures and can still maintain its antioxidant effect during the high-temperature treatment process of impregnated paper. Glucose oxidase catalyzes the oxidation of glucose to generate gluconic acid and hydrogen peroxide, which can form a protective oxide film on the surface of paper, helping to prevent the organic matter in the paper from being oxidized. The generated hydrogen peroxide can be used as a cross-linking agent to promote the cross-linking reaction of cellulose in the paper, thereby increasing the mechanical strength and folding resistance of the paper.
[0033] (4) The base paper used for impregnated paper in the present invention adopts a laccase pulping method during pulping, and laccase is used to degrade lignin. The method is simple and has no pollution to the environment. The raw material lignin is degraded into low molecular weight lignin by laccase, which increases the dissolution and extraction capacity of lignin, thereby achieving the separation of lignin from cellulose and hemicellulose. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below.
[0035] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0036] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments. The present invention provides the following embodiments.
[0037] Example 1
[0038] An antioxidant impregnation solution comprises the following components in percentage by weight:
[0039] Core Antioxidant Blend 40%,
[0040] Auxiliary antioxidant 15%,
[0041] Solvent 60%,
[0042] Thickener 8%,
[0043] Emulsifier 2%,
[0044] Preservative 1%,
[0045] Functional additives 10%.
[0046] The Core Antioxidant Blend contains a 1:1 ratio of natural antioxidants to synthetic antioxidants.
[0047] Propyl gallate was selected as the auxiliary antioxidant.
[0048] The solvent is a mixture of ethanol, isopropanol and water in a volume ratio of 1:1:1.
[0049] The thickener is sodium carboxymethyl cellulose and the emulsifier is Tween 80.
[0050] The functional additives include moisture-proofing agent and ultraviolet light absorber.
[0051] A method for producing an antioxidant impregnated paper using the above antioxidant impregnating solution comprises the following steps:
[0052] Step 1: prepare an impregnation solution, add the above-provided solution in proportion into a stirrer for mixing and stirring, first add a solvent into the stirrer, heat the solvent to 40°, add a core antioxidant mixture and an auxiliary antioxidant, start the stirrer for stirring, and the stirring time is at least 20 minutes. Add a thickener while the stirrer is running, and add an emulsifier and a preservative after the thickener is added. After the stirring gas is running for 30 minutes, finally add a functional additive and stir for 10 minutes;
[0053] Step 2: Immerse the paper substrate in the solution, and immerse it twice. During the first immersion, the base paper is pressed into the impregnation solution by a pressing roller in the prior art. The base paper stays in the impregnation solution for no less than three seconds before being taken out. The base paper needs to stay for thirty seconds after being taken out, so that the excess impregnation liquid on the base paper drips off for recycling. The first immersed paper is blown by an air drying device to dry the surface of the paper. The dried paper is immersed for the second time. The second immersion time is 1 second and then it is taken out and stayed for thirty seconds;
[0054] Step 3: Drying and curing. The twice impregnated paper is dried using a drying device. The drying is performed twice. The first drying is performed at 120°C for 40 minutes. After the first drying, the impregnated paper is taken out and cooled for 20 minutes. The second drying is performed at 140°C for 10 minutes.
[0055] Step 4: Quality inspection. In order to ensure that the impregnated paper meets the specified standards and performance requirements, the impregnated paper is tested as follows:
[0056] (1) Thickness test, measuring the thickness of the impregnated paper to ensure it meets the specification requirements;
[0057] (2) Density test, to determine the mass per unit volume of the impregnated paper, reflecting its compactness;
[0058] (3) Water absorption test, which tests the ability of impregnated paper to absorb water, usually measured by water absorption rate or water absorption height;
[0059] (4) Thermal stability test, to evaluate the dimensional stability and deformation of the impregnated paper at high temperatures;
[0060] (5) Wear resistance test, to check the wear resistance of the impregnated paper surface, usually completed by friction test;
[0061] (6) Tensile strength test, measuring the maximum load-bearing capacity of the impregnated paper under tension;
[0062] (7) Elongation at break test, which detects the extension length of the impregnated paper before breaking, reflecting its toughness;
[0063] (8) Bending strength test, to evaluate the strength of the impregnated paper under bending.
[0064] (9) Surface roughness test, measuring the smoothness or roughness of the impregnated paper surface.
[0065] (10) Bonding strength test: to detect the bonding strength between impregnated paper and other materials.
[0066] (11) Chemical stability test, to evaluate the resistance of impregnated paper to chemicals, such as acid and alkali resistance, solvent resistance, etc.
[0067] (12) Fire resistance test, to check the fire resistance or flame retardant properties of the impregnated paper.
[0068] (13) Formaldehyde emission test: For impregnated paper containing formaldehyde resin, its formaldehyde emission is tested to ensure that it meets environmental protection standards.
[0069] (14) Appearance inspection: visually inspect the surface of the impregnated paper for defects, color differences, stains, etc.
[0070] (15) Dimensional stability test, to evaluate the dimensional changes of impregnated paper under different temperature and humidity conditions.
[0071] Example 2
[0072] An antioxidant impregnation solution comprises the following components in percentage by weight:
[0073] Core Antioxidant Blend 30%,
[0074] Auxiliary antioxidant 10%,
[0075] Solvent 50%,
[0076] Thickener 5%,
[0077] Emulsifier 1%,
[0078] Preservative 0.5%,
[0079] Functional additives 5%.
[0080] The core antioxidant blend contains a 1.5:1 ratio of natural antioxidants to synthetic antioxidants.
[0081] Glucose oxidase is selected as an auxiliary antioxidant.
[0082] The solvent was a mixture of ethanol, isopropanol, and water in a volume ratio of 1:1:1.
[0083] The thickener is sodium carboxymethyl cellulose and the emulsifier is Tween 80.
[0084] A method for producing an antioxidant impregnated paper using the above antioxidant impregnating solution comprises the following steps:
[0085] Step 1: prepare the impregnation solution, add the above-provided solution in proportion into a stirrer for mixing and stirring, first add the solvent into the stirrer, heat the solvent to 40°, add the core antioxidant mixture and the auxiliary antioxidant, start the stirrer for stirring, and the stirring time is at least 15 minutes. Add the thickener while the stirrer is running, and add the emulsifier and preservative after the thickener is added. After the stirring gas is running for 25 minutes, finally add the functional additive and stir for 8 minutes;
[0086] Step 2: Immerse the paper substrate in the solution, and immerse it twice. During the first immersion, the base paper is pressed into the impregnation solution by a pressing roller in the prior art. The base paper stays in the impregnation solution for no less than three seconds before being taken out. The base paper needs to stay for thirty seconds after being taken out, so that the excess impregnation liquid on the base paper drips off for recycling. The first immersed paper is blown by an air drying device to dry the surface of the paper. The dried paper is immersed for the second time. The second immersion time is 1 second and then it is taken out and stayed for thirty seconds;
[0087] Step 3: Drying and curing. The twice impregnated paper is dried using a drying device. The drying is performed twice. The first drying is performed at 100°C for 35 minutes. After the first drying, the impregnated paper is taken out and cooled for 15 minutes. The second drying is performed at 120°C for 8 minutes.
[0088] Step 4: Quality inspection. In order to ensure that the impregnated paper meets the specified standards and performance requirements, the impregnated paper is tested as follows:
[0089] (1) Thickness test, measuring the thickness of the impregnated paper to ensure it meets the specification requirements;
[0090] (2) Density test, to determine the mass per unit volume of the impregnated paper, reflecting its compactness;
[0091] (3) Water absorption test, which tests the ability of impregnated paper to absorb water, usually measured by water absorption rate or water absorption height;
[0092] (4) Thermal stability test, to evaluate the dimensional stability and deformation of the impregnated paper at high temperatures;
[0093] (5) Wear resistance test, to check the wear resistance of the impregnated paper surface, usually completed by friction test;
[0094] (6) Tensile strength test, measuring the maximum load-bearing capacity of the impregnated paper under tension;
[0095] (7) Elongation at break test, which detects the extension length of the impregnated paper before breaking, reflecting its toughness;
[0096] (8) Bending strength test, to evaluate the strength of the impregnated paper under bending.
[0097] (9) Surface roughness test, measuring the smoothness or roughness of the impregnated paper surface.
[0098] (10) Bonding strength test: to detect the bonding strength between impregnated paper and other materials.
[0099] (11) Chemical stability test, to evaluate the resistance of impregnated paper to chemicals, such as acid and alkali resistance, solvent resistance, etc.
[0100] (12) Fire resistance test, to check the fire resistance or flame retardant properties of the impregnated paper.
[0101] (13) Formaldehyde emission test: For impregnated paper containing formaldehyde resin, its formaldehyde emission is tested to ensure that it meets environmental protection standards.
[0102] (14) Appearance inspection: visually inspect the surface of the impregnated paper for defects, color differences, stains, etc.
[0103] (15) Dimensional stability test, to evaluate the dimensional changes of impregnated paper under different temperature and humidity conditions.
[0104] Example 3
[0105] An antioxidant impregnation solution comprises the following components in percentage by weight:
[0106] Core Antioxidant Blend 20%,
[0107] Auxiliary antioxidant 5%,
[0108] Solvent 40%,
[0109] Thickener 2%,
[0110] Emulsifier 0.5%,
[0111] Preservative 0.1%,
[0112] Functional additives 0%.
[0113] The Core Antioxidant Blend contains a 2:1 ratio of natural to synthetic antioxidants.
[0114] Propyl gallate and glucose oxidase were selected as auxiliary antioxidants.
[0115] The solvent was a mixture of ethanol, isopropanol, and water in a volume ratio of 1:1:1.
[0116] The thickener is sodium carboxymethyl cellulose and the emulsifier is Tween 80.
[0117] A method for producing an antioxidant impregnated paper using the above antioxidant impregnating solution comprises the following steps:
[0118] Step 1: prepare the impregnation solution, add the above-provided solution in proportion into a stirrer for mixing and stirring, first add the solvent into the stirrer, heat the solvent to 40°, add the core antioxidant mixture and the auxiliary antioxidant, start the stirrer for stirring, and the stirring time is at least 18 minutes. Add the thickener while the stirrer is running, and add the emulsifier and preservative after the thickener is added. After the stirring gas is running for 25 minutes, finally add the functional additive and stir for 10 minutes;
[0119] Step 2: Immerse the paper substrate in the solution, and immerse it twice. During the first immersion, the base paper is pressed into the impregnation solution by a pressing roller in the prior art. The base paper stays in the impregnation solution for no less than three seconds before being taken out. The base paper needs to stay for thirty seconds after being taken out, so that the excess impregnation liquid on the base paper drips off for recycling. The first immersed paper is blown by an air drying device to dry the surface of the paper. The dried paper is immersed for the second time. The second immersion time is 1 second and then it is taken out and stayed for thirty seconds;
[0120] Step 3: Drying and curing. The twice impregnated paper is dried using a drying device. The drying is performed twice. The first drying is performed at 90°C for 30 minutes. After the first drying, the impregnated paper is taken out and cooled for 8 minutes. The second drying is performed at 110°C for 8 minutes.
[0121] Step 4: Quality inspection. In order to ensure that the impregnated paper meets the specified standards and performance requirements, the impregnated paper is tested as follows:
[0122] (1) Thickness test, measuring the thickness of the impregnated paper to ensure it meets the specification requirements;
[0123] (2) Density test, to determine the mass per unit volume of the impregnated paper, reflecting its compactness;
[0124] (3) Water absorption test, which tests the ability of impregnated paper to absorb water, usually measured by water absorption rate or water absorption height;
[0125] (4) Thermal stability test, to evaluate the dimensional stability and deformation of the impregnated paper at high temperatures;
[0126] (5) Wear resistance test, to check the wear resistance of the impregnated paper surface, usually completed by friction test;
[0127] (6) Tensile strength test, measuring the maximum load-bearing capacity of the impregnated paper under tension;
[0128] (7) Elongation at break test, which detects the extension length of the impregnated paper before breaking, reflecting its toughness;
[0129] (8) Bending strength test, to evaluate the strength of the impregnated paper under bending.
[0130] (9) Surface roughness test, measuring the smoothness or roughness of the impregnated paper surface.
[0131] (10) Bonding strength test: to detect the bonding strength between impregnated paper and other materials.
[0132] (11) Chemical stability test, to evaluate the resistance of impregnated paper to chemicals, such as acid and alkali resistance, solvent resistance, etc.
[0133] (12) Fire resistance test, to check the fire resistance or flame retardant properties of the impregnated paper.
[0134] (13) Formaldehyde emission test: For impregnated paper containing formaldehyde resin, its formaldehyde emission is tested to ensure that it meets environmental protection standards.
[0135] (14) Appearance inspection: visually inspect the surface of the impregnated paper for defects, color differences, stains, etc.
[0136] (15) Dimensional stability test, to evaluate the dimensional changes of impregnated paper under different temperature and humidity conditions.
[0137] Furthermore, the base paper in the present application adopts a fiber mixture to obtain pulp using an enzyme pulping method. The fiber mixture is a mixture of bamboo fiber and hemp fiber in a mixing ratio of 2:1. Laccase is selected as a catalyst in the enzyme pulping method. The specific manufacturing method of the base paper is as follows:.
[0138] (1) Pulp preparation: bamboo fiber and hemp fiber are mixed evenly, and then chopped and steamed for subsequent processing;
[0139] (2) Pulp treatment: The pretreated fiber raw material is mixed with a laccase solution. The role of laccase is to oxidize the phenolic structure in lignin, change the chemical properties of lignin, and make it more easily degraded. The above process is usually carried out under mild conditions, avoiding high temperatures to avoid excessive damage to the fiber. In this process, ligninase or manganese peroxidase is added to cooperate with the action of laccase and improve the degradation efficiency of lignin.
[0140] (3) Fermentation: After enzyme treatment, the fiber raw material may need to be fermented for a certain period of time so that the enzyme has enough time to act on the lignin;
[0141] (4) Refining: The fermented fiber raw materials are refined by mechanical methods to further separate the fibers and remove some lignin;
[0142] (5) Paper preparation: dry strength agent, CMC, retention agent and defoamer are added to the pulp after the refining treatment, and paper is prepared through steps such as dehydration on a forming wire, forming, pressing and drying.
[0143] The above content is a further detailed description of the present invention in combination with specific implementation methods. It cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the scope of protection determined by the claims submitted for the present invention.
Claims
1. An anti-oxidation impregnated paper, comprising base paper, wherein the base paper is impregnated in an anti-oxidation impregnation liquid and then taken out and dried, wherein the anti-oxidation impregnation liquid adheres to the surface of the base paper to form at least one anti-oxidation film, It is characterized in that The antioxidant impregnation solution includes the following components in weight percentage: Core Antioxidant Blend 20%-40%, Auxiliary antioxidant 5%-15%, Solvent 40%-60%, Thickener 2%-8%, Emulsifier 0.5%-2%, Preservatives 0.1%-1%, Functional additives 0%-10%.
2. The anti-oxidative impregnated paper according to claim 1, characterized in that: The core antioxidant mixture includes natural antioxidants and synthetic antioxidants, and the ratio of natural antioxidants to synthetic antioxidants is 1:1 to 2:1; the natural antioxidants are specifically flavonoid compounds, and the synthetic antioxidant is tert-butylhydroquinone.
3. The anti-oxidative impregnated paper according to claim 1, characterized in that: The auxiliary antioxidant is propyl gallate or glucose oxidase.
4. The anti-oxidative impregnated paper according to claim 2, characterized in that: The solvent was a mixture of ethanol, isopropanol, and water in a volume ratio of 1:1:
1.
5. The anti-oxidative impregnated paper according to claim 2, characterized in that: The thickener is sodium carboxymethyl cellulose and the emulsifier is Tween 80.
6. The anti-oxidative impregnated paper according to claim 5, characterized in that: The functional additives include one or more of a moisture-proof agent, an ultraviolet light absorber and an antibacterial agent.
7. The anti-oxidative impregnated paper according to claim 6, characterized in that: The base paper adopts a fiber mixture to obtain pulp by an enzyme pulping method, and the fiber mixture is a mixture of bamboo fiber and hemp fiber in a mixing ratio of 2:
1. Laccase is selected as a catalyst in the enzyme pulping method.
8. A method for producing antioxidant impregnated paper using the impregnation solution according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: preparing an impregnation solution; Step 2: Immerse the paper substrate in the solution; Step 3: Drying and curing; Step 4: Quality inspection.
9. The method for producing impregnated paper according to claim 8, characterized in that: The solution preparation in step 1 requires the use of a stirrer.
10. The method according to claim 8, characterized in that: The drying and curing in step 3 is carried out in two steps, and the drying temperature ranges from 90° C. to 140° C., and the drying time ranges from 10 min to 60 min.
Citation Information
Patent Citations
Tea flavonoids containing water-based coating for cigarette plug wrap paper
CN101864694A
Biochemical pulping method for non-wood raw material
CN106283788A
High-toughness non-woven coated paper and preparation method thereof
CN109667197A
Bioflavonoid-coated materials
CN110004714A
Impregnation paper for floor material
JP2010150852A