Optical cable inner sheath and preparation method thereof

By embedding evenly distributed aramid reinforcement in the sheath in the optical cable, the problem of simple structure and insufficient strength of the sheath in the existing optical cable is solved, and a more uniform force distribution and compressive resistance are achieved, reducing fiber loss.

CN118962924APending Publication Date: 2024-11-15FAR EAST COMMUNICATIONS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411035368.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The inner sheathing of the existing optical cable is simple in structure and insufficient in strength, making it difficult to ensure protection effect under the condition of reducing the specifications of external armor, resulting in large deformation and fiber loss of optical cables when impacted by external forces.

Method used

Using tubular structure, the inner sheath of optical cables is embedded with evenly distributed aramid reinforcements, including high-modulus aramid yarn and carbon fiber rods, reduce misalignment through spiral twisting and adhesive filling, and apply glue to the outer layer to form a whole The structure is uniformly subjected to stress and improves compressive resistance.

Benefits of technology

It effectively reduces the deformation of the sheath in the optical cable, improves its overall strength and rigidity, reduces the bending amount and loss of the optical fiber, and ensures that the loss of the optical cable under temperature changes is less than 0.02dB/km.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118962924A_ABST
    Figure CN118962924A_ABST
Patent Text Reader

Abstract

The invention discloses an optical cable inner sheath and a preparation method thereof, the structure of the inner sheath is tubular, the inner sheath comprises a sheath tube body and aramid fiber reinforcements uniformly distributed in the sheath, the aramid fiber reinforcements comprise high-modulus aramid fiber yarns and carbon fiber rods, bonding glue is filled between the aramid fiber yarns and the carbon fiber rods, and the aramid fiber yarns and the carbon fiber rods are spirally twisted. And outer layer glue is coated between the aramid fiber reinforcer and the sheath tube body. According to the invention, the aramid fiber reinforcer is embedded in the middle of the sheath tube body, the inside and the outside of the sheath tube body are infiltrated with glue, the aramid fiber yarns and the carbon fiber rods in the assembly of the aramid fiber reinforcer are spirally twisted, the dislocation between the aramid fiber yarns and the carbon fiber rods is reduced, and the gap is filled with the adhesive glue in the twisting process to reduce the dislocation. When the inner sheath is in an extruded state, the aramid fiber reinforcer embedded in the inner sheath effectively controls deformation, the surface of the inner sheath is uniformly stressed after the inner sheath is stressed, and finally the inner sheath is in a circular arc shape, so that the inner sheath becomes a whole, and large deformation caused by local strong extrusion of the inner sheath of the optical cable is completely eradicated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an optical cable inner sheath and a preparation method thereof, belonging to the technical field of optical cables. Background Art

[0002] With the development of network communication technology, the demand for information and communication has exploded, and the amount of cable laying has increased day by day. The typical optical cable structure includes an inner sheath, an outer sheath, an armor layer, etc., and each layer plays a different role. Among them, the inner sheath of the optical cable is in direct contact with the optical fiber, and plays the ultimate role in protecting the optical cable when the optical cable is impacted by external forces. The inner sheath of the optical cable on the market currently generally adopts a rubber structure, and its outer layer is laid with a variety of armor structures, which only plays a simple protective role. When the outer diameter of the optical cable is required to be extremely small, resulting in limited armor thickness, in actual projects, it is often necessary to balance the optical cable diameter and protection strength due to the overly simple structure and insufficient strength. How to ensure the protective effect of the optical cable under the condition of reducing the specifications of the external armor has become an important issue that needs to be solved in the industry. Summary of the invention

[0003] The object of the present invention is to provide an optical cable inner sheath and a preparation method thereof to solve the above-mentioned problems in the background technology.

[0004] The technical solution for achieving the purpose of the present invention is:

[0005] The invention discloses an inner sheath of an optical cable, which has a tubular structure and comprises a sheath body and aramid reinforcement members uniformly distributed in the sheath. The aramid reinforcement members comprise high modulus aramid yarn and carbon fiber rods. Adhesive glue is filled between the aramid yarn and the carbon fiber rods and they are spirally twisted. An outer layer of glue is applied between the aramid reinforcement members and the sheath body.

[0006] The optical cable inner sheath of the present invention has an aramid reinforcement member embedded in the middle of the sheath tube body, and is soaked with glue inside and outside the sheath. In the assembly of the aramid reinforcement member, the aramid yarn and the carbon fiber rod are spirally twisted to reduce the misalignment between the aramid yarn and the carbon fiber rod during the torsion process. During the twisting process, the gap between them is filled with adhesive glue to reduce the misalignment, and the outer layer is coated with external glue. When the inner sheath is squeezed, the aramid reinforcement member embedded inside it will effectively control the deformation. After being stressed, the surface of the inner sheath is evenly stressed and will eventually be in an arc shape, so that the inner sheath itself becomes a whole, and the large deformation caused by the local strong squeezing of the optical cable inner sheath is prevented, which can effectively improve.

[0007] The absolute value of the linear expansion coefficient of the aramid yarn at 80°C is less than 5.3×10-6°C-1, and the elastic modulus is ≥320GPa; the elastic modulus of the carbon fiber rod is ≥580GPa, and the comprehensive modulus is ≥450GPa.

[0008] The significance of the above parameter control is to ensure the control of the comprehensive strength of the inner sheath and the injection shrinkage. After testing, under the above parameter conditions, the shrinkage of the inner sheath can be reduced by 20% during the extrusion process, of which the sheath material shrinks by 2.5% at 870°C, and the comprehensive shrinkage is controlled at 1.8-2%. In terms of laying effect, increasing the rigidity of the inner sheath can reduce the bending amount of the optical fiber, thereby reducing the optical fiber loss. The use of this solution can make the additional loss of the optical cable under a temperature cycle of -40°C to 70°C less than 0.02dB / km.

[0009] The aramid reinforcement is evenly distributed in a 360° circle around the center of the cross section of the inner sheath tube body, and is placed at the center of the thickness of the inner sheath tube body and integrated with it in the form of extrusion.

[0010] Increasing the uniformity of the distribution of the aramid reinforcements can make the force distribution of the inner sheath more uniform, making the stress more balanced under impact.

[0011] The present invention also provides a method for preparing the above-mentioned optical cable inner sheath, which specifically comprises the following steps:

[0012] S1: The central strength member of the optical fiber is twisted with the loose tube and fixed by aramid yarn to form a cable core;

[0013] S2: The cable core is molded from the center hole of the mold core, and the aramid reinforcement is molded around the cable core at the same time and then extruded to obtain an inner sheath;

[0014] In the step of putting on the mold, the mold core is a tubular structure, the cable core and the aramid reinforcement are not in contact during the extrusion process, and the aramid reinforcement is located in the middle of the sheath layer of the inner sheath;

[0015] In the step S2, the cable core is molded from the center hole of the mold core during the extrusion process, and the mold is synchronously molded with the cable core during the operation. The aramid reinforcement enters from the holes evenly distributed on the mold core. The extrusion temperature is controlled at 155-185°C during the extrusion process. The low-temperature extrusion scheme is adopted here, which can effectively reduce the influence of the heat margin of extrusion on the internal structure of the optical fiber, thereby ensuring the performance stability of the internal optical fiber.

[0016] Further or optionally, the processing steps of the aramid reinforcement are:

[0017] Paying off the carbon fiber rods and aramid yarns;

[0018] Apply glue to the outer layer of the carbon fiber rod and the aramid yarn, and preheat them to maintain the glue in a semi-solid state;

[0019] Twisting of carbon fiber rods and aramid yarns;

[0020] The outer glue of the carbon fiber rod and aramid yarn is cured to complete the shaping;

[0021] Baking the formed aramid reinforcement;

[0022] Conduct a qualitative closing.

[0023] During the above preparation process, the carbon fiber rod and aramid yarn are released by active pay-off. During the defense process, the pay-off tension is controlled to be 350-550g. The carbon fiber rod, aramid yarn and carbon fiber rod at the inner end are released in a straightened state, and a dividing plate is performed. The dividing plate is divided into two layers, and the inner layer is provided with a glue filling device and a preheating device. The carbon fiber rod at the inner end enters the dividing plate for positioning in turn, and is coated with the glue filling device and heated by the preheating device so that the glue adhered to the carbon fiber rod is in a semi-solid state. Subsequently, the twisting device is used to shape the pitch, and the carbon fiber rod and aramid yarn at the inner end are twisted into one, and the twisting pitch is 10mm. After twisting, they are cured and shaped again. The solidified mixture is twisted with the carbon fiber rod at the outer end by glue and extruded through a molding mold, and shaped by baking.

[0024] Further or optionally, in the preheating treatment step, the temperature is controlled to be 40±5°C and the glue is kept in a semi-solid state. In the glue curing process, the curing temperature is 65±5°C. In the baking step, the baking temperature is 75±5°C, and the solidification state of the glue is controlled to ensure that it is always in a semi-solid state. After the twisting is completed, the inner and outer layers of glue of the aramid reinforcement are brought together after operation, so that the carbon fiber rod and the aramid yarn and the outer inner sheath body become a whole, and their various parts become a whole with the inner sheath, which can effectively improve the integrity and compressive resistance of the inner sheath.

[0025] By adopting the above technical solution, the present invention has the following beneficial effects:

[0026] (1) The inner sheath of the optical cable of the present invention has an aramid reinforcement member embedded in the middle of the sheath tube body, and is soaked with glue inside and outside. In the assembly of the aramid reinforcement member, the aramid yarn and the carbon fiber rod are spirally twisted to reduce the misalignment between the aramid yarn and the carbon fiber rod during the torsion process. During the twisting process, the gap between them is filled with adhesive glue to reduce the misalignment, and the outer layer is coated with external glue. When the inner sheath is squeezed, the aramid reinforcement member embedded inside it will effectively control the deformation. After the force is applied, the surface of the inner sheath is evenly stressed and finally becomes an arc shape, so that the inner sheath itself becomes a whole, and the large deformation caused by the local strong squeezing of the inner sheath of the optical cable is eliminated, which can effectively improve the performance.

[0027] (2) The present invention also restricts the selection of the embedded aramid yarn material, so that the comprehensive strength of the inner sheath and the amount of injection molding shrinkage are improved, which effectively controls the comprehensive shrinkage of the inner sheath, effectively reduces the bending amount of the optical fiber, and thus reduces the optical fiber loss.

[0028] (3) The aramid reinforcement members in the inner sheath of the present invention are arranged uniformly in a surrounding manner, so that the supporting force of the inner sheath is more uniform.

[0029] (4) The present invention also provides a method for preparing an inner sheath, which strictly controls the operation steps and extrusion temperature, effectively reduces the influence of the extrusion margin on the internal structure of the optical fiber, and can effectively maintain the stability of the internal structure of the optical fiber.

[0030] (5) The present invention strictly controls the operating temperature of each step in the preparation process, so that the glue is always in a semi-solid state in each stage before the operation is completed, which can effectively achieve the fusion of the inner and outer layers of glue and make the aramid reinforcement and the inner sheath become a whole, effectively improving their integrity and compressive resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments and in conjunction with the accompanying drawings, wherein

[0032] Figure 1 It is a structural schematic diagram of the present invention.

[0033] Figure 2 Schematic diagram of the structure of the aramid reinforcement.

[0034] Figure 3 It is a schematic diagram of the principle of the inner sheath of the present invention under stress state.

[0035] The reference numerals in the accompanying drawings are:

[0036] Sheath tube body 1, aramid reinforcement 2, aramid yarn 21, carbon fiber rod 22, bonding glue 23, outer layer glue 24. DETAILED DESCRIPTION

[0037] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0039] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0041] In the description of the embodiments of the present invention, it should be understood that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the inventive product is conventionally placed when used, or are the orientations or positional relationships conventionally understood by those skilled in the art. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0042] In the description of the embodiments of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. The present invention is further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the scope of protection of the present invention.

[0043] (Example 1)

[0044] like Figure 1 The present invention is an optical cable inner sheath, wherein aramid reinforcement members 2 are evenly arranged in the inner sheath tube body 1 with the center thereof as the center of the circle.

[0045] like Figure 2 The aramid reinforcement 2 includes aramid yarn 21, carbon fiber rod 22, adhesive glue 23 and external glue 24. The adhesive glue 23 is filled between the high modulus aramid yarn 21 and the carbon fiber rod 22 and spirally twisted.

[0046] The role of the carbon fiber rod 22 in the above structural design is to improve the overall strength of the aramid reinforcement 2. The materials are selected during the design process, wherein the high modulus aramid yarn 21 is prepared using aromatic ring structure raw materials, and the carbon fiber rod 212 is selected to have an elastic modulus above 580 GPa. Finally, the overall elastic modulus of the aramid reinforcement should be controlled above 450 GPa.

[0047] It should be emphasized that the aramid reinforcement 2 is extruded inside the sheath body to prevent the misalignment that causes the rigidity of the inner sheath to decrease. When the aramid reinforcement 2 is extruded outside the inner sheath body, the inner sheath 2 is deformed unevenly before and after being squeezed, and only one side is deformed, resulting in a decrease in overall strength, which is not conducive to protecting the internal cable core structure. When the aramid reinforcement 2 is extruded inside the sheath body of the inner sheath, the inner sheath is in a state before and after being squeezed. Figure 3 As shown, the inner sheath is deformed as a whole, and all the aramid reinforcement members 2 of the inner sheath are used for support during the compression process, so that the optical cable will be elliptical after being stressed.

[0048] The steps for preparing the aramid reinforcement 2 are as follows:

[0049] Paying off the carbon fiber rod 22 and the high modulus aramid yarn 21;

[0050] Glue is applied to the outer layer of the carbon fiber rod 22 and the high modulus aramid yarn 21, and preheated to maintain the glue in a semi-solid state;

[0051] The carbon fiber rod 22 and the high modulus aramid yarn 21 are twisted;

[0052] The outer layer glue 24 of the carbon fiber rod 22 and the high modulus aramid yarn 21 is cured.

[0053] The carbon fiber rod 22 and the aramid yarn 21 release all the components by active pay-off, and the pay-off tension is controlled at 350g-550g. The carbon fiber rod 22 at the inner end, the aramid yarn 21 and the carbon fiber rod 22 at the outer end are released in a straightened state, and a splitter plate is made. The splitter plate is divided into two layers, and the inner layer is provided with a glue filling device and a preheating device. The carbon fiber rod 22 at the inner end enters the splitter plate for positioning in turn, and the glue filling device is used for coating, and the preheating device is used for heating, and the preheating temperature is 40±5 ℃, so that the glue adhered to the carbon fiber rod 22 is in a semi-solid state, and then the twisting device is used to shape the pitch, and the carbon fiber rod 22 and the aramid yarn 21 at the inner end are twisted into one, and the twisting pitch is 10mm. After twisting, they are cured and shaped again, and the curing temperature is 65±5℃. The cured mixture is twisted with the carbon fiber rod 22 at the outer end through glue and extruded through a molding die, and shaped by baking, and the thermal curing temperature is: 75±5℃. After shaping, it is collected on a tray.

[0054] The preparation steps of the inner sheath are:

[0055] The central strength member of the cable is twisted with the loose tube and fixed by aramid yarn to form a cable core;

[0056] The cable core is molded from the center hole of the mold core, and the aramid reinforcement member 2 is molded around the cable core and then extruded to obtain an inner sheath;

[0057] In the step of putting on the mold, the mold core is a tubular structure. During the extrusion process, there is no contact between the cable core and the aramid reinforcement member 2, and the aramid reinforcement member 2 is located in the middle of the inner sheath layer.

[0058] Specifically, the central reinforcement and the loose tube are produced by SZ twisting and fixed by aramid yarn. The absolute value of the linear expansion coefficient of the aramid yarn used at 80°C is less than 5.3×10-6°C-1. The extremely low shrinkage reduces the problem of tightening the bundle tube due to thermal expansion and contraction during the temperature cycle, thereby reducing the optical fiber duty cycle and increasing the loss. The yarn pitch and the twisting pitch are adjusted according to the product structure. The cable core is filled with water-blocking cable paste to block water, while preventing the inner sheath from directly contacting the loose tube. During the extrusion process, if the inner sheath directly contacts the loose tube, the loose tube will expand due to heat, causing the excess length to change. At the same time, it is easy to adhere to the inner sheath tube body 1, and change with the inner sheath, thereby further inducing the excess length change, so the cable paste is fully filled. The cable core is molded from the center hole of the mold core, and the aramid strength member 2 enters from the evenly distributed holes on the mold core and is molded at the same time as the cable core. The sheath material is squeezed in from between the mold core and the mold sleeve. The mold core is a tubular structure. The cable core and the aramid strength member 2 can be effectively separated during extrusion, so that the aramid strength member 2 is extruded between the inner sheath and the sheath body 1, and the cable core is extruded in the sheath body 1 of the inner sheath. The extrusion temperature is from 155 to 185°C, and low-temperature extrusion is also to reduce the influence of heat on the excess length of the loose sheath.

[0059] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An inner sheath of an optical cable, characterized in that: The structure is tubular, comprising a sheath body (1) and aramid reinforcement members (2) uniformly distributed in the sheath, the aramid reinforcement members (2) comprising high modulus aramid yarn (21) and carbon fiber rods (22), adhesive glue (23) is filled between the aramid yarn (21) and the carbon fiber rods (22) and spirally twisted, and an outer layer of glue (24) is coated between the aramid reinforcement member and the sheath body.

2. The optical cable inner sheath according to claim 1, characterized in that: The absolute value of the linear expansion coefficient of the aramid yarn (21) at 80°C is less than 5.3×10 -6 ℃ -1 , elastic modulus ≥ 320 GPa, the elastic modulus of the carbon fiber rod (22) ≥ 580 GPa, and the comprehensive modulus ≥ 450 GPa.

3. The optical cable inner sheath according to claim 1, characterized in that: The aramid reinforcement (2) is evenly distributed in a 360° circle around the center of the cross section of the inner sheath tube body (1), and is placed at the center of the thickness of the inner sheath tube body (1) and integrated with it in the form of extrusion.

4. A method for preparing an inner sheath of an optical cable according to any one of claims 1 or 2, characterized in that The steps include: S1: The central strength member of the optical fiber is twisted with the loose tube and fixed by aramid yarn to form a cable core; S2: The cable core is molded from the center hole of the mold core, and the aramid reinforcement member (2) is molded around the cable core and then extruded to obtain an inner sheath; In the step of applying the mold, the mold core is a tubular structure, and during the extrusion process, the cable core and the aramid reinforcement member (2) do not come into contact with each other, and the aramid reinforcement member (2) is located in the middle of the sheath layer of the inner sheath.

5. The method for preparing an inner sheath of an optical cable according to claim 4, characterized in that: In the step S2, during the extrusion process, the cable core is molded from the center hole of the mold core, and the aramid reinforcement (2) enters from the holes evenly distributed on the mold core. During the extrusion process, the extrusion temperature is controlled to be 155 to 185°C.

6. The method for preparing an inner sheath of an optical cable according to claim 4, characterized in that: The processing steps of the aramid reinforcement (2) are as follows: Paying off the carbon fiber rod (22) and the aramid yarn (21); Applying adhesive glue (23) on the outer layer of the carbon fiber rod (22) and the aramid yarn (21), and preheating the adhesive glue to maintain the semi-solid state; The carbon fiber rod (22) and the aramid yarn (21) are subjected to a twisting process; The carbon fiber rod (22) and the outer layer glue (24) of the aramid yarn (21) are cured to complete the shaping; Baking the formed aramid reinforcement member (2); Conduct a qualitative closing.

7. The method for preparing an inner sheath of an optical cable according to claim 6, characterized in that: In the preheating step, the temperature is controlled to be 40±5°C and the glue is kept in a semi-solid state. In the glue curing process, the curing temperature is 65±5°C. In the baking step, the baking temperature is 75±5°C.