Preparation method of micro-nano optical structural color film based on all-dielectric silicon

By adjusting the dual-beam laser interference optical path and inductively coupled plasma etching technology, a high-resolution and high-brightness micro-nano optical structure color film is prepared, which solves the low efficiency and high cost of micro-nano optical structure color preparation in the existing technology The problem has realized the possibility of large-scale commercial production.

CN118962880AActive Publication Date: 2024-11-15CHANGCHUN UNIV OF SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411162614.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing micro-nano optical structure color preparation technology has low processing efficiency and high cost, making it difficult to be suitable for large-scale commercial production.

Method used

The micro-nano optical structure color film preparation method based on all dielectric silicon is adopted. By adjusting the parameters of the dual-beam laser interference optical path, the grating period and characteristic size can be adjusted, combined with the ultraviolet laser beam exposure time and sample stage movement, the processing area is controlled. The structural parameters were designed using the time domain finite difference method, and a high-resolution, high-brightness micro-nano optical structure chromatic film was prepared through inductively coupled plasma etching technology.

Benefits of technology

The color and area of ​​the micro-nano optical structure color film is adjustable, with high resolution and high brightness, and is suitable for large-scale commercial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118962880A_ABST
    Figure CN118962880A_ABST
Patent Text Reader

Abstract

The invention provides a micro-nano optical structural color film preparation method based on all-dielectric silicon, and the method comprises the steps: obtaining the structural parameters of an optical structural color film through a finite difference time domain method according to the chromaticity and reflectivity of the optical structural color film to be prepared; the method comprises the following steps of: performing ultrasonic cleaning on an SOI chip, plating a chromium adhesion layer with the thickness of 2nm to obtain an SOI substrate, and uniformly coating photoresist with the thickness of 150nm to obtain an SOI adhesive layer; adjusting parameters of a double-beam laser interference light path to perform interference exposure on the SOI adhesive layer to obtain a micro-nano optical structure pattern; after a metal chromium film with the thickness of 30 nm is evaporated on the micro-nano optical structure pattern, the photoresist is dissolved with a developing solution to peel off the metal chromium film, and a chromium mask with the micro-nano optical structure pattern is formed; and etching the SOI chip by using an inductively coupled plasma etching technology to obtain the Si micro-nano optical structural color film. The Si micro-nano optical structural color film obtained by the method has high resolution and high brightness, the color is adjustable, and the processing area is adjustable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of laser interference lithography technology, and in particular relates to a method for preparing a micro-nano optical structure color film based on all-dielectric silicon. Background Art

[0002] The characteristic of micro-nano optics is that it can precisely control the light field at a very small spatial scale, which makes it of great significance in new physics and applications. The micro-nano structures (such as nanowires, nanoholes, nanopillars, nanoparticles, etc.) of micro-nano optical structured color surfaces can regulate the light waves scattered by the surface by changing the periodic distribution and characteristic size, so it has broad prospects in cutting-edge applications such as ultra-high resolution backlight-free display, optical information storage, and image encryption.

[0003] At present, the scale of preparation of micro-nano optical structural colors is mostly at the micron level, and common manufacturing technologies used for structural color preparation include: focused ion beam lithography, electron beam lithography, reactive ion beam etching, nanoimprinting and self-assembly technology. Although these methods can achieve the preparation of micro-nano optical metal / dielectric structural colors with controllable period, size, morphology and arrangement, they are limited by low processing efficiency and high cost and are not suitable for large-scale commercial production. Summary of the invention

[0004] In view of this, the purpose of the present application is to provide a method for preparing a micro-nano optical structural color film based on all-dielectric silicon. By adjusting the parameters of the dual-beam laser interference optical path, the grating period and characteristic size of the micro-nano optical structure can be adjusted, and the color of the micro-nano optical structural color film can be adjusted. At the same time, by controlling the exposure time of the ultraviolet laser beam and the movement of the sample stage, the processing area of ​​the micro-nano optical structural color film can be adjusted. In addition, due to the advantage of the high refractive index of the all-dielectric silicon material, the micro-nano optical structural color film based on the all-dielectric silicon has the characteristics of high resolution and high brightness.

[0005] The present application provides a method for preparing a micro-nano optical structure color film based on all-dielectric silicon, the method comprising:

[0006] According to the chromaticity and reflectivity of the optical structural color film to be prepared, the structural parameters of the optical structural color film are obtained by using the time-domain finite difference method; the structural parameters include: grating period, characteristic size and height;

[0007] After ultrasonic cleaning of the SOI chip of the height, a 2nm thick chromium adhesion layer is plated to obtain an SOI substrate, and a 150nm thick photoresist is uniformly coated on the surface of the SOI substrate to obtain an SOI adhesive layer;

[0008] Based on the structural parameters, adjusting the parameters of the dual-beam laser interference optical path to perform interference exposure on the SOI glue layer to obtain a micro-nano optical structure pattern with the grating period and characteristic size;

[0009] After evaporating a metal chromium film with a thickness of 30 nm on the micro-nano optical structure pattern, dissolving the photoresist on the micro-nano optical structure pattern with a developer to peel off the metal chromium film to form a chromium mask having the micro-nano optical structure pattern;

[0010] The SOI chip is etched according to the pattern of the chromium mask by using inductively coupled plasma etching technology, and the chromium mask layer remaining on the surface is removed to obtain a Si micro-nano optical structure color film.

[0011] Furthermore, the dual-beam laser interference optical path includes: a laser, a beam splitter, a reflective element, a half-wave plate, a polarizer, and a micro-displacement sample stage;

[0012] The laser is used to emit a 360nm ultraviolet laser beam;

[0013] The beam splitting element is used to split the ultraviolet laser beam into two laser beams with the same power;

[0014] The reflective element is used to adjust the propagation path of the laser beam so that the two laser beams are incident on the micro-displacement sample stage at the same angle;

[0015] The half-wave plate and polarizer are used to adjust the polarization direction and laser power of the laser beam so that the amplitudes of the two laser beams are the same and interference occurs, and to change the grating period and characteristic size of the micro-nano optical structure pattern;

[0016] The micro-displacement sample stage is used to fix the SOI glue layer.

[0017] Furthermore, the dual-beam laser interference optical path further includes: an aperture, a convex lens and a pinhole;

[0018] The aperture is arranged between the polarizer and the sample stage, and is used to shape the spot shapes of the two laser beams into a square to adapt to the shape of the SOI chip;

[0019] The convex lens and the small hole are arranged between the reflective element and the aperture, and are used for filtering and amplifying the laser beam.

[0020] Furthermore, the dual-beam laser interference optical path further includes: an optical gate;

[0021] The optical shutter is arranged between the laser and the beam splitter element, and is used to control the exposure time of the ultraviolet laser beam;

[0022] After the SOI glue layer is fixed on the micro-displacement sample stage, a large-area interference exposure of the SOI glue layer is achieved by setting a moving speed and a moving path of the micro-displacement sample stage and an exposure time of the light gate;

[0023] Wherein, the micro-displacement sample stage can perform micro-movement in a two-dimensional plane.

[0024] Furthermore, the micro-nano optical structure includes: a Si nanowire grid structure.

[0025] Furthermore, the grating period of the micro-nano optical structure ranges from 200 to 300 nm;

[0026] The characteristic size of the micro-nano optical structure ranges from 50 to 200 nm.

[0027] Furthermore, the reflection wavelength range of the Si micro-nano optical structure color film is 400-700nm;

[0028] The thickness of the Si micro-nano optical structure color film ranges from 50 to 400 nm;

[0029] The area of ​​the Si micro-nano optical structure color film ranges from 1 to 100 cm 2 .

[0030] Furthermore, the etching parameters of the inductively coupled plasma etching technology are set as follows: CHF3 gas flow rate is 80 sccm, the front RF voltage is 300 V, the rear RF voltage is 20 V, and the etching time is 360 s.

[0031] Furthermore, after obtaining the Si micro-nano optical structure color film, the method further comprises:

[0032] A scanning electron microscope is used to obtain a scanning electron microscope image of the Si micro-nano optical structural color film to verify the structural characteristics of the Si micro-nano optical structural color film.

[0033] Furthermore, after obtaining the Si micro-nano optical structure color film, the method further comprises:

[0034] A high-power halogen light is used as the light source, and a 100x objective lens is used for focusing, so that the incident light is incident perpendicularly to the surface of the Si micro-nano optical structure color film. The full-angle illumination reflection mode of the microscopic angle-resolved spectrometer is used for measurement to obtain the reflection spectrum of the Si micro-nano optical structure color film.

[0035] Based on the reflection spectrum, the reflection wavelength and reflectivity of the Si micro-nano optical structure color film are obtained to test the performance of the Si micro-nano optical structure color film.

[0036] The method for preparing a micro-nano optical structural color film based on all-dielectric silicon of the present application adjusts the parameters of the dual-beam laser interference optical path so that the grating period and characteristic size of the micro-nano optical structure and the color of the micro-nano optical structural color film can be adjusted. At the same time, by controlling the exposure time of the ultraviolet laser beam and the movement of the sample stage, the processing area of ​​the micro-nano optical structural color film can be adjusted. In addition, since the all-dielectric silicon material has the advantage of a high refractive index, the micro-nano optical structural color film based on all-dielectric silicon has the characteristics of high resolution and high brightness. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 A flow chart of a method for preparing a micro-nano optical structure color film based on all-dielectric silicon provided in an embodiment of the present application is shown;

[0038] Figure 2 A schematic diagram of a dual-beam laser interference optical path provided in an embodiment of the present application is shown;

[0039] Figure 3 A sample image of a blue all-dielectric silicon micro-nano optical structure color film provided in an embodiment of the present application is shown;

[0040] Figure 4 A scanning electron microscopic image of a blue all-dielectric silicon micro-nano optical structure color film provided in an embodiment of the present application is shown;

[0041] Figure 5 The reflection spectrum of the blue all-dielectric silicon micro-nano optical structure color film provided in the embodiment of the present application is used;

[0042] Figure 6 A sample image of a green all-dielectric silicon micro-nano optical structure color film provided in an embodiment of the present application is shown;

[0043] Figure 7 A scanning electron microscopic image of a green all-dielectric silicon micro-nano optical structure color film provided in an embodiment of the present application is shown;

[0044] Figure 8 The reflection spectrum of the green all-dielectric silicon micro-nano optical structure color film provided in the embodiment of the present application is used;

[0045] Fig. 9 A sample image of a red all-dielectric silicon micro-nano optical structure color film provided in an embodiment of the present application is shown;

[0046] Fig.10 A scanning electron microscopic image of a red all-dielectric silicon micro-nano optical structure color film provided in an embodiment of the present application is shown;

[0047] Fig.11 The reflection spectrum of the red all-dielectric silicon micro-nano optical structure color film provided in the embodiment of the present application is used;

[0048] The reference numerals include: 1-laser, 2-optical gate, BS-spectrometric element, HR-reflective element, H-half-wave plate, P-polarizer, 3-convex lens, 4-pinhole, 5-aperture, 6-SOI adhesive layer, 7-micro-displacement sample stage, 8-computer. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solution and advantages of the technical solution more clear, the technical solution is further described in detail below in conjunction with specific implementation methods. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the technical solution.

[0050] Si materials are frequently used in the preparation of micro-nano optical structural color films due to their low cost, high refractive index, high reliability and compatibility with optoelectronic devices. Subwavelength-sized Si structures exhibit strong electromagnetic resonance after interacting with visible light. Nanofilters of different shapes prepared using Si materials can achieve high-purity and wide-color-gamut structural colors in the visible light band. At the same time, since all-dielectric silicon materials have a higher refractive index than metal materials, the brightness of the structural colors is higher and the colors are more vivid.

[0051] Laser interference lithography is a method for processing large-area periodic micro-nanostructure patterns. The periodically distributed light intensity in the interference area is directly exposed on the photoresist surface, which has the advantages of no mask, low cost, high efficiency and large-area preparation.

[0052] In view of this, the present application uses all-dielectric silicon material and laser interference lithography technology to prepare Si micro-nano optical structure color film with high resolution and high brightness. By adjusting the laser interference lithography parameters, the grating period and characteristic size of the micro-nano optical structure can be changed to achieve the adjustment of the surface color and brightness of the Si micro-nano optical structure color film.

[0053] Next, the method for preparing the micro-nano optical structure color film based on all-dielectric silicon provided in the present application and the structural characteristics of the obtained Si micro-nano optical structure color film will be explained in conjunction with specific embodiments.

[0054] Embodiment 1

[0055] See also Figure 1 , Figure 1 This is a flow chart of the method for preparing a micro-nano optical structure color film based on all-dielectric silicon provided in the embodiment of the present application. Figure 1 As shown, the method includes:

[0056] S101. According to the chromaticity and reflectivity of the optical structural color film to be prepared, the structural parameters of the optical structural color film are obtained by using the finite difference time domain method; the structural parameters include: grating period, characteristic size and height.

[0057] In this step, the surface color of the optical structural color film is related to the surface structure of the optical structural color film. Specifically, the surface color can be changed by changing the grating period and characteristic size of the surface structure to adjust its reflection wavelength. In addition, the reflectivity of the optical structural color film is related to the grating depth, that is, a larger grating depth will lead to a higher reflectivity, and a smaller grating depth will enhance the transmission effect. Therefore, according to the needs, based on the chromaticity and reflectivity of the optical structural color film, the surface structure of the optical structural color film can be designed using the time-domain finite difference method to obtain the structural parameters of the optical structural color film including the grating period, characteristic size and height.

[0058] S102, ultrasonically clean the SOI chip of the height, plate a 2nm thick chromium adhesion layer to obtain an SOI substrate, and uniformly coat a 150nm thick photoresist on the surface of the SOI substrate to obtain an SOI adhesive layer.

[0059] In this step, first, a SOI (Silicon On Insulator) chip with the same height as that in the structural parameters is selected as a sample, and the SOI chip is ultrasonically cleaned in acetone solution, anhydrous ethanol, and deionized water solution for 5 minutes in turn to wash away surface pollutants; secondly, since the SOI chip is hydrophobic, a 2nm thick chromium adhesion layer is plated on the cleaned SOI chip to obtain an SOI substrate to improve its coating quality; thirdly, Allresist AR-P-3170 photoresist is used, and a spin coating method is adopted, and the rotation speed is set to 1200r / min, and a photoresist with a thickness of 150nm is evenly coated on the surface of the SOI substrate to obtain an SOI adhesive layer.

[0060] S103, based on the structural parameters, adjusting the parameters of the dual-beam laser interference optical path to perform interference exposure on the SOI glue layer to obtain a micro-nano optical structure pattern with the grating period and characteristic size.

[0061] Wherein, the micro-nano optical structure comprises: a Si nanowire grid structure; the grating period of the micro-nano optical structure ranges from 200 to 300 nm; and the characteristic size of the micro-nano optical structure ranges from 50 to 200 nm.

[0062] Here, please see Figure 2 , Figure 2 Schematic diagram of the dual-beam laser interference optical path provided in the embodiment of the present application. Figure 2 As shown, the dual-beam laser interference optical path includes: a laser, a beam splitter, a reflective element, a half-wave plate, a polarizer and a micro-displacement sample stage.

[0063] Among them, the laser is used to emit a 360nm ultraviolet laser beam; the spectroscopic element is used to split the ultraviolet laser beam into two laser beams with the same power; the reflective element is used to adjust the propagation path of the laser beam so that the two laser beams are incident on the micro-displacement sample stage at the same angle; the half-wave plate and the polarizer are used to adjust the polarization direction and laser power of the laser beam so that the amplitudes of the two laser beams are the same and interference is generated, and the grating period and characteristic size of the micro-nano optical structure pattern are changed; the micro-displacement sample stage is used to fix the SOI glue layer.

[0064] Specifically, the beam splitter element is a 1:1 ultraviolet beam splitter, and the reflective element is an ultraviolet high reflector.

[0065] In addition, the dual-beam laser interference optical path also includes: an aperture, a convex lens and a pinhole;

[0066] The aperture is arranged between the polarizer and the sample stage, and is used to shape the spot shapes of the two laser beams into a square to adapt to the shape of the SOI chip; the convex lens and the small hole are arranged between the reflective element and the aperture, and are used to filter and amplify the laser beams.

[0067] The dual-beam laser interference optical path further includes: an optical gate;

[0068] The optical shutter is arranged between the laser and the beam splitter element, and is used to control the exposure time of the ultraviolet laser beam;

[0069] After the SOI glue layer is fixed on the micro-displacement sample stage, a large-area interference exposure of the SOI glue layer is achieved by setting a moving speed and a moving path of the micro-displacement sample stage and an exposure time of the light gate;

[0070] Wherein, the micro-displacement sample stage can perform micro-movement in a two-dimensional plane.

[0071] Here, both the optical shutter and the micro-displacement sample stage are controlled by a computer.

[0072] S104, after evaporating a metal chromium film with a thickness of 30 nm on the micro-nano optical structure pattern, using a developer to dissolve the photoresist on the micro-nano optical structure pattern to peel off the metal chromium film to form a chromium mask having the micro-nano optical structure pattern.

[0073] S105, using inductively coupled plasma etching technology, after etching the SOI chip according to the pattern of the chromium mask, remove the chromium mask layer remaining on the surface to obtain a Si micro-nano optical structure color film.

[0074] The etching parameters of the inductively coupled plasma etching technology are set as follows: CHF3 gas flow rate is 80 sccm, the front RF voltage is 300 V, the rear RF voltage is 20 V, and the etching time is 360 s.

[0075] In this step, the etching time is determined by the thickness of the SOI chip so as to etch through the surface Si film to the SiO2 layer, and finally form a Si micro-nano optical structure on the SiO2 surface to obtain a Si micro-nano optical structure color film.

[0076] The reflection wavelength range of the Si micro-nano optical structure color film is 400-700nm; the thickness range of the Si micro-nano optical structure color film is 50-400nm; the area range of the Si micro-nano optical structure color film is 1-100cm 2 .

[0077] After obtaining the Si micro-nano optical structure color film, the method further comprises:

[0078] Step 106: Using a scanning electron microscope, obtain a scanning electron microscope image of the Si micro-nano optical structure color film to verify the structural characteristics of the Si micro-nano optical structure color film.

[0079] In this step, the structural characteristics of the Si micro-nano optical structural color film, such as etching depth, grating period, and average feature size, can be obtained by analyzing the scanning electron microscopy image. By comparing the structural parameters of the optical structural color film obtained using the finite difference time domain method, it is verified whether the structural characteristics of the Si micro-nano optical structural color film meet the requirements.

[0080] Step 107: Use high-power halogen light as a light source and focus it with a 100x objective lens so that the incident light is perpendicular to the surface of the Si micro-nano optical structure color film. Use a microscopic angle-resolved spectrometer in full-angle illumination reflection mode for measurement to obtain a reflection spectrum of the Si micro-nano optical structure color film.

[0081] In this step, the diffuse light of the high-power halogen light source is focused onto the back focal plane of a 100x objective lens, wherein the numerical aperture NA of the objective lens is 0.7.

[0082] Step 108: Based on the reflection spectrum, obtain the reflection wavelength and reflectivity of the Si micro-nano optical structure color film to test the performance of the Si micro-nano optical structure color film.

[0083] Embodiment 2

[0084] The preparation method of the blue all-dielectric silicon micro-nano optical structural color film includes:

[0085] Step 201: According to the chromaticity and reflectivity of the blue light micro-nano optical structure color film, the structural parameters of the blue light micro-nano optical structure color film are obtained by using the time-domain finite difference method: grating period 300nm, characteristic size 60nm and height 200nm.

[0086] Step 202 , after ultrasonic cleaning of a 200 nm thick SOI chip, a 2 nm thick chromium adhesion layer is plated to obtain an SOI substrate, and a 150 nm thick photoresist is evenly coated on the surface of the SOI substrate to obtain an SOI adhesive layer.

[0087] Step 203: Based on the above structural parameters, a 360nm ultraviolet laser (CNI MSL-FN-360-S) is selected, and the parameters of the dual-beam laser interference optical path are adjusted: the incident angle of the two laser beams is 36.9°, and the laser power is set to 4mW / cm 2 The exposure time is set to 8s, and the SOI glue layer is subjected to interference exposure to obtain the micro-nano optical structure. At the same time, the moving speed and moving path of the micro-displacement sample stage, as well as the switching time of the optical gate, are coordinated to complete an area of ​​about 30cm 2 Processing of micro-nano optical structure patterns.

[0088] Step 204 : after evaporating a metal chromium film with a thickness of 30 nm on the micro-nano optical structure pattern, a developer is used to dissolve the photoresist on the micro-nano optical structure pattern to peel off the metal chromium film, thereby forming a chromium mask having the micro-nano optical structure pattern.

[0089] Step 205, using ICP-RIE (Sentech SI 500), set the etching parameters: CHF3 gas flow rate is 80sccm, the front RF voltage is 300V, the rear RF voltage is 20V, and the etching time is 360s. After etching the SOI chip according to the pattern of the chromium mask, remove the residual chromium mask layer on the surface to obtain Figure 3 The blue all-dielectric silicon micro-nano optical structural color film shown.

[0090] Step 206: Using a scanning electron microscope (FEI Helios NanoLab G4), obtain Figure 4 The scanning electron microscopy image of the blue all-dielectric silicon micro-nano optical structural color film is shown. By analyzing the scanning electron microscopy image, it can be seen that the blue all-dielectric silicon micro-nano optical structural color film has a Si nanowire grid structure, and its structural characteristics are: etching depth of 200nm, grating period of 300nm, and average characteristic size of 54nm.

[0091] Step 207: Use high-power halogen light as the light source, focus it with a 100x objective lens, make the incident light vertically incident on the surface of the blue all-dielectric silicon micro-nano optical structure color film, and use the full-angle illumination reflection mode of the micro-angle resolution spectrometer (ideaoptics ARMS) for measurement, and obtain the following: Figure 5 The reflection spectrum of the blue all-dielectric silicon micro-nano optical structural color film is shown.

[0092] Step 208: From the reflection spectrum, it can be seen that the reflection wavelength of the blue all-dielectric silicon micro-nano optical structure color film is 460nm, and the maximum reflectivity can be 62%, which shows that the performance of the blue all-dielectric silicon micro-nano optical structure color film is good.

[0093] Embodiment 3

[0094] The preparation method of the green all-dielectric silicon micro-nano optical structural color film includes:

[0095] Step 301: According to the chromaticity and reflectivity of the green light micro-nano optical structure color film, the structural parameters of the green light micro-nano optical structure color film are obtained by using the time-domain finite difference method: grating period 300nm, characteristic size 80nm and height 200nm.

[0096] Step 302 , after ultrasonic cleaning of a 200 nm thick SOI chip, a 2 nm thick chromium adhesion layer is plated to obtain an SOI substrate, and a 150 nm thick photoresist is evenly coated on the surface of the SOI substrate to obtain an SOI adhesive layer.

[0097] Step 303: Based on the above structural parameters, a 360nm ultraviolet laser (CNI MSL-FN-360-S) is selected, and the parameters of the dual-beam laser interference optical path are adjusted: the incident angle of the two laser beams is 36.9°, and the laser power is set to 3mW / cm 2 The exposure time is set to 8s, and the SOI glue layer is subjected to interference exposure to obtain the micro-nano optical structure. At the same time, the moving speed and moving path of the micro-displacement sample stage, as well as the switching time of the optical gate, are coordinated to complete an area of ​​about 30cm 2 Processing of micro-nano optical structure patterns.

[0098] Step 304 : after evaporating a metal chromium film with a thickness of 30 nm on the micro-nano optical structure pattern, a developer is used to dissolve the photoresist on the micro-nano optical structure pattern to peel off the metal chromium film, thereby forming a chromium mask having the micro-nano optical structure pattern.

[0099] Step 305, using ICP-RIE (Sentech SI 500), set the etching parameters: CHF3 gas flow rate is 80sccm, the front RF voltage is 300V, the rear RF voltage is 20V, and the etching time is 360s. After etching the SOI chip according to the pattern of the chromium mask, remove the residual chromium mask layer on the surface to obtain Figure 6 The green all-dielectric silicon micro-nano optical structural color film shown.

[0100] Step 306: Using a scanning electron microscope (FEI Helios NanoLab G4), obtain Figure 7 The scanning electron microscopy image of the green all-dielectric silicon micro-nano optical structural color film is shown. By analyzing the scanning electron microscopy image, it can be seen that the green all-dielectric silicon micro-nano optical structural color film has a Si nanowire grid structure, and its structural characteristics are: etching depth of 200nm, grating period of 300nm, and average characteristic size of 74nm.

[0101] Step 307: Use high-power halogen light as the light source, focus it with a 100x objective lens, make the incident light vertically incident on the surface of the green all-dielectric silicon micro-nano optical structure color film, and use the full-angle illumination reflection mode of the micro-angle resolution spectrometer (ideaoptics ARMS) for measurement, and obtain the following: Figure 8 The reflection spectrum of the green all-dielectric silicon micro-nano optical structural color film is shown.

[0102] Step 308: From the reflection spectrum, it can be seen that the reflection wavelength of the green all-dielectric silicon micro-nano optical structure color film is 560nm, and the maximum reflectivity can reach 73%, which indicates that the performance of the green all-dielectric silicon micro-nano optical structure color film is good.

[0103] Embodiment 4:

[0104] The preparation method of the red all-dielectric silicon micro-nano optical structural color film includes:

[0105] Step 401: According to the chromaticity and reflectivity of the red light micro-nano optical structure color film, the structural parameters of the red light micro-nano optical structure color film are obtained by using the time-domain finite difference method: grating period 300nm, characteristic size 120nm and height 200nm.

[0106] Step 402 , after ultrasonic cleaning of a 200 nm thick SOI chip, a 2 nm thick chromium adhesion layer is plated to obtain an SOI substrate, and a 150 nm thick photoresist is evenly coated on the surface of the SOI substrate to obtain an SOI adhesive layer.

[0107] Step 403: Based on the above structural parameters, a 360nm ultraviolet laser (CNI MSL-FN-360-S) is selected, and the parameters of the dual-beam laser interference optical path are adjusted: the incident angle of the two laser beams is 36.9°, and the laser power is set to 2mW / cm 2 The exposure time is set to 8s, and the SOI glue layer is subjected to interference exposure to obtain the micro-nano optical structure. At the same time, the moving speed and moving path of the micro-displacement sample stage, as well as the switching time of the optical gate, are coordinated to complete an area of ​​about 30cm 2 Processing of micro-nano optical structure patterns.

[0108] Step 404 : after evaporating a metal chromium film with a thickness of 30 nm on the micro-nano optical structure pattern, a developer is used to dissolve the photoresist on the micro-nano optical structure pattern to peel off the metal chromium film, thereby forming a chromium mask with the micro-nano optical structure pattern.

[0109] Step 405, using ICP-RIE (Sentech SI 500), set the etching parameters: CHF3 gas flow rate is 80sccm, the front RF voltage is 300V, the rear RF voltage is 20V, and the etching time is 360s. After etching the SOI chip according to the pattern of the chromium mask, remove the residual chromium mask layer on the surface to obtain Fig. 9 The red all-dielectric silicon micro-nano optical structural color film shown.

[0110] Step 406: Using a scanning electron microscope (FEI Helios NanoLab G4), obtain Fig.10 The scanning electron microscopy image of the red all-dielectric silicon micro-nano optical structural color film is shown. By analyzing the scanning electron microscopy image, it can be seen that the red all-dielectric silicon micro-nano optical structural color film has a Si nanowire grid structure, and its structural characteristics are: etching depth of 200nm, grating period of 300nm, and average characteristic size of 106nm.

[0111] Step 407: Use high-power halogen light as the light source, focus it with a 100x objective lens, make the incident light vertically incident on the surface of the red all-dielectric silicon micro-nano optical structure color film, and use the full-angle illumination reflection mode of the micro-angle resolution spectrometer (ideaoptics ARMS) for measurement, and obtain the following: Fig.11 The reflection spectrum of the red all-dielectric silicon micro-nano optical structural color film is shown.

[0112] Step 408: From the reflection spectrum, it can be seen that the reflection wavelength of the red all-dielectric silicon micro-nano optical structure color film is 670nm, and the maximum reflectivity can reach 91%, which indicates that the performance of the red all-dielectric silicon micro-nano optical structure color film is good.

[0113] The above contents are only preferred embodiments of the present invention. For ordinary technicians in this field, many changes can be made in the specific implementation methods and application scopes based on the ideas of the present technical content. As long as these changes do not deviate from the concept of the present invention, they all fall within the scope of protection of this patent.

Claims

1. A method for preparing a micro-nano optical structural color film based on all-dielectric silicon, characterized in that: The method comprises: According to the chromaticity and reflectivity of the optical structural color film to be prepared, the structural parameters of the optical structural color film are obtained by using the time-domain finite difference method; the structural parameters include: grating period, characteristic size and height; After ultrasonic cleaning of the SOI chip of the height, a 2nm thick chromium adhesion layer is plated to obtain an SOI substrate, and a 150nm thick photoresist is uniformly coated on the surface of the SOI substrate to obtain an SOI adhesive layer; Based on the structural parameters, adjusting the parameters of the dual-beam laser interference optical path to perform interference exposure on the SOI glue layer to obtain a micro-nano optical structure pattern with the grating period and characteristic size; After evaporating a metal chromium film with a thickness of 30 nm on the micro-nano optical structure pattern, dissolving the photoresist on the micro-nano optical structure pattern with a developer to peel off the metal chromium film to form a chromium mask having the micro-nano optical structure pattern; The SOI chip is etched according to the pattern of the chromium mask by using inductively coupled plasma etching technology, and the chromium mask layer remaining on the surface is removed to obtain a Si micro-nano optical structure color film.

2. The method according to claim 1, characterized in that The double-beam laser interference optical path includes: a laser, a beam splitter, a reflective element, a half-wave plate, a polarizer and a micro-displacement sample stage; The laser is used to emit a 360nm ultraviolet laser beam; The beam splitting element is used to split the ultraviolet laser beam into two laser beams with the same power; The reflective element is used to adjust the propagation path of the laser beam so that the two laser beams are incident on the micro-displacement sample stage at the same angle; The half-wave plate and polarizer are used to adjust the polarization direction and laser power of the laser beam so that the amplitudes of the two laser beams are the same and interference occurs, and to change the grating period and characteristic size of the micro-nano optical structure pattern; The micro-displacement sample stage is used to fix the SOI glue layer.

3. The method according to claim 2, characterized in that The double-beam laser interference optical path also includes: an aperture, a convex lens and a pinhole; The aperture is arranged between the polarizer and the sample stage, and is used to shape the spot shapes of the two laser beams into a square to adapt to the shape of the SOI chip; The convex lens and the small hole are arranged between the reflective element and the aperture, and are used for filtering and amplifying the laser beam.

4. The method according to claim 2, characterized in that The dual-beam laser interference optical path further includes: an optical gate; The optical shutter is arranged between the laser and the beam splitter element, and is used to control the exposure time of the ultraviolet laser beam; After the SOI glue layer is fixed on the micro-displacement sample stage, a large-area interference exposure of the SOI glue layer is achieved by setting a moving speed and a moving path of the micro-displacement sample stage and an exposure time of the light gate; Wherein, the micro-displacement sample stage can perform micro-movement in a two-dimensional plane.

5. The method according to claim 1, characterized in that The micro-nano optical structure includes: a Si nanowire grid structure.

6. The method according to claim 1, characterized in that The grating period of the micro-nano optical structure ranges from 200 to 300 nm; The characteristic size of the micro-nano optical structure ranges from 50 to 200 nm.

7. The method according to claim 1, characterized in that The reflection wavelength range of the Si micro-nano optical structure color film is 400-700nm; The thickness of the Si micro-nano optical structure color film ranges from 50 to 400 nm; The area of ​​the Si micro-nano optical structure color film ranges from 1 to 100 cm 2 .

8. The method according to claim 1, characterized in that The etching parameters of the inductively coupled plasma etching technology are set as follows: CHF3 gas flow rate is 80 sccm, the front RF voltage is 300 V, the rear RF voltage is 20 V, and the etching time is 360 s.

9. The method according to claim 1, characterized in that After obtaining the Si micro-nano optical structure color film, the method further comprises: A scanning electron microscope is used to obtain a scanning electron microscope image of the Si micro-nano optical structural color film to verify the structural characteristics of the Si micro-nano optical structural color film.

10. The method according to claim 1, characterized in that After obtaining the Si micro-nano optical structure color film, the method further comprises: A high-power halogen light is used as the light source, and a 100x objective lens is used for focusing, so that the incident light is incident perpendicularly to the surface of the Si micro-nano optical structure color film. The full-angle illumination reflection mode of the microscopic angle-resolved spectrometer is used for measurement to obtain the reflection spectrum of the Si micro-nano optical structure color film. Based on the reflection spectrum, the reflection wavelength and reflectivity of the Si micro-nano optical structure color film are obtained to test the performance of the Si micro-nano optical structure color film.

Citation Information

Patent Citations

  • Preparation method and system of butterfly wing bionic structure color

    CN112518102A

  • Preparation method of silicon nanostructure and laser

    CN113363150A

  • Preparation method and preparation system of orthogonal grating type micro-nano structure

    CN114509836A

  • Patterned structural color processing device and processing method

    CN117471868A

  • Preparation method of microlens array based on moth eye structure

    CN118409375A