High-power thick electrode and preparation method and application thereof

By using gradient distribution and low-temperature drying technology of different particle sizes in lithium-ion capacitors, high-power thick electrodes are designed, which solves the problem of limited lithium ion diffusion kinetics at high magnifications of thick electrode sheets, and achieves high energy density, The combination of power density and super fast charging improves the overall performance of lithium-ion capacitors.

CN118969518APending Publication Date: 2024-11-15GUIZHOU MEILING POWER SUPPLY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411242445.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

There is a contradiction between the high load capacity and the lithium ion diffusion speed of the lithium ion, which makes it difficult to take into account the energy density and power density of the thick electrode sheet, especially at high magnification, the lithium ion diffusion kinetics are limited, and the utilization rate of the electrode active substances is reduced.

Method used

Using gradient distribution of different particle sizes, through the hierarchical design of small and large particle electrode slurries, the first layer of high compact density structure and the second layer of high porosity structure are formed, and the "ion and electron high-speed channel" is constructed, and the The low-temperature drying process reduces bubbles caused by solvent evaporation, forms a multi-layer pore gradient distribution, and reduces the lithium ion diffusion resistance.

Benefits of technology

It achieves a balance between high energy density, power density and super fast charging performance, reduces lithium ion diffusion resistance, avoids device micro-short circuitry, and improves device power performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969518A_ABST
    Figure CN118969518A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-power thick electrode in the technical field of lithium ion capacitors, and the method comprises the following steps: firstly, preparing small-particle electrode slurry, mixing a small-particle hard carbon material (particle size D50 is 1-3 [mu] m), a conductive agent and a binder, and adding a proper amount of solvent to adjust the viscosity to 4000-5000 mPa.s; secondly, large-particle electrode slurry is prepared, a large-particle hard carbon material (the particle size D50 is 5-9 microns), a conductive agent and a binder are mixed, and the viscosity is adjusted to 3000-4000 mPa.s; and finally, coating the small-particle electrode slurry on the surface of a current collector, drying, coating the large-particle electrode slurry, and drying to obtain the high-power thick electrode. The electrode has excellent performance of high energy density, power density, super fast charge and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion capacitors, and in particular relates to a high-power thick electrode and a preparation method and application thereof. Background Art

[0002] Ion capacitors are complex systems whose performance depends not only on electrode materials, electrolytes and diaphragms, but also on the structure of the cell, manufacturing equipment and processes, environment, cell grouping and production control. At present, the research hotspots of device technology are mainly concentrated on the modification and optimization of electrode materials, the development of new materials, the study of electrochemical processes and mechanisms, and the exploration of new devices. Materials are the basis of devices. Designing and synthesizing new materials with better performance is one of the means to continuously improve device performance. However, the performance of lithium-ion devices is closely related to the physical and chemical processes such as the transmission of electrons within the device, the transmission of lithium ions in the solid phase or electrolyte, and their embedding / de-embedding. In addition to the inherent properties of the electrode material, the microstructure of the device pole also has an important influence on these processes.

[0003] At present, in order to solve the problem of electric vehicle range, improving energy density is an important direction for the development of lithium-ion capacitors. The preparation of ultra-thick pole pieces with high coating amount is the most direct way to improve the specific energy of the device, which can effectively reduce the proportion of inactive substances, such as current collectors, pole ears, device shells, etc. With the increase of pole piece thickness (30-300μm), the specific energy of the device increases accordingly at lower rates; however, at higher rates, the lithium ion diffusion kinetics is limited, the utilization rate of electrode active materials decreases accordingly, and the energy density of the device is impaired. Therefore, for thick pole pieces, in order to ensure the lithium ion diffusion speed and the full utilization of active materials while ensuring high loading, it is more important to design and optimize the microstructure of the electrode. In addition, the energy density and power density of the device are two important parameters, but the two are contradictory. How to balance the two through the optimization design of the electrode microstructure is also the key to electrode design. Summary of the invention

[0004] The present invention aims to provide a method for preparing a high-power thick electrode, so as to take into account the high energy density, power density and super fast charging performance of the thick electrode.

[0005] A method for preparing a high-power thick electrode in this scheme comprises the following steps:

[0006] Step 1, preparation of small particle electrode slurry: mixing small particle hard carbon material, conductive agent and binder, adding appropriate amount of solvent and mixing evenly to obtain small particle electrode slurry; wherein the particle size D50 of the small particle hard carbon material is 1-3 μm, and the viscosity of the small particle electrode slurry is 4000-5000 mPa·s;

[0007] Step 2, preparation of large particle electrode slurry: mixing large particle hard carbon material, conductive agent and binder, adding appropriate amount of solvent and mixing evenly to obtain large particle electrode slurry; wherein the particle size D50 of the large particle hard carbon material is 5-9 μm, and the viscosity of the large particle electrode slurry is 3000-4000 mPa·s;

[0008] Step three: coat the surface of the current collector with small-particle electrode slurry, dry it at 60-80°C for 110-150 minutes to form a first electrode layer, and then coat the surface of the first electrode layer with large-particle electrode slurry, and then dry it to form a second electrode layer. The current collector, the first electrode layer and the second electrode layer together constitute the high-power thick electrode.

[0009] The beneficial effects of this solution are: the gradient distribution of different particle sizes is adopted to achieve a high porosity structure in the second layer and a high compaction density structure in the first layer, so that the electrode sheets can be finely designed at the hierarchical level, constructing a "high-speed channel for ions and electrons", reducing the diffusion resistance of lithium ions, slowing down capacity attenuation, and perfectly taking into account high energy density, power density, and super-fast charging performance.

[0010] Further, in step three, the drying includes preliminary drying, low-temperature drying and vacuum drying; preliminary drying refers to drying at a temperature of 60 to 80 ° C for 110 to 150 minutes; low-temperature drying refers to drying at a temperature of -20 to -40 ° C for 1.5 to 2.5 hours; vacuum drying refers to drying at a temperature of 120 to 140 ° C for 11 to 13 hours under a vacuum environment. In the traditional pole piece production process, the most commonly used blast heating for early drying is the hot air that dries the pole piece continuously. Due to the oven temperature, the solvent evaporates rapidly, and white spots are easily formed on the surface of the pole piece, which is also the most likely to cause micro-short circuits during the device charging and discharging process. This scheme introduces a low-temperature drying process in the pole piece drying process, which effectively reduces the bubbles caused by the rapid evaporation of the solvent on the pole piece surface, and avoids pole piece defects and device micro-short circuits. At the same time, using the principle of low-temperature drying, when the solid solvent sublimates, it leaves gaps that match the particle size of the Mars material, forming a multi-layer pole piece porosity gradient distribution, providing abundant migration channels for subsequent lithium ions, reducing the internal resistance of the device, and improving the power performance of the device.

[0011] Furthermore, the porosity of the first electrode layer is lower than the porosity of the second electrode layer.

[0012] Furthermore, the porosity of the first electrode layer is 25-30%.

[0013] Furthermore, the porosity of the second electrode layer is 30-35%.

[0014] Furthermore, if the total mass of the hard carbon material, the conductive agent and the binder is 100%, the mass percentage of the hard carbon material is 92% to 94.5%, the mass percentage of the conductive agent is 1% to 3.5%, and the mass percentage of the binder is 2% to 5%.

[0015] Furthermore, the thickness of the first electrode layer is 0-50 μm, the thickness of the second electrode layer is 0-50 μm, and the thickness of the first electrode layer and the second electrode layer are not zero at the same time.

[0016] Furthermore, the conductive agent is at least one of KS-6, CNTs, SP and carbon nanotube dispersion.

[0017] Furthermore, the binder is PVDF.

[0018] Furthermore, the solvent is NMP.

[0019] Experimental verification has shown that the high-power thick electrode prepared by the above preparation method has well taken into account the high energy density, power density and super-fast charging performance of the thick electrode. Therefore, the present application also requests protection for the high-power thick electrode prepared by the above preparation method, as well as the application of the high-power thick electrode in energy storage devices, especially ion capacitors.

[0020] In the present application, the first electrode layer is a coating formed by coating a small-particle electrode slurry on the surface of the current collector and drying it; the second electrode layer is a coating formed by coating a large-particle electrode slurry on the surface of the first electrode layer and drying it. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the SEM image of the electrode coated with a single layer of small-particle hard carbon;

[0022] Figure 2 The pore distribution diagram of the electrode coated with a single layer of small-particle hard carbon;

[0023] Figure 3 This is the SEM image of the electrode coated with a single layer of large-particle hard carbon;

[0024] Figure 4 The pore distribution diagram of the electrode coated with a single layer of large-grained hard carbon;

[0025] Figure 5 This is a SEM image of a high-power thick electrode prepared in Example 1 of the present invention;

[0026] Figure 6 This is a pore distribution diagram of a high-power thick electrode prepared in Example 1 of the present invention;

[0027] Figure 7 0.2C charge-discharge curves of each electrode in Example 1;

[0028] Figure 8 0.2C charge-discharge curves of the double-layer electrode {high-power thick electrode (low-temperature drying) and double-layer thick electrode (without low-temperature drying)} of Example 1;

[0029] Fig. 9 0.2C charge-discharge curve diagram of the high-power thick electrode prepared in Example 2 of the present invention;

[0030] Fig.10 This is a comparison diagram of the electrochemical impedance of the high-power thick electrode and the single-layer coated electrode prepared in Examples 1 to 5. DETAILED DESCRIPTION

[0031] The following is further described in detail through specific implementation methods:

[0032] The small-particle hard carbon D50 used in the following examples and comparative examples is 3 μm, and the large-particle hard carbon D50 is 6.2 μm. The electrode slurries used are all prepared from the same batch. The viscosity of the small-particle electrode slurry is 4600 mPa·s, and the viscosity of the large-particle electrode slurry is 3400 mPa·s.

[0033] Example 1: A method for preparing a high-power thick electrode

[0034] (1) Preparation of small particle electrode slurry

[0035] 30 g of small-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 48 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain small-particle electrode slurry.

[0036] (2) Preparation of large particle electrode slurry

[0037] 30 g of large-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 54 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain large-particle electrode slurry.

[0038] (3) Preparation of high power thick electrodes

[0039] 1) Double-layer electrode preparation

[0040] Keeping the total electrode thickness at 50 μm unchanged, the small-particle electrode slurry was uniformly coated on the copper foil with a thickness of 10 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min to obtain an electrode sheet coated with the first layer. The large-particle electrode slurry was coated on the first layer with a thickness of 40 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min, then transferred to a low-temperature drying oven at -30°C for drying for 2 h, and finally transferred to a vacuum drying oven at 140°C for drying for 12 h to obtain a high-power thick electrode.

[0041] Keeping the total electrode thickness at 50 μm unchanged, the small-particle electrode slurry was uniformly coated on the copper foil with a thickness of 10 μm, and preliminarily dried in a blast drying oven at 80°C for 130 min to obtain an electrode sheet coated with the first layer. The large-particle electrode slurry was coated on the first layer with a thickness of 40 μm, and preliminarily dried in a blast drying oven at 80°C for 130 min, and then transferred to a vacuum drying oven and dried at 140°C for 13 h to obtain a double-layer thick electrode without low-temperature drying.

[0042] 2) Single-layer electrode preparation

[0043] The small particle electrode slurry was coated with 50μm, the large particle electrode slurry was coated with 50μm, and the single-layer electrode prepared by mixing the small particle electrode slurry and the large particle electrode slurry was used for comparative analysis. The details are as follows:

[0044] The small particle electrode slurry was uniformly coated on the copper foil with a thickness of 50 μm, initially dried in an 80°C forced air drying oven for 130 min, then transferred to a low temperature drying oven at -30°C for 2 h, and finally transferred to a vacuum drying oven at 140°C for 12 h to obtain a small particle hard carbon single-layer coated electrode.

[0045] The large-particle electrode slurry was uniformly coated on the copper foil with a thickness of 50 μm, initially dried in an 80°C forced air drying oven for 130 min, then transferred to a low-temperature drying oven at -30°C for 2 h, and finally transferred to a vacuum drying oven at 140°C for 12 h to obtain a large-particle hard carbon single-layer coated electrode.

[0046] The small particle electrode slurry and the large particle electrode slurry were mixed and evenly coated on the copper foil with a thickness of 50 μm. The mixture was initially dried in an 80°C forced air drying oven for 130 min, then transferred to a low temperature drying oven at -30°C for 2 h, and finally transferred to a vacuum drying oven at 140°C for 12 h to obtain a large particle hard carbon single-layer coated electrode.

[0047] Figure 1 , Figure 2 They are the SEM image and void distribution diagram of the unrolled electrode coated with a single layer of small-particle hard carbon. Figure 3 , Figure 4The SEM images and void distribution diagrams of the large particle hard carbon single layer coated electrode are shown in Figure 2. The average porosity of the small particle hard carbon single layer coated electrode and the large particle hard carbon single layer coated electrode calculated by Image-J software is 33.4% and 49.37%, respectively. The average porosity of the small particle hard carbon single layer coated electrode and the large particle hard carbon single layer coated electrode after rolling is 28.7% and 33.2%, respectively.

[0048] Figure 5 , Figure 6 The SEM images and void distribution diagrams of the high-power thick electrode after rolling in Example 1 are shown respectively. The pores can be clearly distinguished from the cross-sectional morphology. The average porosity of the double-layer electrode calculated by Image-J software is 27.1%. Compared with the double-layer, the electrode prepared by the single-layer coating process has a relatively high porosity and uneven pore distribution, while the electrode prepared by the double-layer coating process has a more uniform and dense pore structure, which is conducive to forming a denser structure during the rolling process.

[0049] Figure 7 The 0.2C charge and discharge curves of the single-layer electrodes and double-layer electrodes of this embodiment are compared. The single-layer large-particle electrode has a higher porosity, but the higher the porosity, the better. Too high a porosity will result in the inability to form effective contact between the conductive agents and to build a complete three-dimensional conductive network. Therefore, the electrode impedance is large and the capacity cannot be fully utilized. The single-layer small-particle electrode forms a relatively dense pore structure and tortuosity, which increases the diffusion path of lithium ions, resulting in increased electrode impedance and decreased power performance. The single-layer electrode formed by the mixture of large and small particles takes into account the characteristics of small and large particles, forming a uniformly distributed void structure with better power performance. However, compared with the double-layer electrode (high-power thick electrode), the void structure formed by the interweaving of large and small particles has a larger tortuosity. The double-layer electrode combines the advantages of large and small particle electrodes. Figure 8 As shown in the figure, the double-layer electrode (high-power thick electrode) is combined with a low-temperature drying process to create gaps with matching active material particle sizes, forming a multi-layer electrode with a porosity gradient distribution, providing abundant migration channels for subsequent lithium ions, reducing device internal resistance, and improving device power performance. Compared with the conventional drying process, the electrode sheet after low-temperature drying has a higher first efficiency and reversible capacity.

[0050] Example 2: A method for preparing a high-power thick electrode

[0051] (1) Preparation of small particle electrode slurry

[0052] 30 g of small-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 48 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain small-particle electrode slurry.

[0053] (2) Preparation of large particle electrode slurry

[0054] 30 g of large-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 54 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain large-particle electrode slurry.

[0055] (3) Preparation of high power thick electrodes

[0056] Keeping the total electrode thickness at 50 μm unchanged, the small-particle electrode slurry was uniformly coated on the copper foil with 20 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min to obtain an electrode sheet coated with the first layer. The large-particle electrode slurry was coated on the first layer with 30 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min, then transferred to a low-temperature drying oven at -30°C for drying for 2 h, and finally transferred to a vacuum drying oven at 140°C for drying for 12 h to obtain a high-power thick electrode.

[0057] Example 3: A method for preparing a high-power thick electrode

[0058] (1) Preparation of small particle electrode slurry

[0059] 30 g of small-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 48 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain small-particle electrode slurry.

[0060] (2) Preparation of large particle electrode slurry

[0061] 30 g of large-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 54 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain large-particle electrode slurry.

[0062] (3) Preparation of high power thick electrodes

[0063] Keeping the total electrode thickness at 50 μm unchanged, the small-particle electrode slurry was uniformly coated on the copper foil with 25 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min to obtain an electrode sheet coated with the first layer. The large-particle electrode slurry was coated on the first layer with 25 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min, then transferred to a low-temperature drying oven at -30°C for drying for 2 h, and finally transferred to a vacuum drying oven at 140°C for drying for 12 h to obtain a high-power thick electrode.

[0064] Example 4: A method for preparing a high-power thick electrode

[0065] (1) Preparation of small particle electrode slurry

[0066] 30 g of small-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 48 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain small-particle electrode slurry.

[0067] (2) Preparation of large particle electrode slurry

[0068] 30 g of large-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 54 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain large-particle electrode slurry.

[0069] (3) Preparation of high power thick electrodes

[0070] Keeping the total electrode thickness at 50 μm unchanged, the small-particle electrode slurry was uniformly coated on the copper foil with a thickness of 30 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min to obtain an electrode sheet coated with the first layer. The large-particle electrode slurry was coated on the first layer with a thickness of 20 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min, then transferred to a low-temperature drying oven at -30°C for drying for 2 h, and finally transferred to a vacuum drying oven at 140°C for drying for 12 h to obtain a high-power thick electrode. Fig. 9 This is the 0.2C charge and discharge curve of the high-power thick electrode of this embodiment, and the gram-specific capacity reaches 312mAh / g.

[0071] Example 5: A method for preparing a high-power thick electrode

[0072] (1) Preparation of small particle electrode slurry

[0073] 30 g of small-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 48 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain small-particle electrode slurry.

[0074] (2) Preparation of large particle electrode slurry

[0075] 30 g of large-particle hard carbon, 0.81 g of conductive agent (SP and KS-6 mass ratio is 1:1), and 1.62 g of binder PVDF were weighed respectively, stirred at 800 r / min for 6 min in a planetary mixer, and then 54 g of solvent NMP was added, and stirred at 1200 r / min and 1000 r / min for 6 min and 5 min respectively to obtain large-particle electrode slurry.

[0076] (3) Preparation of high power thick electrodes

[0077] Keeping the total electrode thickness at 50 μm unchanged, the small-particle electrode slurry was evenly coated on the copper foil at 40 μm, and preliminarily dried in an 80°C forced air drying oven for 130 min to obtain an electrode sheet coated with the first layer. A second layer of electrode slurry of 10 μm was coated on the first layer, and preliminarily dried in an 80°C forced air drying oven for 30 min, then transferred to a low-temperature drying oven at -30°C for drying for 2 h, and finally transferred to a vacuum drying oven at 140°C for drying for 12 h to obtain a high-power thick electrode.

[0078] Electrochemical performance test

[0079] In order to detect the performance of the high-power thick electrode of the present invention, the half-device and full-device testing methods are used. The above single-layer motor and the high-power thick electrodes of Examples 1 to 5 are used as negative electrodes; the full device uses lithium cobalt oxide as the positive electrode active material, the electrolyte is the electrolyte for high-power lithium-ion devices, and the diaphragm uses a ceramic diaphragm; the half-device uses a lithium strip as the counter electrode, and other conditions are the same. The capacity test and AC impedance test of the half-device are carried out at a rate of 0.2C, and the power performance test of the full device is carried out. The charge and discharge voltage is limited to 2.5 to 4.3V, and the electrochemical impedance comparison chart is shown in the attached figure. Fig.10 The test results are shown in the following table:

[0080]

[0081] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for preparing a high-power thick electrode, characterized in that: The following steps are involved: Step 1, preparation of small particle electrode slurry: mixing small particle hard carbon material, conductive agent and binder, adding appropriate amount of solvent and mixing evenly to obtain small particle electrode slurry; wherein the particle size D50 of the small particle hard carbon material is 1-3 μm, and the viscosity of the small particle electrode slurry is 4000-5000 mPa·s; Step 2, preparation of large particle electrode slurry: mixing large particle hard carbon material, conductive agent and binder, adding appropriate amount of solvent and mixing evenly to obtain large particle electrode slurry; wherein the particle size D50 of the large particle hard carbon material is 5-9 μm, and the viscosity of the large particle electrode slurry is 3000-4000 mPa·s; Step three: coat the surface of the current collector with small-particle electrode slurry, dry it at 60-80°C for 110-150 minutes to form a first electrode layer, and then coat the surface of the first electrode layer with large-particle electrode slurry, and then dry it to form a second electrode layer. The current collector, the first electrode layer and the second electrode layer together constitute the high-power thick electrode.

2. The method for preparing a high-power thick electrode according to claim 1, characterized in that: In step three, the drying includes preliminary drying, low-temperature drying and vacuum drying; preliminary drying refers to drying at a temperature of 60 to 80°C for 110 to 150 minutes; low-temperature drying refers to drying at a temperature of -20 to -40°C for 1.5 to 2.5 hours; vacuum drying refers to drying at a temperature of 120 to 140°C under a vacuum environment for 11 to 13 hours.

3. The method for preparing a high-power thick electrode according to claim 2, characterized in that: The porosity of the first electrode layer is lower than that of the second electrode layer.

4. The method for preparing a high-power thick electrode according to claim 3, characterized in that: The porosity of the first electrode layer is 25-30%.

5. The method for preparing a high-power thick electrode according to claim 4, characterized in that: The porosity of the second electrode layer is 30-35%.

6. The method for preparing a high-power thick electrode according to claim 5, characterized in that: The total mass of the hard carbon material, the conductive agent and the binder is 100%, the mass percentage of the hard carbon material is 92% to 94.5%, the mass percentage of the conductive agent is 1% to 3.5%, and the mass percentage of the binder is 2% to 5%.

7. The method for preparing a high-power thick electrode according to claim 6, characterized in that: The thickness of the first electrode layer is 0-50 μm, the thickness of the second electrode layer is 0-50 μm, and the thickness of the first electrode layer and the second electrode layer are not zero at the same time.

8. The method for preparing a high-power thick electrode according to claim 7, characterized in that: The conductive agent is at least one of KS-6, CNTs, SP and carbon nanotube dispersion.

9. The method for preparing a high-power thick electrode according to claim 8, characterized in that: The binder is PVDF.

10. The method for preparing a high-power thick electrode according to claim 9, characterized in that: The solvent is NMP.

11. A high-power thick electrode, characterized in that: The high-power thick electrode is prepared by the preparation method of any one of claims 1 to 10.

12. Use of the high-power thick electrode according to claim 11 in energy storage devices.

13. The use of the high-power thick electrode in an energy storage device according to claim 12, characterized in that: The energy storage device is an ion capacitor.

14. The use of the high-power thick electrode in an energy storage device according to claim 13, characterized in that: The energy storage device is a negative electrode sheet for an ion capacitor.

Citation Information

Patent Citations

  • Positive pole plate of lithium-sulfur cell and manufacturing method thereof

    CN101399329A

  • Current collector, pole piece with same and lithium battery

    CN109830690A

  • Preparation method and application of electrode plate

    CN114068857A

  • Negative plate, preparation method thereof and lithium iron phosphate battery

    CN115440932A

  • Air electrode preparation method and metal-air battery

    CN116598417A