GSH (at) Fe3O4 / GSH (at) AAO membrane modified micro-nano channel electrode and application thereof in cadmium ion detection
By adhering the GSH@Fe3O4/GSH@AAO composite film to the screen printing electrode, the accuracy and stability of cadmium ion detection are solved, and the cadmium ion detection effect with high sensitivity and low detection limit is achieved.
Patent Information
- Application Number
- CN202411014721.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The existing cadmium ion detection methods are susceptible to interference from other substances, have poor detection accuracy, insufficient stability of homemade electrodes, and there is no document for cadmium ion detection using porous anodized aluminum oxide (AAO) film or its modified film.
Glutathione (GSH) and iron tetraoxide (Fe3O4) nanoparticles were used to form a GSH@Fe3O4/GSH@AAO composite film, and adhere it to the screen printed electrode to form a modified electrode for use in the Cadmium ion detection.
It realizes fast and accurate detection of cadmium ions, high sensitivity, extremely low detection limit, excellent stability and reproducibility, simple operation, and reduces production costs.
Smart Images

Figure CN118961827A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a GSH@Fe3O4 / GSH@AAO film-modified micro-nano channel electrode and application thereof in cadmium ion detection, belonging to the technical field of electrochemical sensors and food safety detection. Background Art
[0002] With the continuous advancement of industrialization and agriculturalization, environmental pollution problems are becoming increasingly serious, especially heavy metal pollution. Cadmium (Cd), as a highly toxic heavy metal element, is widely present in nature and industrial waste. After entering the human body through the food chain, it can cause serious damage to organs such as the kidneys and liver. Therefore, the development of an efficient, sensitive and simple cadmium ion detection method is of great significance for environmental monitoring and food safety.
[0003] Traditional methods for detecting cadmium ions include atomic absorption spectroscopy, fluorescence, and inductively coupled plasma mass spectrometry. Although these methods are highly sensitive, they usually require expensive instruments and complex sample processing and are not suitable for rapid on-site detection.
[0004] At present, some methods using screen-printed electrodes to detect cadmium ions have emerged, such as: the literature (Barton J, García, María Begoa González, Santos, David Hernández, et al. Screen-printed electrodes for environmental monitoring of heavy metal ions: a review [J]. Microchimica Acta, 2016, 183 (2): 503-517. DOI: 10.1007 / s00604-015-1651-0.) discloses mercury-coated SPE and gold-coated SPE, which are based on mercury and gold for the detection of cadmium ions; the literature (P. Pasakon; W. Kamsong; V. Primpray; A. Wisitsoraat; T. Lomas; A. Tuantranont; C. Karuwan. Simultaneous electrochemical sensing of Cd 2+ and Pb 2+using screen-printed ionic liquid / graphene electrodes[J].International JournalofEnvironmentalAnalyticalChemistry,:1-1) discloses that ionic liquid / graphene electrodes are used to modify SPE to improve detection sensitivity and selectivity; the literature (Haidong Xing;Xiangxiang Zhang;Siyao Zhai;Wei Mu;Chao Li;Xiaojun Han.Screen-printed electrode containing bismuth / graphene oxide hybrid for simultaneous detection of cadmium and lead ions[J].Journal ofElectroanalyticalChemistry,2024,Vol.961:118222) discloses the use of the synergistic effect of bismuth and graphene oxide to enhance the detection ability of cadmium ions; however, these methods have low accuracy for cadmium ions, poor sensitivity, small detection range, and relatively complicated operation.
[0005] Micro-nanochannel electrochemical sensing technology has become an emerging detection method due to its unique physicochemical properties, such as high specific surface area, high mass transfer efficiency and excellent electrochemical performance. Among them, porous anodic aluminum oxide (AAO) membrane is a typical nanochannel array with a high-density nanochannel structure. Compared with single nanopores, porous AAO membranes can provide several orders of magnitude larger ion current changes, thereby significantly improving the sensitivity and response speed of the sensor. The nanochannel size of the porous AAO membrane is controllable and similar to the size of the molecule to be detected, enabling high selectivity and high-precision detection. This structure not only increases the detection surface area, but also improves the detection efficiency and accuracy. The high specific surface area of the nanochannel allows more target molecules to contact the electrode surface, enhancing the intensity of the electrochemical signal.
[0006] In order to enhance the accuracy of porous anodic aluminum oxide (AAO) membranes for electrochemical detection, metal or metal oxide nanoparticles are conventionally deposited in the nanopores of the AAO membranes so that the nanoparticles can be used as adsorbents or catalysts for cadmium ions to enhance the effect of electrochemical detection. Some methods also use organic molecules such as thiol compounds and alkynyl compounds to functionalize the AAO membranes to increase the affinity for the detected substances. However, different substances have different properties and different requirements for detection. Currently, no literature has been found on the use of porous anodic aluminum oxide (AAO) membranes or modified porous anodic aluminum oxide (AAO) membranes to detect cadmium ions. Summary of the invention
[0007] [Technical issues]
[0008] Although the electrochemical detection method is convenient for on-site application, it is easily interfered by other substances, which affects the accuracy of the detection;
[0009] The lack of stability of homemade electrodes may also interfere with the test results;
[0010] No literature was found that used porous anodic aluminum oxide (AAO) membrane or modified porous anodic aluminum oxide (AAO) membrane to detect cadmium ions.
[0011] [Technical solution]
[0012] In order to solve the above problems, the present invention first uses glutathione (GSH, CAS: 70-18-8) combined with ferroferric oxide (Fe3O4) to obtain GSH@Fe3O4 nanoparticles; glutathione (GSH) combines with micro-nano channel membrane (AAO) to form GSH@AAO membrane; then GSH@Fe3O4 nanoparticles are loaded on the GSH@AAO membrane to form a functionalized GSH@Fe3O4 / GSH@AAO composite membrane; then the functionalized GSH@Fe3O4 / GSH@AAO composite membrane is adhered to the surface of the screen-printed electrode using conductive glue to form a modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE); finally, the modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) is used to detect cadmium ions. The method of the present invention can be used for rapid and accurate detection of Cd2+ content, is simple to operate, has high sensitivity and extremely low detection limit, and has excellent stability and reproducibility.
[0013] The first object of the present invention is to provide a method for preparing a functionalized GSH@Fe3O4 / GSH@AAO composite membrane, comprising the following steps:
[0014] (1) Preparation of GSH@Fe3O4 nanoparticles:
[0015] The Fe3O4 nanoparticles were dispersed in anhydrous ethanol, and then water was added for ultrasonic treatment; reduced glutathione was added and the ultrasonic treatment was continued; finally, a magnet was used to collect, wash, and dry the nanoparticles to obtain GSH@Fe3O4;
[0016] (2) Preparation of GSH@AAO membrane:
[0017] The anodic aluminum oxide (AAO) film is immersed in a NaOH solution for treatment, and then taken out; then placed in a (3-aminopropyl) triethoxysilane (APTES) solution for treatment, and after the treatment is completed, washed to obtain a treated anodic aluminum oxide (AAO) film;
[0018] The treated anodic aluminum oxide (AAO) membrane was incubated in a MES buffer solution of N-hydroxysuccinimide (NHS), and then incubated in a glutathione (GSH) solution to obtain a GSH@AAO membrane.
[0019] (3) Preparation of GSH@Fe3O4 / GSH@AAO composite membrane:
[0020] dispersing GSH@Fe3O4 nanoparticles in water to form a GSH@Fe3O4 nanoparticle suspension;
[0021] The GSH@Fe3O4 nanoparticle suspension was dropped onto the GSH@AAO membrane and dried to obtain the functionalized GSH@Fe3O4 / GSH@AAO composite membrane.
[0022] In one embodiment of the present invention, in step (1), the dosage ratio of Fe3O4 nanoparticles, anhydrous ethanol, water, and reduced glutathione is 1.0 g: 10 mL: 30 mL: 0.4 g.
[0023] In one embodiment of the present invention, the dispersion in step (1) is performed by stirring at a speed of 200-500 rpm.
[0024] In one embodiment of the present invention, the ultrasound after adding water in step (1) is performed at 20-30° C. and 35-45 kW for 1.5-2.5 h.
[0025] In one embodiment of the present invention, the continued ultrasonication in step (1) is carried out at 20-30° C. and 35-45 kW for 0.5-1.5 h.
[0026] In one embodiment of the present invention, the washing in step (1) is washing with water.
[0027] In one embodiment of the present invention, the drying in step (1) is vacuum drying at 55-65° C. for 6-10 h.
[0028] In one embodiment of the present invention, the anodized aluminum oxide (AAO) film and the screen-printed electrode in step (2) are of the same size.
[0029] In one embodiment of the present invention, the NaOH solution in step (2) is a NaOH aqueous solution with a concentration of 0.2-0.3%, more preferably 0.25%, where % is mass percentage.
[0030] In one embodiment of the present invention, the treatment in the NaOH solution in step (2) is an ultrasonic treatment, specifically a treatment at 35-45 kW for 1-3 min, in order to improve the hydrophilicity.
[0031] In one embodiment of the present invention, the concentration of the (3-aminopropyl)triethoxysilane (APTES) solution in step (2) is 4-6%, the solvent is anhydrous ethanol, and % is volume percentage.
[0032] In one embodiment of the present invention, the treatment in the (3-aminopropyl)triethoxysilane (APTES) solution in step (2) is carried out at 20-30° C. for 1.5-2.5 h, in order to ensure that the APTES molecules fully form silicon-oxygen bonds with the AAO surface.
[0033] In one embodiment of the present invention, the washing in step (2) is performed with anhydrous ethanol to remove unreacted APTES.
[0034] In one embodiment of the present invention, the concentration of N-hydroxysuccinimide (NHS) in the MES buffer solution of N-hydroxysuccinimide (NHS) in step (2) is 0.05-0.15 M, and the pH of the MES buffer solution is 5-6.
[0035] In one embodiment of the present invention, incubation in a MES buffer solution of N-hydroxysuccinimide (NHS) in step (2) is carried out at 20-30° C. for 1-3 h; the surface of the AAO membrane is chemically modified using a MES buffer solution of N-hydroxysuccinimide (NHS); NHS is an activation reagent that can effectively react with hydroxyl groups on the membrane surface to form a stable imide bond; the formation of such a bond provides the necessary activation sites for subsequent biomolecule grafting, allowing glutathione to be firmly bound to the membrane surface; incubation in a MES buffer solution of pH 5-6 can optimize the efficiency of the NHS activation process, ensure the maximum activation of hydroxyl groups on the surface of the AAO membrane, and thus enhance the functionalization effect of the membrane.
[0036] In one embodiment of the present invention, the concentration of the glutathione (GSH) solution in step (2) is 4-6 mM, and the solvent is water.
[0037] In one embodiment of the present invention, the incubation in the glutathione (GSH) solution in step (2) is carried out at 20-30° C. for 0.5-1.5 h.
[0038] In one embodiment of the present invention, the concentration of the GSH@Fe3O4 nanoparticle suspension in step (3) is 0.5-1.5 mg / mL.
[0039] In one embodiment of the present invention, the amount of GSH@Fe3O4 nanoparticle suspension on the GSH@AAO membrane in step (3) is 5-15 μL / 6.25πmm 2 .
[0040] In one embodiment of the present invention, the drying in step (3) is performed at 40-60° C. for 20-40 min.
[0041] The second object of the present invention is the functionalized GSH@Fe3O4 / GSH@AAO composite membrane prepared by the method described in the present invention.
[0042] The third object of the present invention is to provide a method for preparing a modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE), comprising the following steps:
[0043] The magnetic material (flexible magnet sheet) was first pasted on the surface of the screen-printed electrode using conductive glue, and then the functionalized GSH@Fe3O4 / GSH@AAO composite film was pasted on the surface of the magnetic material (flexible magnet sheet) using conductive glue. Then, the surface was sealed all around with sealant and dried to obtain the modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE).
[0044] In one embodiment of the present invention, the magnetic material is a flexible magnet sheet with a thickness of 0.4-0.6 mm.
[0045] In one embodiment of the present invention, the conductive adhesive is silver conductive adhesive.
[0046] In one embodiment of the present invention, the sealant is a silicone sealant.
[0047] The fourth object of the present invention is to provide a modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) which uses the functionalized GSH@Fe3O4 / GSH@AAO composite film of the present invention.
[0048] A fifth object of the present invention is to provide a method for preparing an electrochemical sensor based on micro-nano channels and screen printing, comprising the following steps:
[0049] The modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) was used as the working electrode, and the working electrode, reference electrode and counter electrode were respectively connected to a portable electrochemical workstation to form an electrochemical sensor based on micro-nano channels and screen printing.
[0050] In one embodiment of the present invention, the reference electrode is Ag / AgCl and the counter electrode is a platinum wire.
[0051] The sixth object of the present invention is to provide an electrochemical sensor based on micro-nano channels and screen printing, which adopts the functionalized GSH@Fe3O4 / GSH@AAO composite film or modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) described in the present invention.
[0052] The seventh object of the present invention is to provide a method for detecting cadmium ions using an electrochemical sensor based on micro-nano channels and screen printing, comprising the following steps:
[0053] The test solution containing cadmium ions is dropped onto the working electrode of the micro-nano channel and screen-printed electrochemical sensor to detect the cadmium ions using the DPV method.
[0054] In one embodiment of the present invention, the parameters of the DPV method are set as follows: calibration time 1 s, test voltage -0.5 V to 0 V, step potential 0.01 V, scan rate 0.002 V / s., pH 5.
[0055] In one embodiment of the present invention, the amount of the solution to be tested containing cadmium ions is 5-15 μL / 6.25πmm 2 .
[0056] In one embodiment of the present invention, the concentration of cadmium ions in the test solution containing cadmium ions is 5 μg / L-120 μg / L.
[0057] In one embodiment of the present invention, the detection limit of the method of the present invention is 0.1 μg / L.
[0058] The eighth objective of the present invention is the application of the functionalized GSH@Fe3O4 / GSH@AAO composite film, the modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) or the electrochemical sensor based on micro-nano channels and screen printing described in the present invention in the field of electrochemical detection.
[0059] In one embodiment of the present invention, the application is for detecting cadmium ions.
[0060] [Beneficial Effects]
[0061] (1) The present invention adopts a simplified structure and a low-cost preparation method, and directly applies the micro-nano channel membrane modified with ferroferric oxide and glutathione to the screen-printed electrode, which not only reduces the production cost but also provides mild reaction conditions.
[0062] (2) The unique structure of the micro-nano channel used in the present invention increases the surface area and provides more capture sites for cadmium ions, thereby improving the sensitivity and detection efficiency of the sensor.
[0063] (3) The electrochemical sensor prepared by the present invention can respond quickly and complete the detection of cadmium ions almost immediately.
[0064] (4) The glutathione used in the present invention provides a highly selective recognition site, which, combined with the signal enhancement effect of ferroferric oxide, enables the sensor to show high sensitivity and an extremely low detection limit, which is as low as 0.1 μg / L.
[0065] (5) The electrochemical sensor prepared by the present invention has excellent stability and reproducibility, which can further ensure the accuracy and reliability of cadmium ion detection data.
[0066] (6) The present invention integrates surface modification and nanotechnology to improve the biocompatibility and functionality of GSH@Fe3O4 / GSH@AAO composite films for advanced sensing applications.
[0067] (7) The design of the working electrode in the electrochemical sensor of the present invention enables the micro-nano channels of the anodized aluminum film to effectively capture target molecules; the use of magnetic materials (flexible magnet sheets) enables the ferroferric oxide nanoparticles to adhere more firmly to the surface of the anodized aluminum film, thereby improving the stability and durability of the composite material; this enhanced adhesion not only ensures the reliability of the electrochemical sensor during long-term use or in harsh environments, but also promotes more efficient electron transfer and enhances the electrochemical activity of the sensor. Therefore, this composite structure based on micro-nano channels and magnetic nanoparticles exhibits significant advantages in improving sensing sensitivity and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] Figure 1 The present invention is a flow chart of the cadmium ion detection method based on micro-nano channels and screen-printed electrochemical sensors.
[0069] Figure 2 This is the effect of different ultrasonic treatment times on the water contact angle of porous anodic aluminum oxide membrane (AAO) in Comparative Example 1.
[0070] Figure 3 Figure 3 is the microstructural evolution of the anodized aluminum oxide (AAO) surface modified by glutathione (GSH) and glutathione combined with ferrous oxide (GSH@Fe3O4); where a is the surface of anodized aluminum oxide (AAO) at a magnification of 10,000 times; b is AAO modified with glutathione (GSH) at a magnification of 10,000 times; cf are scanning electron microscope (SEM) images of GSH@Fe3O4 / GSH@AAO film at magnifications of 350, 1000, 3500, and 5000.
[0071] Figure 4Comparison of infrared absorption spectra of unmodified and modified anodic aluminum oxide (AAO) films; curve a is anodic aluminum oxide (AAO); curve b is glutathione-modified anodic aluminum oxide (GSH@AAO); curve c is glutathione-bound ferrous oxide-modified anodic aluminum oxide (GSH@Fe3O4 / AAO).
[0072] Figure 5 X-ray diffraction analysis for crystal structure comparison of anodized aluminum film and its modified forms.
[0073] Figure 6 Cyclic voltammetric responses of GSH@Fe3O4 / GSH@AAO / SPCE electrode at different rates (20 mV / s to 140 mV / s); the inset shows the linear relationship between peak current and scan rate.
[0074] Figure 7 These are the cyclic voltammetric electrochemical characterization diagrams of bare electrode, GSH@AAO / SPCE, GSH@Fe3O4 / SPCE, and GSH@Fe3O4 / GSH@AAO / SPCE during the electrode modification process.
[0075] Figure 8 These are the AC impedance diagrams (Nyquist diagrams) of bare electrode, GSH@AAO / SPCE, GSH@Fe3O4 / SPCE, and GSH@Fe3O4 / GSH@AAO / SPCE during the electrode modification process.
[0076] Fig. 9 These are the response diagrams of bare electrode, GSH@AAO / SPCE, GSH@Fe3O4 / SPCE, and GSH@Fe3O4 / GSH@AAO / SPCE to cadmium ion signals in buffer solution during the electrode modification process.
[0077] Fig.10 Cyclic voltammetric response of 3 mM / L potassium ferrocyanide on AAO membrane combined with screen-printed electrode at a scan rate of 100 mV / s.
[0078] Fig.11 The differential pulse voltammetry (DPV) response curves of cadmium ions at different concentrations, and the inset shows the linear relationship between the current response and the concentration.
[0079] Fig.12 This is the current response of cadmium ions at different pH values in differential pulse voltammetry (DPV), and the inset is the relationship between the current peak and pH value.
[0080] Fig.13 This is the cyclic voltammetry response curve of cadmium ions at different scan rates of differential pulse voltammetry (DPV), and the inset shows the change of current peak with scan rate.
[0081] Fig.14 These are the stability test results of the modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE).
[0082] Fig.15 This is the specific detection result of the modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE). DETAILED DESCRIPTION
[0083] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0084] The raw materials used in the examples are:
[0085] AOO membrane: pore size 390nm, thickness 50μm, diameter 5mm;
[0086] Screen-printed electrode: 5 mm in diameter;
[0087] Fe3O4 nanoparticles: particle size 20 nm, purchased from Shanghai MacLean Biochemical Materials Co., Ltd.;
[0088] Reduced glutathione: 98%, reduced type, purchased from Aladdin Reagent Co., Ltd. (Shanghai, China);
[0089] MES buffer solution: pH 5.5;
[0090] Silver nano-glue: K-181 conductive glue was purchased from Zhuhai Jinsineng Technology Co., Ltd.;
[0091] Silicone sealant: Kraft K-705 was purchased from Guangdong Hengda New Materials Co., Ltd.;
[0092] Magnetic material (flexible magnet sheet): Use a hole puncher to cut a 0.5 mm thick flexible magnetic sheet (iron sheet) into round pieces with a diameter of 3 mm.
[0093] The solutions mentioned in the examples and comparative examples without specifying the solvent used are water.
[0094] Example 1
[0095] A method for preparing a functionalized GSH@Fe3O4 / GSH@AAO composite membrane comprises the following steps:
[0096] (1) Preparation of GSH@Fe3O4 nanoparticles:
[0097] 1.0 g of Fe3O4 nanoparticles were fully dispersed in 10 mL of anhydrous ethanol by stirring at 300 rpm, and then 30 mL of water was added, and ultrasonic treatment was performed at 40 kW and 25 °C for 2 h; 0.4 g of reduced glutathione was added, and ultrasonic treatment was continued at 40 kW and 25 °C for 1 h; finally, the mixture was collected by a magnet, washed repeatedly with water, and vacuum dried at 60 °C for 8 h to obtain GSH@Fe3O4 nanoparticles;
[0098] (2) Preparation of GSH@AAO membrane:
[0099] The anodic aluminum oxide (AAO) film was immersed in a 0.25% (% is mass percentage) NaOH aqueous solution, treated at 40kW for 2 minutes, left to stand for 2 minutes, and taken out; then placed in a 5% (% is volume percentage) (3-aminopropyl) triethoxysilane (APTES) solution (the solvent is anhydrous ethanol) at 25°C (room temperature) for 2 hours, and after the treatment, washed with anhydrous ethanol to remove unreacted APTES to obtain a treated anodic aluminum oxide (AAO) film;
[0100] The treated anodic aluminum oxide (AAO) membrane was incubated in a MES buffer solution (pH 5.5) containing 0.1 M N-hydroxysuccinimide (NHS) at 25°C for 2 h, and then incubated in a 5 mM glutathione (GSH) solution at 25°C for 1 h to obtain a GSH@AAO membrane.
[0101] (3) Preparation of GSH@Fe3O4 / GSH@AAO composite membrane:
[0102] The GSH@Fe3O4 nanoparticles were dispersed in water to form a GSH@Fe3O4 nanoparticle suspension with a concentration of 1 mg / ml;
[0103] 10 μL of GSH@Fe3O4 nanoparticle suspension was dropped on the GSH@AAO membrane (diameter 5 mm) and dried at 50 °C for 30 min to obtain the functionalized GSH@Fe3O4 / GSH@AAO composite membrane.
[0104] Comparative Example 1
[0105] The ultrasonic treatment time of the anodized aluminum oxide (AAO) membrane in 0.25% (% is mass percentage) NaOH aqueous solution in step (2) of Example 1 was adjusted to 0, 1, and 2 min, without standing for 2 min. The rest was consistent with Example 1, and anodized aluminum oxide (AAO) membrane treated with sodium hydroxide was obtained.
[0106] The performance of the anodic aluminum oxide (AAO) film treated with sodium hydroxide was tested. Figure 2 ;
[0107] from Figure 2 It can be seen that the contact angle of the original state (AAO) membrane is 57.6°; without any ultrasonic treatment, the contact angle of the AAO membrane is 57.6°, showing a certain hydrophobicity; after ultrasonic treatment for 1 minute (Ultrasound for 1 minute / AAO), the contact angle is 51.0°; although the change is not large, it shows that short-term ultrasonic treatment has a certain effect on the hydrophilicity of the membrane; the contact angle of ultrasonic treatment for 2 minutes (Ultrasound for 2 minutes / AOO) is 49.9°, showing an increase in hydrophilicity. The increase in ultrasonic treatment time may lead to more nanopores exposed on the membrane surface, thereby increasing hydrophilicity. The contact angle of ultrasonic treatment for 2 minutes and rest for 2 minutes (Ultrasound for 2 minutes and rest for 2 minutes / AOO) is 16.7°. After 2 minutes of ultrasonic treatment and rest for 2 minutes, the contact angle is significantly reduced to 16.7°, indicating that the hydrophilicity of the membrane is increased after ultrasonic treatment under weak alkaline conditions, and the droplets can pass through the micro-nano channels more easily, and the contact angle is significantly reduced.
[0108] Example 2
[0109] A method for preparing a modified screen-printed electrode comprises the following steps:
[0110] The magnetic material (flexible magnet sheet) was first pasted on the surface of the screen-printed electrode using silver conductive glue, and then the functionalized GSH@Fe3O4 / GSH@AAO composite film of Example 1 was pasted on the surface of the magnetic material (flexible magnet sheet), and then sealed on all sides with silicone sealant and dried to obtain the modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE).
[0111] Comparative Example 2
[0112] A method for preparing a modified electrode comprises the following steps:
[0113] 100 μL of 1 mg / mL GSH@Fe3O4 nanoparticle suspension was added dropwise onto the surface of SPCE (5 mm in diameter) to ensure uniform coverage of the working area of the electrode, and then placed in an oven for drying at 50° for 30 min to evaporate the solvent in the suspension, leaving an electrode uniformly modified with GSH@Fe3O4 nanoparticles (GSH@Fe3O4 / SPCE).
[0114] Comparative Example 3
[0115] A method for preparing a modified screen-printed electrode comprises the following steps:
[0116] The magnetic material (flexible magnet sheet) was first pasted on the surface of the screen-printed electrode using silver conductive glue, and then the GSH@AAO film was pasted on the surface of the magnetic material (flexible magnet sheet). The surface was then sealed all around with silicone sealant and dried to obtain the modified screen-printed electrode (GSH@AAO / SPCE).
[0117] The obtained screen-printed electrode was subjected to performance testing, and the test results are as follows:
[0118] Figure 3 The microstructure evolution of the anodized aluminum oxide (AAO) surface modified by glutathione (GSH) and glutathione combined with ferrous oxide (GSH@Fe3O4); a is the surface of anodized aluminum oxide (AAO) at a magnification of 10,000 times; b is the AAO modified by glutathione (GSH) at a magnification of 10,000 times; cf are scanning electron microscope (SEM) images of GSH@Fe3O4 / GSH@AAO membranes at magnifications of 350, 1000, 3500, and 5000. Figure 3 As can be seen in a, the surface of anodized aluminum (AAO) has a highly ordered pore structure. This structure is usually made on the aluminum surface by anodizing, and the pore size and pore spacing are controlled by the preparation conditions; Figure 3 As can be seen in Figure b, the pore surface of AAO modified with glutathione (GSH) becomes slightly rougher than that of AAO without modification, which may be caused by the adsorption of GSH molecules on the surface of AAO. Figure 3 It can be seen from the figure that: the sample surface is relatively uniform at 350 times magnification, with no obvious particle aggregation; the particle distribution is good, and the overall surface shows a large-scale structure; the sample surface particle structure is clear at 1000 times magnification, with a particle size of about tens of microns; the particle distribution is uniform, with no obvious aggregation phenomenon; the contrast and brightness differences indicate that there may be a modified layer on the surface; the sample surface details are clearer at 3500 times magnification, showing the roughness and irregular morphology of the particle surface; the particle shape is irregular, and the surface shows some small protrusions and depressions, which may be a glutathione modification layer; the surface contrast and brightness differences are more obvious; the sample surface particle structure is very delicate at 5000 times magnification, showing the microscopic morphology of the particle surface; the particle surface shows more organic layer attachments; the contrast and brightness differences are obvious, and the surface texture and structure are clear. Therefore, the images at all magnifications show that the sample surface is relatively uniform, without obvious aggregation phenomenon, indicating that the sample has good dispersibility. The images at medium and high magnification (1000x, 3500x, 5000x) showed the rough and irregular morphology of the particle surface, suggesting the possible presence of a glutathione modification layer. The images at the highest magnification (5000x) clearly showed the microscopic morphology of the particle surface, further confirming the presence of a glutathione modification layer.
[0119] Figure 4 Comparison of infrared absorption spectra of unmodified and modified anodic aluminum oxide (AAO) films; curve a is anodic aluminum oxide (AAO); curve b is glutathione-modified anodic aluminum oxide (GSH@AAO); curve c is glutathione-bound ferric oxide-modified anodic aluminum oxide (GSH@Fe3O4 / AAO). Figure 4 It can be seen that: curve a has characteristic absorption peaks of 1650cm-1 and 1569cm-1, corresponding to the amide bonds (C=O and NH) in the glutathione molecule. These peaks clearly indicate that glutathione has been modified on the surface of anodized aluminum; curve b has characteristic absorption peaks of 1162cm-1 and 1038cm-1, corresponding to CO or CN bonds. The absorption peaks in the range of 1000cm-1 to 500cm-1 indicate the presence of Fe-O bonds, which indicates that ferroferric oxide has been successfully combined with the surface of the glutathione-modified anodized aluminum (AAO) film; curve c has no obvious characteristic absorption peaks, the spectrum is flat and mainly shows the absorption characteristics of the Al-O bond.
[0120] Figure 5 X-ray diffraction analysis for crystal structure comparison of anodized aluminum film and its modified forms. Figure 5 It can be seen that the characteristic peaks of anodic aluminum oxide (AAO) are observed at 2θ≈37° and 45°. These peaks correspond to the characteristic diffraction peaks of γ-Al2O3. The characteristic peaks of anodic aluminum oxide (GSH@AAO) bound to glutathione are still observed at 2θ≈37° and 45°, but the intensity is reduced. Compared with pure AAO, some new diffraction peaks appear. Glutathione modification may cause changes in the lattice structure of the alumina surface, thereby causing changes in the intensity of the diffraction peaks. The characteristic peaks of glutathione-bound ferroferric oxide modified porous anodic aluminum oxide film (GSH@Fe3O4 / AAO) are observed at 2θ≈30.2°, 35.6°, 43.3°, 57.3° and 62.9°. These peaks correspond to the characteristic diffraction peaks of ferroferric oxide (Fe3O4). At the same time, the characteristic diffraction peaks of alumina still exist, but the intensity is further reduced. The characteristic diffraction peak of ferroferric oxide indicates the presence of Fe3O4 crystal structure in the sample. The sample of porous anodic aluminum oxide film modified with glutathione combined with ferroferric oxide shows a mixed crystal structure of Fe3O4 and γ-Al2O3. The introduction of glutathione molecules may cause lattice deformation on the surface of part of the aluminum oxide, resulting in a decrease in the intensity of the characteristic peak of aluminum oxide.
[0121] Example 3
[0122] A method for preparing an electrochemical sensor based on micro-nano channels and screen printing comprises the following steps:
[0123] The modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) was used as the working electrode, and the working electrode, reference electrode (Ag / AgCl) and counter electrode (platinum wire) were respectively connected to a portable electrochemical workstation to form an electrochemical sensor based on micro-nano channels and screen printing.
[0124] 3mM / L potassium ferrocyanide solution is used for electrochemical characterization of electrochemical sensors, as follows:
[0125] 100 μL of 3 mM potassium ferrocyanide solution was dropped onto the prepared screen-printed electrode, and then the sensor was comprehensively electrochemically characterized using cyclic voltammetry (CV), differential pulse voltammetry (DPV), and electrochemical impedance spectroscopy (EIS) on an electrochemical workstation.
[0126] The results are as follows:
[0127] Figure 6 The cyclic voltammetric response of GSH@Fe3O4 / GSH@AAO / SPCE electrode at different rates (20mV / s to 140mV / s); the inset is the linear relationship between the peak current and the scan rate. Figure 6 It can be seen that as the scan rate increases, the currents of the oxidation peak and the reduction peak also increase accordingly. The oxidation peak shows a positive linear relationship (slope is 0.9836, intercept is 52.371, R 2 =0.9686), the reduction peak showed a negative linear relationship (slope was -1.1386, intercept was -113.17, R 2 =0.9831). This linear relationship indicates that the electrochemical reaction is mainly controlled by the diffusion process. As the scan rate increases, the peak potentials of the oxidation peak and the reduction peak also move to a certain extent, which may reflect the electrochemical kinetic properties of the sensor material. The sensitivity of the sensor is reflected by the linear increase of the peak current with the scan rate, and the higher R 2 The values indicate that its response is consistent and repeatable. Therefore, through the analysis of the CV curves, it can be concluded that the sensor has excellent sensitivity, stability and consistency at different scan rates, which makes it show high reliability in detecting target substances.
[0128] Figure 7 Cyclic voltammetry electrochemical characterization diagrams of bare electrode, GSH@AAO / SPCE, GSH@Fe3O4 / SPCE, GSH@Fe3O4 / GSH@AAO / SPCE during electrode modification; Figure 7It can be seen that: the peak current of SPCE (bare electrode) is relatively small, and the positions of oxidation and reduction peaks are relatively symmetrical; as a benchmark, it shows the basic electrochemical behavior of the unmodified electrode. The peak current of the GSH@AAO / SPCE electrode increased, indicating that the glutathione-modified AAO film enhanced the electrochemical reaction activity; the modified layer may provide more active sites and better electronic conductivity. The peak current of the GSH@Fe3O4 / SPCE electrode increased significantly, indicating that the glutathione-modified ferroferric oxide nanoparticles greatly improved the electrochemical reaction performance of the electrode; the conductivity and electrochemical active sites of Fe3O4 nanoparticles may be the reasons for the increase in current. The peak current of the GSH@Fe3O4 / GSH@AAO / SPCE electrode is the largest, and the redox peak is sharper, indicating that the dual modification (GSH@Fe3O4 and GSH@AAO) significantly improves the electrochemical reaction activity of the electrode; the dual modification may bring about a synergistic effect, increase the reaction sites and improve the electronic conduction path.
[0129] Figure 8 The AC impedance diagram (Nyquist diagram) of bare electrode, GSH@AAO / SPCE, GSH@Fe3O4 / SPCE, and GSH@Fe3O4 / GSH@AAO / SPCE during the electrode modification process; Figure 8 It can be seen that: SPCE (bare electrode) shows a larger semicircle in the Nyquist plot, indicating that the charge transfer resistance (Rct) of the electrode is higher; it shows the higher impedance of the bare electrode in the electrochemical reaction. The GSH@AAO / SPCE electrode shows a smaller semicircle in the Nyquist plot, indicating that the charge transfer resistance is significantly reduced; it shows that the glutathione-modified AAO film effectively enhances the charge transfer efficiency of the electrode and reduces the impedance. The GSH@Fe3O4 / SPCE electrode shows a smaller semicircle in the Nyquist plot, and the modification of Fe3O4 nanoparticles provides more electrochemical active sites. The semicircle shown by the GSH@AAO / SPCE electrode in the Nyquist plot is smaller than that of the GSH@Fe3O4 / SPCE electrode, because the addition of silver conductive glue in the GSH@AAO / SPCE electrode further improves the conductivity and charge transfer efficiency of the electrode. The GSH@Fe3O4 / GSH@AAO / SPCE electrode shows the smallest semicircle in the Nyquist plot and has the lowest charge transfer resistance; the dual modification (GSH@Fe3O4 and GSH@AAO) brings about a significant synergistic effect, greatly improving the charge transfer efficiency of the electrode and significantly reducing the impedance.
[0130] Fig. 9The following are the responses of bare electrode, GSH@AAO / SPCE, GSH@Fe3O4 / SPCE, and GSH@Fe3O4 / GSH@AAO / SPCE to cadmium ion signals in buffer solution during the electrode modification process; Fig. 9 It can be seen that the current response of SPCE (bare electrode) is small and the peak is not obvious; it shows that the unmodified electrode has a strong effect on Cd 2 + detection, the sensitivity is low. The current response of GSH@AAO / SPCE electrode increased significantly, and a more obvious peak appeared, indicating that the glutathione-modified AAO membrane enhanced the electrode's detection sensitivity to Cd2+; the micro-nano channel structure of the AAO membrane may provide more active sites, which helps to improve the electrochemical performance of the electrode. The current response of GSH@Fe3O4 / SPCE electrode increased, but not as significantly as GSH@AAO / SPCE, indicating that the single Fe3O4 nanoparticles have no significant effect on Cd 2 The detection effect of + was limited; Fe3O4 nanoparticles may provide a certain electrochemical activity, but their distribution and effective surface area may be limited. The GSH@Fe3O4 / GSH@AAO / SPCE electrode has the largest current response, and the peak value is significantly higher than that of other electrodes, indicating that the dual modification (GSH@Fe3O4 and GSH@AAO) significantly improves the electrode's detection of Cd 2 + detection sensitivity; the double modification brings about a synergistic effect, increasing the reaction sites and improving the electron conduction path.
[0131] Fig.10 The cyclic voltammetric response of 3 mM / L potassium ferrocyanide on the AAO membrane combined with screen-printed electrode at a scan rate of 100 mV / s. Fig.10 It can be seen that as the number of scans increases, the current gradually increases until it stabilizes. This phenomenon is used to verify the effect of liquid penetration through micro-nano channels.
[0132] Example 4
[0133] A method for detecting cadmium ions based on a micro-nano channel and a screen-printed electrochemical sensor comprises the following steps:
[0134] Prepare cadmium ion solutions with concentrations of 5 μg / L, 10 μg / L, 20 μg / L, 40 μg / L, 60 μg / L, 80 μg / L, 100 μg / L, and 120 μg / L (the solvent is acetic acid-sodium acetate buffer solution with a pH of 5);
[0135] 100 μL was taken and dropped on the working electrode of the modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE). After the electrode was connected to a portable electrochemical workstation, the Cd2+ in the group was detected by the DPV method.
[0136] The DPV parameters are as follows: calibration time 1 s, test voltage -0.5 V to 0 V, step potential 0.01 V, scan rate 0.002 V / s, and pH 5.
[0137] The results are as follows Fig.11 ,from Fig.11 It can be seen that different concentrations of Cd2+ correspond to different colored curves, from 5μg / L to 120μg / L, showing obvious concentration dependence; as the Cd2+ concentration increases, the peak current gradually increases. The inset shows the relationship between the peak current and the Cd2+ concentration, showing an obvious linear relationship; the linear regression equation is: I DPV(μA) =-0.31+0.98 Correlation coefficient (R 2 ) is 0.99908, where I DPV represents the DPV response peak current, Represents Cd 2 + concentration. According to the formula LOD = 3s / b (where s is the standard deviation of the blank sample and b is the slope of the standard curve), the detection limit is calculated to be 0.1 μg / L. The above results show that the constructed electrochemical sensor is suitable for detecting Cd 2 + Feasibility.
[0138] Example 5 Differential Pulse Voltammetry (DPV) pH Optimization
[0139] The modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) was used as the working electrode. In the acetic acid-sodium acetate buffer solution with a pH range of 3.5 to 6.5, 20 μg / L divalent cadmium ions (Cd 2 +)(Cadmium chloride solution) DPV response curve;
[0140] The parameters of the DPV method were set as follows: calibration time 1 s, test voltage from -0.5 V to 0 V, step potential 0.01 V, and scan rate 0.002 V / s.
[0141] Combination Fig.12 As shown, from Fig.12 It can be seen that the pH range is from 3.5 to 6.5, with a total of 7 different pH values; as the pH value changes, the peak current and peak position also change. The inset shows the relationship between the peak current and the pH value, showing the trend of the peak current changing with the pH value; at a pH value of 5, the peak current reaches the maximum value, indicating that the electrode has a low sensitivity to Cd under this pH condition. 2 + has the highest detection sensitivity. Under the condition of pH 5, the peak value of the current-potential curve is the highest, indicating that the detection sensitivity is best under this condition; under other pH conditions, the peak value is lower, indicating that under these conditions the electrode is sensitive to Cd 2+ has low detection sensitivity.
[0142] Example 6 Differential Pulse Voltammetry (DPV) Scan Rate Optimization
[0143] The modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) was used as the working electrode. In the acetic acid-sodium acetate buffer solution with pH = 5, 20 μg / L divalent cadmium ions (Cd 2 +) (cadmium chloride solution). The parameters of the DPV method are set as follows: calibration time 1s, test voltage -0.5V to 0V, step potential 0.01V. By analyzing these response curves, the scan rate can be optimized to obtain the best detection sensitivity.
[0144] Results milk Fig.13 ,from Fig.13 It can be seen that the scan rate ranges from 0.002V / s to 0.01V / s, with a total of 5 different rates; as the scan rate increases, the peak current gradually decreases. The inset shows the relationship between the peak current and the scan rate. It is obvious that the peak current decreases with the increase of the scan rate; when the scan rate is low (0.002V / s), the peak current is the largest, indicating that the electrode is sensitive to Cd at a low rate. 2 + has higher detection sensitivity. At a lower scan rate (such as 0.002V / s), the current-potential curve is sharper and the peak is higher, indicating that the detection at this rate is more sensitive; at a higher scan rate (such as 0.01V / s), the peak is lower, indicating that the electrochemical reaction at this rate is less complete and the sensitivity is reduced.
[0145] Example 7 Stability Test
[0146] Stability test of electrochemical sensor using modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) as working electrode:
[0147] The modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) was used as the working electrode to test the stability of the electrochemical sensor at the same time of 2 days, 4 days, 6 days, 8 days and 10 days. The results are shown in Figure 2. Fig.14 ;
[0148] from Fig.14 It can be seen that the current response (about 20 μA) of the electrode remained stable at the time points of 2 days, 4 days, 6 days, 8 days and 10 days. The error range was small and the current value hardly changed significantly, indicating that the electrode showed good stability in different time periods.
[0149] Example 8 Specificity Test
[0150] Specificity test of electrochemical sensor using modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) as working electrode:
[0151] The modified screen-printed electrode (GSH@Fe3O4 / GSH@AAO / SPCE) was used as the working electrode, and the test object was a mixed solution (Na + , K + Mg 2+ , Ca 2+ Cu 2+ 、Zn 2+ The concentration of Cd was 400 μg / L. 2+ The concentration was 20 μg / L) and the specificity test of the electrochemical sensor was performed. The results were as follows Fig.15 ;
[0152] from Fig.15 It can be seen that: + , K + Mg 2+ , Ca 2+ Cu 2+ 、Zn 2+ Ion excess 20 times, Cd 2 The dissolution signal of + did not change significantly, indicating that the electrode had good specificity for the target ions.
[0153] Comparative Example 4
[0154] The incubation in glutathione (GSH) solution in step (2) of Example 1 was omitted, and the rest was the same as Example 1.
[0155] The results showed that Fe3O4 nanoparticles could rarely be loaded on the AAO membrane, resulting in poor detection performance.
[0156] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. Preparation of functionalized GSH@Fe 3 O 4 / GSH@AAO composite membrane method, It is characterized in that The steps include: (1)GSH@Fe 3 O 4 Preparation of Nanoparticles: Fe 3 O 4 The nanoparticles were dispersed in anhydrous ethanol, and then water was added for ultrasonic treatment. Reduced glutathione was then added and ultrasonic treatment was continued. Finally, a magnet was used to collect, wash, and dry the nanoparticles to obtain GSH@Fe 3 O 4 Nanoparticles; (2) Preparation of GSH@AAO membrane: The anodic aluminum oxide (AAO) film is immersed in a NaOH solution for treatment, and then taken out; then placed in a (3-aminopropyl) triethoxysilane (APTES) solution for treatment, and after the treatment is completed, washed to obtain a treated anodic aluminum oxide (AAO) film; The treated anodic aluminum oxide (AAO) membrane was incubated in a MES buffer solution of N-hydroxysuccinimide (NHS), and then incubated in a glutathione (GSH) solution to obtain a GSH@AAO membrane. (3)GSH@Fe 3 O 4 Preparation of GSH@AAO composite membrane: GSH@Fe 3 O 4 Nanoparticles dispersed in water to form GSH@Fe 3 O 4 Nanoparticle suspensions; GSH@Fe 3 O 4 The nanoparticle suspension was dropped onto the GSH@AAO membrane and dried to obtain the functionalized GSH@Fe 3 O 4 / GSH@AAO composite film.
2. The functionalized GSH@Fe prepared by the method of claim 1 3 O 4 / GSH@AAO composite film.
3. Preparation of modified screen-printed electrodes (GSH@Fe 3 O 4 / GSH@AAO / SPCE) method, It is characterized in that The steps include: The magnetic material was first pasted on the surface of the screen-printed electrode using conductive glue, and then the functionalized GSH@Fe 3 O 4 The / GSH@AAO composite film was pasted on the surface of the magnetic material, and then sealed with sealant on all sides and dried to obtain the modified screen-printed electrode (GSH@Fe 3 O 4 / GSH@AAO / SPCE).
4. A modified screen-printed electrode (GSH@Fe 3 O 4 / GSH@AAO / SPCE), It is characterized in that The functionalized GSH@Fe 3 O 4 / GSH@AAO composite film.
5. A method for preparing an electrochemical sensor based on micro-nano channels and screen printing, It is characterized in that The steps include: The modified screen-printed electrode (GSH@Fe 3 O 4 / GSH@AAO / SPCE) was used as the working electrode, and the working electrode, reference electrode and counter electrode were respectively connected to a portable electrochemical workstation to form an electrochemical sensor based on micro-nano channels and screen printing.
6. An electrochemical sensor based on micro-nano channels and screen printing, It is characterized in that The functionalized GSH@Fe 3 O 4 / GSH@AAO composite film or the modified screen-printed electrode according to claim 4 (GSH@Fe 3 O 4 / GSH@AAO / SPCE).
7. A method for detecting cadmium ions based on micro-nano channels and screen-printed electrochemical sensors. It is characterized in that The steps include: The solution to be tested containing cadmium ions is dropped onto the working electrode of the electrochemical sensor based on micro-nano channels and screen printing according to claim 6, and the cadmium ions are detected by the DPV method.
8. The method according to claim 7, It is characterized in that The parameters of the DPV method were set as follows: calibration time 1 s, test voltage -0.5 V to 0 V, step potential 0.01 V, scan rate 0.002 V / s., and pH 5.
9. The method according to claim 7, It is characterized in that The concentration of cadmium ions in the test solution containing cadmium ions is 5 μg / L-120 μg / L.
10. The functionalized GSH@Fe according to claim 2 3 O 4 / GSH@AAO composite film, the modified screen-printed electrode according to claim 4 (GSH@Fe 3 O 4 / GSH@AAO / SPCE) or the electrochemical sensor based on micro-nano channels and screen printing as described in claim 6 in the field of electrochemical detection.