Preparation method for TEM ultrathin section sample
By adjusting the resin composition and processing technology, the problem of insufficient resin quality and slice efficiency in ultra-thin slice technology is solved, the stability and high-quality slice of the sample under the electron beam are achieved, the preparation efficiency is improved, and the transmission electron microscopy analysis is provided. A solid foundation.
Patent Information
- Application Number
- CN202411291342.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
AI Technical Summary
The existing ultra-thin slice technology has problems such as insufficient resin quality control and slice efficiency during sample preparation, which leads to unstable samples in transmission electron microscopy experiments and makes it difficult to obtain high-quality TEM images.
By adjusting the ratio of resin components Epon812, DDSA, MNA and BDMA, combining machine block repair and finishing technology, different resin ratios and tools are used for rough processing and finishing, ensuring the flatness and dimensional accuracy of the sample surface and achieving efficient preparation continuous , regular ultra-thin slices.
The stability and sheet continuity of the sample under the electron beam are achieved, the sample preparation cycle is shortened, the preparation efficiency is improved, and the high-quality ultra-thin sectioned samples are ensured, providing a solid foundation for subsequent microscopy.
Smart Images

Figure CN118961271A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of transmission electron microscope slice samples, and in particular relates to a preparation method for TEM ultra-thin slice samples. Background Art
[0002] Low-dimensional materials such as nanosheets, nanowires and quantum dots have shown extensive development potential and application value in many fields due to their unique physical and chemical properties. To optimize and regulate the performance of these low-dimensional materials, it is first necessary to conduct in-depth characterization and analysis of their structure. Transmission electron microscopy (TEM) is a powerful tool for characterizing materials. Its imaging mode can characterize the microscopic morphology of samples and the lattice information at the atomic scale, and the diffraction mode can study the crystal orientation and structural information of samples. A series of high-quality TEM images are inseparable from sample preparation. According to electron microscopists, excellent sample preparation accounts for 70% of the success of TEM research. Excellent TEM samples should have electron beam transparency and be relatively stable under the irradiation of high-energy electron beams. Different samples require different preparation methods. For example, for bulk materials, ion thinning methods can be used, for thin film samples, focused ion beam processing and thinning can be used, and for powder samples, ultrasonic dispersion preparation is generally selected. However, for some samples with uneven thickness and samples that want to observe cross-sections, ultrasonic dispersion methods often cannot obtain high-quality TEM images.
[0003] The development of ultrathin sectioning technology is closely related to the progress of electron microscopy. In the early days, scientists had difficulty taking advantage of the high-resolution capabilities of electron microscopes due to the lack of effective sample preparation methods. In the mid-20th century, with the invention of ultramicrotomes and the application of ion beam cutting technology, ultrathin sectioning technology developed rapidly. These technological advances have greatly promoted research in fields such as biology and materials science, allowing scientists to observe structural details at the atomic or molecular level. However, ultrathin sectioning technology still faces problems such as difficult sample preparation, poor sectioning uniformity, and microscopic damage control. To solve these problems, scientists have developed a variety of advanced sample fixation, embedding, and cutting techniques. For example, the use of chemical fixatives and cryosectioning techniques can effectively reduce damage to biological samples during preparation. At the same time, the application of focused ion beam (FIB) technology makes it possible to prepare ultrathin sections in specific areas, greatly improving the accuracy and efficiency of sample preparation.
[0004] At present, ultrathin sections usually involve embedding the sample with resin first, then manually trimming the block, and finally slicing. However, the existing technology still has deficiencies in controlling the resin quality and slicing efficiency, which may lead to unstable samples during TEM experiments. Therefore, a method for preparing ultrathin section samples for TEM is proposed. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a TEM ultrathin section sample, aiming to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention firstly selects resins of different proportions according to different samples, which determines the stability of the sample under the electron beam after slicing and the continuity between the slices. Secondly, through the method of machine trimming and then fine trimming, continuous, regular and high-quality slice samples can be obtained efficiently.
[0008] A method for preparing a TEM ultrathin section sample comprises the following steps:
[0009] Step 1: Mix Epon812, DDSA, MNA and BDMA and pour into a beaker.
[0010] Step 2: Place the beaker in step 1 in a water bath, heat to 30°C, and stir slowly for 20 minutes until the resin is uniform in color. Since the resin is viscous, the stirring rate should be slow to prevent bubbles from forming that may cause resin configuration failure.
[0011] Step 3: Use ethanol, acetone and ultrapure water to ultrasonically clean the embedding mold in sequence, and put the cleaned embedding mold into an oven for drying.
[0012] Step 4: Take the powder sample and place it in the embedding mold that has been cleaned and dried in step 3. Fill the tip of the mold, use a pipette to absorb the prepared resin, and drop it into the embedding mold in mid-air until the resin completely fills the embedding mold. It is worth noting that if the resin is not dropped in mid-air but dripped along the inner wall of the embedding mold, bubbles are likely to be generated inside, causing difficulties in the subsequent preparation process.
[0013] Step 5: Place the mold after adding the resin in step 4 into an oven at 60°C for curing for at least 48 hours.
[0014] Step 6. Fix the cured resin in step 5 on the fixture, and use the Leica EM TXP lapping machine to perform rough processing on the sample: adjust the sample rotation handle to 30°, use a milling cutter to process a bevel, and after processing one side, rotate the sample 180° to process the second bevel until the two bevels are symmetrical; continue to rotate 90° to process the third bevel, and then rotate 180° to process the fourth bevel until the resin block presents a pyramid-like structure; adjust the sample rotation handle to 0° to process a small plane, so that the resin block presents a Mayan pyramid-like structure, and complete the rough processing.Figure 1 shown.
[0015] Step 7. Use the Leica EMUC7 ultrathin slicer to fine-process the sample: replace the tool with a 45° diamond knife and set the tool table inclination angle to 6°; turn on the bottom illumination lamp to perform tool setting, and fine-tune the hand wheel to observe the change in the width of the bright line of the tool on the sample surface when the sample moves up and down, until the bright line almost does not change up and down, at which time the tool setting is completed. After the tool setting is completed, fine-process the left and right sides of the top table of the sample to reduce the width of the table; rotate the sample 90° and process the remaining two sides until a rectangular table with a smaller side length is obtained; finally, manually flatten the top of the sample to facilitate subsequent ultrathin sectioning.
[0016] Step 8, replace the tool with an Ultrathin diamond knife, keep the tool table inclination angle unchanged, and use the same tool setting method as step 7; after tool setting, turn off the bottom irradiation lamp, turn on the top irradiation lamp, drip ultrapure water into the tool water tank until the liquid surface is raised, and then slowly absorb water until the liquid surface is flat, which is manifested by the reflection on the liquid surface being completely spread out and without barrel-shaped or pillow-shaped distortion; start slicing, and adjust the step length to 500nm in the initial empty cutting stage. When the sample is cut, immediately reduce the step length to 100nm, and after stably cutting 3 consecutive slices, reduce the step length to 70nm, and stop slicing after stably cutting 3 consecutive slices, and use an eyelash pen to move the first few slices to a remote area; reduce the step length to 40nm, and after cutting 5 consecutive slices, use an eyelash pen to disconnect the connection between the slice and the blade, and repeat the operation until 3 rows of slice samples are obtained;
[0017] Step 9. Use TEM precision tweezers to pick up a micro-grating and place it face down at a 45° angle to the horizontal direction. Dip the thin slice sample vertically downward to complete the preparation of the TEM ultra-thin section sample.
[0018] Furthermore, the volume ratio of Epon812, DDSA, MNA and BDMA is 25:(16-20):(10-14):(1.3-1.7).
[0019] Furthermore, the BDMA is replaced by DMP-30.
[0020] Furthermore, the 45° diamond knife is replaced with a glass knife.
[0021] Furthermore, the Ultrathin diamond knife is replaced with a glass knife.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention controls the hardness and softness of the resin by adjusting the ratio of the resin components Epon812, DDSA, MNA and BDMA, meeting the preparation requirements under different materials and seasonal conditions. The prepared samples are transparent and stable under electron beam, providing a solid foundation for subsequent microscopic analysis.
[0024] 2. The present invention proposes a combined method of trimming and slicing, which effectively shortens the sample preparation cycle and improves the preparation efficiency compared to the traditional embedding and slicing method. By pre-treating the sample before slicing in a mode combining rough processing with fine processing, the surface flatness and dimensional accuracy of the sample before slicing are ensured, thereby obtaining ultra-thin slice samples with uniform thickness and high quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a resin block with a structure similar to a Mayan pyramid.
[0026] Figure 2 This is the HAADF-STEM image of the cross section of the MoO3 nanosheet in Example 1.
[0027] Figure 3 This is a low-magnification morphological image of the MoO3 nanosheets in Example 1.
[0028] Figure 4 This is the HRTEM image of α-CoOOH in Example 2.
[0029] Figure 5 This is the SAED pattern of α-CoOOH in Example 2.
[0030] Figure 6 This is the HAADF-STEM image of NiMoO4 nanorods in Example 3.
[0031] Figure 7 for Figure 6 FFT image corresponding to the HAADF-STEM image of NiMoO4 nanorods. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0033] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0034] Example 1: MoO3 nanosheets are a layered structure that has a wide range of applications in the field of energy storage. However, the interlayer structure cannot be observed by ultrasonic dispersion, so the TEM sample is prepared by embedding and ultrathin sectioning. The preparation steps are as follows:
[0035] (1) Take 25 ml of Epon812, 18 ml of DDSA, 12 ml of MNA and 1.5 ml of BDMA. This ratio of resin has moderate hardness and is suitable for MoO3 nanosheet slicing. Mix the four and heat and stir in an oil bath at 30° for 20 min until the resin is evenly stirred.
[0036] (2) Place an appropriate amount of powder (MoO3 nanosheets) in the cleaned embedding mold, fill the tip of the mold, and drop the resin in mid-air until the resin fills the embedding mold. Place the mold after adding the resin in a 60°C oven for 48 hours.
[0037] (3) A Leica EM TXP lapping machine is used for rough machining to produce a pointed surface similar to that of a Mayan pyramid.
[0038] (4) Leica EMUC7 was used for fine processing. Since the size of MoO3 nanosheets is about 200-400 nm, which is relatively large, the small planes processed were as large as possible to achieve the best effect. Finally, a plane of 500*500 μm was processed for final slicing.
[0039] (5) Final slicing: the thickness of each sample is controlled at 40 nm. After obtaining a series of continuous thin slices, a microgrid is used to fish out the slices.
[0040] in Figure 2 HAADF-STEM image of the cross section of MoO3 nanosheet; Figure 3 This is a low-magnification image of the MoO3 nanosheet. Figure 2 and Figure 3 The morphology of the nanosheet cross section and the lattice fringes at high resolution can be clearly distinguished, proving that the sample preparation effect is very good and high-quality electron microscope images can be obtained.
[0041] Example 2: α-CoOOH has the characteristics of large interlayer spacing and has development potential in the field of energy storage. Its morphology is a large two-dimensional sheet structure, ranging from about 2 to 4 μm. In order to study its interlayer structure, we choose the ultrathin section method to prepare TEM samples. The preparation steps are as follows:
[0042] (1) Take 25 ml of Epon812, 20 ml of DDSA, 10 ml of MNA and 1.7 ml of BDMA. This ratio of resin is softer and has better toughness, which is suitable for very thin and easily deformed samples. Mix the four ingredients and heat and stir them in an oil bath at 30° for 20 minutes until the resin is evenly mixed.
[0043] (2) Place an appropriate amount of powder (α-CoOOH) in the cleaned embedding mold, fill the tip of the mold, and drop the resin in mid-air until the resin fills the embedding mold. Place the mold after adding the resin in a 60°C oven for 48 hours.
[0044] (3) A Leica EM TXP lapping machine is used for rough machining to produce a pointed surface similar to that of a Mayan pyramid.
[0045] (4) Leica EMUC7 was used for fine processing. Since α-CoOOH is very large, the small plane processed was as large as possible to achieve the best effect. Finally, a plane of 800*800 μm was processed for final slicing.
[0046] (5) Final slicing: Since α-CoOOH is not resistant to electron beams, a slightly thicker resin can make the sample more stable under electron beams. Therefore, the thickness of each sample is controlled at 60 nm, and a series of continuous slices are obtained and then the slices are fished out using a microgrid.
[0047] in Figure 4 HRTEM image of α-CoOOH; Figure 5 is the SAED pattern of α-CoOOH. Figure 4 and Figure 5 The lattice fringes of α-CoOOH at high resolution and the clear and sharp diffraction spots can be clearly distinguished, which proves that the sample preparation effect is very good and high-quality electron microscope images can be obtained.
[0048] Example 3: NiMoO4 nanorods, as a nanomaterial with unique physical and chemical properties, have shown potential application value in many fields. The climate in northern regions is cold and dry in winter, so the resin should be harder to ensure the quality of the sheet. The preparation steps are as follows:
[0049] (1) Take 25 ml of Epon 812, 16 ml of DDSA, 14 ml of MNA and 1.3 ml of BDMA. This ratio of resin is relatively hard and is suitable for slicing under cold and dry conditions. Mix the four ingredients and heat and stir them in an oil bath at 30° for 20 minutes until the resin is evenly mixed.
[0050] (2) Place an appropriate amount of powder (NiMoO4 nanorods) in the cleaned embedding mold, fill the tip of the mold, and drop the resin in mid-air until the resin fills the embedding mold. Place the mold after adding the resin in a 60°C oven for curing for 48 hours.
[0051] (3) A Leica EM TXP lapping machine is used for rough machining to produce a pointed surface similar to that of a Mayan pyramid.
[0052] (4) Leica EMUC7 was used for fine processing. Since the size of NiMoO4 nanorods is about 200-400 nm, which is relatively large, the small plane processed was as large as possible to achieve the best effect. Finally, a plane of 500*500 μm was processed for final slicing.
[0053] (5) Final slicing: Since the resin is relatively hard, the thickness of each sample is controlled at 50 nm to ensure the continuity and stability of the slice. After obtaining a series of continuous slices, a microgrid is used to fish out the slices.
[0054] in Figure 6 HAADF-STEM image of NiMoO4 nanorods; Figure 7 for Figure 6 The corresponding FFT image of the HAADF-STEM image of NiMoO4 nanorods. Figure 6 and Figure 7 Clear high-resolution lattice fringes and sharp FFT spots in the corresponding areas can be observed, proving that the sample preparation effect is very good and high-quality electron microscope images can be obtained.
[0055] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A method for preparing a TEM ultrathin section sample, characterized in that: The following steps are involved: Step 1, mix Epon812, DDSA, MNA and BDMA and pour into a beaker; Step 2: Place the beaker in step 1 in a water bath, heat to 30°C, and stir slowly for 20 minutes until the resin has a uniform color; Step 3, ultrasonically clean the embedding mold with ethanol, acetone and ultrapure water in sequence, and place the cleaned embedding mold in an oven for drying; Step 4: Take the powder sample and place it in the embedding mold that has been cleaned and dried in step 3, fill the tip of the mold, use a pipette to absorb the prepared resin, and drop it into the embedding mold in mid-air until the resin completely fills the embedding mold; Step 5, placing the mold after adding the resin in step 4 into an oven at 60°C for curing for at least 48 hours; Step 6. Fix the cured resin in step 5 on the fixture, and use the Leica EM TXP precision grinding machine to perform rough processing on the sample: adjust the sample rotation handle to 30°, use a milling cutter as the tool to process a bevel, then rotate the sample 180°, process the second bevel, until the two bevels are symmetrical; continue to rotate 90°, process the third bevel, and then rotate 180° to process the fourth bevel, until the resin block presents a pyramid-like structure; adjust the sample rotation handle to 0°, process a plane, so that the resin block presents a Mayan pyramid-like structure, and complete the rough processing; Step 7. Use Leica EMUC7 ultrathin slicer to fine-process the sample: replace the tool with a 45° diamond knife and set the tool table inclination angle to 6°; turn on the bottom illumination lamp to perform tool setting operation until the tool does not change the width of the bright line on the sample surface; after tool setting, process the left and right sides of the top table of the sample to reduce the width of the table; rotate the sample 90° and process the remaining two sides until a rectangular table with a smaller side length is obtained; finally, manually flatten the top of the sample; Step 8, replace the tool with an Ultrathin diamond knife, keep the tool table inclination angle unchanged, and use the same tool setting method as step 7; after tool setting, turn off the bottom irradiation lamp, turn on the top irradiation lamp, add ultrapure water to the tool water tank until the liquid surface is raised, and then slowly absorb water until the liquid surface is flat, as shown by the reflection on the liquid surface completely spreading out without barrel-shaped or pillow-shaped distortion; start slicing, initially adjust the step length to 500nm in the empty cutting stage, and when the sample is cut, reduce the step length to 100nm, and after stably cutting 3 consecutive slices, reduce the step length to 70nm, and stop slicing after stably cutting 3 consecutive slices, and use an eyelash pen to move the initially cut slice to one side; reduce the step length to 40nm, and after cutting 5 consecutive slices, use an eyelash pen to disconnect the slice from the blade, and repeat the operation until 3 rows of slice samples are obtained; Step 9. Use TEM precision tweezers to pick up a micro-grating and place it face down at a 45° angle to the horizontal direction. Dip the thin slice sample vertically downward to complete the preparation of the TEM ultra-thin section sample.
2. The method for preparing a TEM ultrathin section sample according to claim 1, characterized in that: The volume ratio of Epon812, DDSA, MNA and BDMA is 25:(16-20):(10-14):(1.3-1.7).
3. The method for preparing a TEM ultrathin section sample according to claim 1, characterized in that: The BDMA was replaced with DMP-30.
4. The method for preparing a TEM ultrathin section sample according to claim 1, characterized in that: The 45° diamond knife was replaced with a glass knife.
5. The method for preparing a TEM ultrathin section sample according to claim 1, characterized in that: The Ultrathin diamond knife was replaced with a glass knife.
Citation Information
Cited By
Sample preparation method of resin sheet
CN119715054A
Preparation method of transmission electron microscope sample for micro-nano deformation analysis of selected area
CN121026693A