Lithium ion battery negative electrode powder as well as collection method and application thereof
By oxidation and water immersion of the negative electrode sheet of lithium-ion battery, the mixing of Cu particles is avoided, and the problem of large ICP analysis error in the prior art is solved, and the negative electrode powder with high purity and high recovery rate is achieved, and the battery failure is accurately analyzed. reason.
Patent Information
- Application Number
- CN202411034509.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the method of collecting negative electrode powder of waste lithium-ion batteries has mixed Cu particles, resulting in large errors in the ICP analysis results, and it is impossible to accurately analyze the major reasons for low voltage or self-discharge of the battery.
By oxidizing the fully charged negative electrode sheet, it prevents the reaction of metal lithium with water to produce hydrogen, prevents the electrode sheet from spontaneous combustion, and uses ultrasonic and drying steps to ensure the purity of the powder, avoids the mixing of Cu particles, and improves the accuracy of ICP testing.
It improves the purity and recovery rate of the negative electrode powder, enhances the accuracy of ICP testing, and can accurately analyze the causes of battery failure, such as low voltage or large self-discharge.
Smart Images

Figure CN118961332A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of material recovery, and in particular relates to a lithium-ion battery negative electrode powder and a collection method and application thereof. Background Art
[0002] By collecting negative electrode powder and using inductively coupled plasma emission spectroscopy (ICP) to test magnetic metal elements, it can be used to analyze one of the reasons for low voltage or large self-discharge of the battery, and is often an important characterization method for analyzing battery failure.
[0003] At present, the conventional and quick method for collecting negative electrode powder from waste batteries is to use a ceramic knife to scrape and collect the negative electrode plate powder. However, this method will cause friction of the current collector Cu during the sampling process, resulting in a large number of Cu particles in the powder, which will lead to large errors in testing the elemental Cu content.
[0004] Therefore, it is urgent to design a method that can accurately and quickly collect negative electrode powder to improve the accuracy of ICP analysis results and obtain a high recovery efficiency of negative electrode powder. Summary of the invention
[0005] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a lithium-ion battery negative electrode powder and a collection method and application thereof. The present invention can oxidize the metallic lithium embedded in the charged negative electrode sheet by directly subjecting the fully charged negative electrode sheet to oxidation treatment, so that it cannot react to produce hydrogen during the subsequent water immersion treatment, thereby preventing the electrode sheet from spontaneously igniting. In addition, the negative electrode powder obtained by this collection method can avoid the mixing of Cu particles in the current collector, effectively improving the purity of the negative electrode powder, which improves the test accuracy of the inductively coupled plasma emission spectroscopy ICP test of magnetic metal elements, can be used to analyze the reasons for low voltage or large self-discharge of the battery, and is an important means of analyzing battery failure. The recovery rate of the negative electrode powder obtained based on this is high.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for collecting negative electrode powder of a lithium ion battery, the collecting method comprising the following steps:
[0008] (1) disassembling the charged battery cell to obtain a fully charged negative electrode sheet;
[0009] (2) subjecting the fully charged negative electrode sheet to oxidation treatment to obtain an oxidized negative electrode sheet;
[0010] (3) The oxidized negative electrode sheet is subjected to water immersion treatment, dried, and collected after post-treatment to obtain the negative electrode powder of the lithium ion battery.
[0011] The present invention can oxidize the metal lithium embedded in the charged negative electrode sheet by directly subjecting the fully charged negative electrode sheet to oxidation treatment, so that it cannot react to produce hydrogen during the subsequent water immersion treatment process, thereby preventing the electrode sheet from spontaneously igniting. In addition, the negative electrode powder obtained by this collection method can avoid the mixing of Cu particles in the current collector, effectively improving the purity of the negative electrode powder, which improves the test accuracy for the inductively coupled plasma emission spectroscopy ICP test of magnetic metal elements, can be used to analyze the reasons for low voltage or large self-discharge of the battery, and is an important means of analyzing battery failure. The negative electrode powder obtained based on this has a high recovery rate.
[0012] It should be noted that the fully charged state refers to when the battery is fully charged, that is, the maximum capacity of electrical energy has been stored. This is called the fully charged state. The fully charged negative electrode sheet in the present invention is a state with a voltage range of 4.17-4.18V.
[0013] As a preferred technical solution of the present invention, the voltage of the charged battery cell in step (1) is 4-4.2V, for example, it can be 4V, 4.1V or 4.2V.
[0014] It should be noted that in response to the needs of electrode analysis and characterization, the fully charged negative electrode is obtained by disassembling the charged battery cell. The color is golden yellow, which is easier to identify electrode defects (such as lithium deposition, poor lithium insertion, self-discharge black spots or electrode black spots, etc.) than the black state of the negative electrode after discharge, and is conducive to locating the cause of the abnormality.
[0015] As a preferred technical solution of the present invention, the atmosphere of the oxidation treatment in step (2) is an oxygen-containing atmosphere.
[0016] In the present invention, a large amount of lithium will be embedded in the fully charged negative electrode sheet, most of which exists in the form of lithium carbide, and a small part exists in the form of metallic lithium. Since metallic lithium is very active, if it is not oxidized, it will react with water directly to produce hydrogen and a large amount of heat, and the electrode will spontaneously combust and destroy the sample.
[0017] Preferably, the oxygen-containing atmosphere is an air atmosphere or an oxygen atmosphere.
[0018] As a preferred technical solution of the present invention, the temperature of the oxidation treatment in step (2) is 20-30°C, for example, 20°C, 25°C or 30°C.
[0019] In the present invention, if the temperature of the oxidation treatment is too low, the oxidation efficiency is slow and the time cost required to achieve the same degree of oxidation increases; if the temperature of the oxidation treatment is too high, the electrode is easily brittle, and the Cu collector structure is unstable, and floating powder falls off, affecting the experimental error.
[0020] Preferably, the oxidation treatment time in step (2) is 18-30 hours, for example, it can be 18 hours, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours or 30 hours.
[0021] As a preferred technical solution of the present invention, during the oxidation treatment in step (2), the ambient humidity is 30-70%, for example, 30%, 40%, 50%, 60% or 70%.
[0022] In the present invention, the oxidation treatment is performed under the condition of an ambient humidity of 30-70%, which is conducive to the slow reaction of the Li element in the electrode with the water molecules in the air, and finally achieves the oxidation effect, and the electrode will not spontaneously combust.
[0023] As a preferred technical solution of the present invention, the water immersion treatment in step (3) is accompanied by ultrasound.
[0024] Preferably, the frequency of the ultrasound is 20-40 kHz, for example, 20 kHz, 30 kHz or 40 kHz.
[0025] As a preferred technical solution of the present invention, the drying temperature in step (3) is 45-80°C, for example, it can be 45°C, 50°C, 60°C, 70°C or 80°C.
[0026] Preferably, the drying time in step (3) is 2-5 days, for example, 2 days, 3 days, 4 days or 5 days.
[0027] Preferably, the post-processing step in step (3) includes: scraping the negative electrode powder with a ceramic knife.
[0028] As a preferred technical solution of the present invention, the collection method comprises the following steps:
[0029] (1) disassembling the charged battery cell to obtain a fully charged negative electrode sheet;
[0030] (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0031] The oxidation treatment temperature is 20-30°C, the oxidation treatment time is 18-30h, and the ambient humidity is 30-70%;
[0032] (3) mixing the oxidized negative electrode sheet with deionized water, and then placing it in an ultrasonic device with a frequency of 20-40 kHz for ultrasonic treatment, leaving it for 0.5-1.5 hours after the ultrasonic treatment, and then placing the obtained water-containing powder in an oven at 45-80° C. and drying it for 2-5 days to obtain a block powder;
[0033] (4) Using a ceramic knife to make the block powder into powder to obtain the negative electrode powder.
[0034] In a second aspect, the present invention provides a negative electrode powder, which is collected by the collection method described in the first aspect.
[0035] In a third aspect, the present invention provides a use of the negative electrode powder as described in the second aspect in analyzing the cause of battery failure.
[0036] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] The invention directly oxidizes the fully charged negative electrode sheet, which can oxidize the metallic lithium embedded in the charged negative electrode sheet, making it unable to react and produce hydrogen during the subsequent water immersion treatment, thereby preventing the electrode sheet from spontaneously igniting. In addition, the negative electrode powder obtained by this collection method can avoid the mixing of Cu particles in the current collector, effectively improving the purity of the negative electrode powder, which improves the test accuracy of the inductively coupled plasma emission spectroscopy ICP test of magnetic metal elements, can be used to analyze the reasons for low voltage or large self-discharge of the battery, and is an important means of analyzing battery failure. The recovery rate of the negative electrode powder obtained based on this collection method is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a process flow chart for collecting negative electrode powder provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0041] It should be noted that the following negative electrode powders are collected by disassembling charged cells with a K value (the larger the K value, the greater the self-discharge, and the standard is 0.08) of 0.04. The following fully charged negative electrode sheets (i.e., the voltage is 4.18V) are all composed of copper foil coated with graphite negative electrode material.
[0042] Example 1
[0043] This embodiment provides a method for collecting negative electrode powder of lithium ion batteries, and its process flow chart is as follows: Figure 1 As shown, the collection method comprises the following steps:
[0044] (1) disassembling a charged battery cell with a voltage of 4.2 V to obtain a fully charged negative electrode sheet;
[0045] (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0046] The oxidation treatment temperature is 25°C, the oxidation treatment time is 24h, and the ambient humidity is 50%;
[0047] (3) The oxidized negative electrode sheet and deionized water are mixed in a beaker, and then placed in an ultrasonic device with a frequency of 40 kHz for ultrasonic water immersion treatment. After the ultrasonic treatment is completed, the mixture is left for 1 hour, and then the obtained water-containing powder is distributed into a small culture dish and placed in an oven at 60° C. for drying for 3 days to obtain a block powder;
[0048] If there is any solute (i.e., residue of negative electrode powder) remaining in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute remains;
[0049] (4) Using a ceramic knife, the block powder finally obtained in step (3) is powdered to obtain the negative electrode powder.
[0050] Example 2
[0051] This embodiment provides a method for collecting negative electrode powder of a lithium ion battery, the collecting method comprising the following steps:
[0052] (1) disassembling a charged battery cell with a voltage of 4.2 V to obtain a fully charged negative electrode sheet;
[0053] (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0054] The oxidation treatment temperature is 20°C, the oxidation treatment time is 30h, and the ambient humidity is 30%;
[0055] (3) The oxidized negative electrode sheet and deionized water are mixed in a beaker, and then placed in an ultrasonic device with a frequency of 20 kHz for ultrasonic water immersion treatment. After the ultrasonic treatment is completed, the mixture is left for 1.5 hours. The obtained water-containing powder is then distributed into a small culture dish and placed in an oven at 45° C. for drying for 3 days to obtain a block powder.
[0056] If there are any solute residues in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute residues remain;
[0057] (4) Using a ceramic knife, the block powder finally obtained in step (3) is powdered to obtain the negative electrode powder.
[0058] Example 3
[0059] This embodiment provides a method for collecting negative electrode powder of a lithium ion battery, the collecting method comprising the following steps:
[0060] (1) disassembling a charged battery cell with a voltage of 4.2 V to obtain a fully charged negative electrode sheet;
[0061] (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0062] The oxidation treatment temperature is 30°C, the oxidation treatment time is 18h, and the ambient humidity is 70%;
[0063] (3) The oxidized negative electrode sheet and deionized water were mixed in a beaker, and then placed in an ultrasonic device with a frequency of 60 kHz for ultrasonic water immersion treatment. After the ultrasonic treatment was completed, the mixture was left aside for 0.5 h. The obtained water-containing powder was then distributed into a small culture dish and placed in an oven at 80° C. for drying for 3 days to obtain a block powder.
[0064] If there are any solute residues in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute residues remain;
[0065] (4) Using a ceramic knife, the block powder finally obtained in step (3) is powdered to obtain the negative electrode powder.
[0066] Example 4
[0067] This embodiment provides a method for collecting negative electrode powder of a lithium ion battery, the collecting method comprising the following steps:
[0068] (1) disassembling a charged battery cell with a voltage of 4.2 V to obtain a fully charged negative electrode sheet;
[0069] (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0070] The oxidation treatment temperature is 25°C, the oxidation treatment time is 12h, and the ambient humidity is 50%;
[0071] (3) The oxidized negative electrode sheet and deionized water were mixed in a beaker, and then placed in an ultrasonic device with a frequency of 40 kHz for ultrasonic water immersion treatment. After the ultrasonic treatment was completed, the mixture was left aside for 0.5 h. The obtained water-containing powder was then distributed into a small culture dish and placed in an oven at 60° C. for drying for 3 days to obtain a block powder.
[0072] If there are any solute residues in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute residues remain;
[0073] (4) Using a ceramic knife, the block powder finally obtained in step (3) is powdered to obtain the negative electrode powder.
[0074] Example 5
[0075] This embodiment provides a method for collecting negative electrode powder of a lithium ion battery, the collecting method comprising the following steps:
[0076] (1) disassembling a charged battery cell with a voltage of 4.2 V to obtain a fully charged negative electrode sheet;
[0077] (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0078] The oxidation treatment temperature is 10°C, the oxidation treatment time is 24h, and the ambient humidity is 50%;
[0079] (3) The oxidized negative electrode sheet and deionized water are mixed in a beaker, and then placed in an ultrasonic device with a frequency of 40 kHz for ultrasonic water immersion treatment. After the ultrasonic treatment is completed, the mixture is left for 1 hour, and then the obtained water-containing powder is distributed into a small culture dish and placed in an oven at 60° C. for drying for 3 days to obtain a block powder;
[0080] If there are any solute residues in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute residues remain;
[0081] (4) Using a ceramic knife, the block powder finally obtained in step (3) is powdered to obtain the negative electrode powder.
[0082] Example 6
[0083] This embodiment provides a method for collecting negative electrode powder of a lithium ion battery, the collecting method comprising the following steps:
[0084] (1) disassembling a charged battery cell with a voltage of 4.2 V to obtain a fully charged negative electrode sheet;
[0085] (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0086] The oxidation treatment temperature is 50°C, the oxidation treatment time is 24h, and the ambient humidity is 50%;
[0087] (3) The oxidized negative electrode sheet and deionized water are mixed in a beaker, and then placed in an ultrasonic device with a frequency of 40 kHz for ultrasonic water immersion treatment. After the ultrasonic treatment is completed, the mixture is left for 1 hour, and then the obtained water-containing powder is distributed into a small culture dish and placed in an oven at 60° C. for drying for 3 days to obtain a block powder;
[0088] If there are any solute residues in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute residues remain;
[0089] (4) Using a ceramic knife, the block powder finally obtained in step (3) is powdered to obtain the negative electrode powder.
[0090] Comparative Example 1
[0091] This comparative example provides a method for collecting negative electrode powder of a lithium ion battery, and the collection method comprises the following steps:
[0092] (1) disassembling the charged battery cell to obtain a fully charged negative electrode sheet;
[0093] (2) mixing the fully charged negative electrode sheet with deionized water, and then placing it in an ultrasonic device with a frequency of 40 kHz for ultrasonic water immersion treatment, leaving it for 1 hour after the ultrasonic treatment, and then placing the obtained water-containing powder in an oven at 60° C. and drying it for 3 days to obtain a block powder;
[0094] If there are any solute residues in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute residues remain;
[0095] (3) Using a ceramic knife, the block powder finally obtained in step (3) is made into powder to obtain the negative electrode powder.
[0096] Comparative Example 2
[0097] This comparative example provides a method for collecting negative electrode powder of a lithium ion battery, and the collection method comprises the following steps:
[0098] (1) disassembling the discharged battery cell to obtain a negative electrode sheet;
[0099] (2) placing the negative electrode sheet in a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet;
[0100] The oxidation treatment temperature is 25°C, the oxidation treatment time is 24h, and the ambient humidity is 50%;
[0101] (3) mixing the oxidized negative electrode sheet with deionized water, and then placing it in an ultrasonic device with a frequency of 40 kHz for ultrasonic water immersion treatment, leaving it for 1 hour after the ultrasonic treatment, and then placing the obtained water-containing powder in an oven at 60° C. and drying it for 3 days to obtain a block powder;
[0102] If there are any solute residues in the culture dish, ultrasonic water immersion treatment and drying are performed again until no solute residues remain;
[0103] (4) Using a ceramic knife, the block powder finally obtained in step (3) is powdered to obtain the negative electrode powder.
[0104] Comparative Example 3
[0105] This comparative example provides a method for collecting negative electrode powder of a lithium ion battery, and the collection method comprises the following steps:
[0106] Use a ceramic knife to scrape and collect the graphite coating on the surface of the negative electrode, and collect the entire negative electrode sheet powder.
[0107] Performance Testing
[0108] 1. Inductively coupled plasma luminescence spectrometry (ICP) was used to test the content of magnetic metal elements in the negative electrode powders collected in the above embodiments and comparative examples.
[0109] The test results are shown in Table 1.
[0110] Table 1
[0111] Cu / ppm Example 1 20.354 Example 2 22.349 Example 3 43.652 Example 4 21.235 Example 5 22.654 Example 6 32.234 Comparative Example 1 / Comparative Example 2 23.467 Comparative Example 3 500.234
[0112] Note: K value refers to the voltage drop of the battery per unit time. It is an indicator used to measure the self-discharge rate of lithium batteries. A K value less than 0.08 indicates that the battery is in good condition.
[0113] analyze:
[0114] As can be seen from the above table, the collection method provided by the present invention can accurately and quickly collect negative electrode powder, and through Examples 1-4, based on the test analysis of the collected negative electrode powder of the present invention, it can be seen that the test results of the battery with a K value of 0.04 show that none of them failed, and the test results are consistent with the actual situation. In addition, the test analysis results of the negative electrode powder collected by the collection method provided in Example 4 are more accurate and the test efficiency is the fastest.
[0115] It can be seen from Examples 1 and 5-6 that if the temperature of the oxidation treatment is too low, the oxidation efficiency is slow, and the time cost of obtaining the negative electrode powder increases, which is not conducive to practical application; if the temperature of the oxidation treatment is too high, the electrode may spontaneously combust. This is because the higher the temperature, the more violent the movement of water molecules, and the more water molecules enter the sealed bag and react with Li per unit time in the same pore; in addition, the copper foil will be oxidized and its crystal structure will be destroyed, indicating that there will be a certain amount of residual powder, resulting in an increase in the experimental error.
[0116] It can be seen from Example 3 that when the ultrasonic frequency is as high as 60KHZ, there is a certain amount of floating powder vibration and the experimental error is large.
[0117] It can be seen from Example 1 and Comparative Example 1 that if the fully charged negative electrode plate is not oxidized, the plate will catch fire and self-ignite, making it impossible to conduct the experiment.
[0118] It can be seen from Example 1 and Comparative Example 2 that if the discharged battery cell is disassembled, there is no obvious difference in the error, but disassembling the fully charged battery cell is more conducive to failure analysis and has certain advantages in identifying more failure modes.
[0119] It can be seen from Example 1 and Comparative Example 3 that the use of a ceramic knife for scraping will cause Cu powder to be mixed into the negative electrode powder over a large area, causing the test results of cells with normal K values to appear abnormal, seriously affecting the accuracy of the experiment and the judgment of the failure mode.
[0120] 2. The recovery rate of the negative electrode powder collected in the above embodiments and comparative examples was tested. It is known that the elements in the negative electrode powder mainly include C, O and Si. When testing ICP, the proportion of all elements (including impurity element Cu) needs to be tested, as shown in Table 2. It is also known that the fixed volume is V0, the fixed volume conversion ratio is K, the volume required for the sample to be placed in the ICP is V1, the mass of the negative electrode powder required to produce a battery cell is M0, and the weight of the negative electrode powder finally obtained is M1. The recovery rate = (M1-(C4×NA×K×(V0 / V1)×M1)) / M0.
[0121] Table 2
[0122]
[0123]
[0124] Table 3
[0125]
[0126] It can be seen from the above table that the negative electrode powder obtained by the collection method provided by the present invention not only has less impurities and high purity, but also has a high recovery rate, and has good development potential.
[0127] 3. The collection method provided in Example 4 was used to disassemble the charged cells with K values of 0.05 and 0.15 under the same conditions, and the cause of the poor K value of the battery was determined to be caused by bottom welding spatter.
[0128] The magnetic metal element content of the collected negative electrode powder was tested using inductively coupled plasma emission spectrometry (ICP).
[0129] The test results are shown in Table 4.
[0130] Table 4
[0131]
[0132] analyze:
[0133] It can be seen from the above table that the collection method provided by the present invention can accurately analyze the reasons for low voltage or large self-discharge of the battery for charged cells in different situations, and identify the failure difference between cells with poor K values and normal cells. It can effectively determine that the root cause of the large K value and abnormal self-discharge is the excessively high Cu content. As a result, during the charge and discharge process, Cu dissolves, oxidizes, and reduces and precipitates, and finally evolves into copper dendrites that pierce the diaphragm and cause a micro-short circuit, thereby causing abnormal self-discharge of the battery cell.
[0134] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for collecting negative electrode powder of lithium ion batteries, characterized in that: The collection method comprises the following steps: (1) disassembling the charged battery cell to obtain a fully charged negative electrode sheet; (2) subjecting the fully charged negative electrode sheet to oxidation treatment to obtain an oxidized negative electrode sheet; (3) The oxidized negative electrode sheet is subjected to water immersion treatment, dried, and collected after post-treatment to obtain the negative electrode powder of the lithium ion battery.
2. The method for collecting negative electrode powder of lithium ion batteries according to claim 1, characterized in that: The voltage of the charged battery cell in step (1) is 4-4.2V.
3. The method for collecting negative electrode powder of lithium ion batteries according to claim 1 or 2, characterized in that: The atmosphere of the oxidation treatment in step (2) is an oxygen-containing atmosphere; Preferably, the oxygen-containing atmosphere is an air atmosphere or an oxygen atmosphere.
4. The method for collecting negative electrode powder of lithium ion batteries according to any one of claims 1 to 3, characterized in that: The temperature of the oxidation treatment in step (2) is 20-30°C; Preferably, the oxidation treatment time in step (2) is 18-30 hours.
5. The method for collecting negative electrode powder of lithium ion batteries according to any one of claims 1 to 4, characterized in that: During the oxidation treatment in step (2), the ambient humidity is 30-70%.
6. The method for collecting negative electrode powder of lithium ion batteries according to any one of claims 1 to 5, characterized in that: The water immersion treatment in step (3) is accompanied by ultrasound; Preferably, the frequency of the ultrasound is 20-40 kHz.
7. The method for collecting negative electrode powder of lithium ion batteries according to any one of claims 1 to 6, characterized in that: The drying temperature in step (3) is 45-80°C; Preferably, the drying time in step (3) is 2-5 days; Preferably, the post-processing step in step (3) includes: scraping the negative electrode powder with a ceramic knife.
8. The method for collecting negative electrode powder of lithium ion batteries according to any one of claims 1 to 7, characterized in that: The collection method comprises the following steps: (1) disassembling the charged battery cell to obtain a fully charged negative electrode sheet; (2) placing the fully charged negative electrode sheet into a sealed bag and performing oxidation treatment in an oxygen-containing atmosphere to obtain an oxidized negative electrode sheet; The oxidation treatment temperature is 20-30°C, the oxidation treatment time is 18-30h, and the ambient humidity is 30-70%; (3) mixing the oxidized negative electrode sheet with deionized water, and then placing it in an ultrasonic device with a frequency of 20-40 kHz for ultrasonic treatment, leaving it for 0.5-1.5 hours after the ultrasonic treatment, and then placing the obtained water-containing powder in an oven at 45-80° C. and drying it for 2-5 days to obtain a block powder; (4) Using a ceramic knife to make the block powder into powder to obtain the negative electrode powder.
9. A negative electrode powder, characterized in that: The negative electrode powder is collected by the collection method according to any one of claims 1 to 8.
10. Use of the negative electrode powder as claimed in claim 9 in analyzing the cause of battery failure.
Citation Information
Cited By
Method for recovering lithium salt in state-of-charge waste lithium ion battery
CN122267347A