Method for improving polycrystalline silicon filling of SGT source and SGT device
By expanding the trench opening in the SGT source polysilicon filling process and forming an inverted trapezoidal opening, the problems of early sealing and joints caused by polysilicon filling are solved, the device performance and reliability are improved, and the subsequent processes are stabilized.
Patent Information
- Application Number
- CN202411087530.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing SGT source polysilicon filling process, due to the premature closing of the top of the trench, the polysilicon seals in advance, forming joints, affecting the device's voltage resistance and leakage performance, and the depth-to-width ratio trench filling uniformity is poor.
By expanding the opening before the groove is filled, an inverted trapezoidal opening similar to a funnel is formed, and a combination process of the insulating layer and the barrier layer is used to ensure that the polysilicon fills the entire filling space and avoids premature sealing.
Improve the filling capability of undoped/doped SGT polysilicon, eliminates the adverse impact of filling on device performance, improves the performance and reliability of semiconductor devices, and protects the film layer on the side walls and bottom of the trench, stabilizing subsequent Craft.
Smart Images

Figure CN118969609A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing, and in particular to a method for improving SGT source polysilicon filling and an SGT device. Background Art
[0002] In the existing process of forming source polysilicon in SGT (Shield Gate Trench) devices, when filling polysilicon 4 in a high aspect ratio trench, the top of the trench will close prematurely, resulting in premature sealing of the polysilicon 4, causing the polysilicon 4 to be generated in the middle of the polysilicon 4. Figure 1 The seams shown in the figure are different, and the severity of the seams in each trench is different, resulting in poor uniformity of the subsequent etching depth of the polysilicon 4, affecting the withstand voltage, leakage and other performances of the SGT device. Summary of the invention
[0003] The purpose of the present application is to provide a method for improving SGT source polysilicon filling and an SGT device, by enlarging the opening before trench filling to form an inverted trapezoidal opening similar to a funnel, thereby improving the undoped / doped SGT polysilicon filling capacity, and eliminating the premature sealing seam phenomenon after polysilicon filling, thereby solving the polysilicon filling problem of high aspect ratio trenches, eliminating the adverse effects of polysilicon filling on device performance, and thus improving the performance and reliability of semiconductor devices.
[0004] To achieve the above object, the present application provides a method for improving SGT source polysilicon filling, comprising:
[0005] providing a substrate having a groove;
[0006] Depositing an insulating layer on the sidewall and bottom of the trench to form a first filling space;
[0007] Filling a barrier layer in the first filling space; the barrier layer has a height lower than the shoulder of the groove, so that the insulating layer at the opening position of the groove is exposed;
[0008] Removing part of the insulating layer at the opening position, so that the thickness of the insulating layer at the opening position decreases in sequence along a direction toward the opening, forming an inverted trapezoidal opening;
[0009] removing the barrier layer to form a second filling space having the inverted trapezoidal opening;
[0010] Polysilicon is deposited in the second filling space so that the polysilicon fills the entire second filling space to form a source polysilicon structure.
[0011] Optionally, when the insulating layer is an oxide layer, depositing the insulating layer on the sidewall and the bottom of the trench to form a first filling space includes:
[0012] Depositing the oxide layer on the sidewall and bottom of the trench by SACVD to form the first filling space;
[0013] When the insulating layer is a nitride layer, depositing the insulating layer on the sidewall and the bottom of the trench to form a first filling space includes:
[0014] The nitride layer is deposited on the sidewall and bottom of the trench by using a furnace tube to form the first filling space.
[0015] Optionally, removing part of the insulating layer at the opening position so that the thickness of the insulating layer at the opening position decreases in sequence along a direction toward the opening to form an inverted trapezoidal opening comprises:
[0016] A portion of the insulating layer at the opening position is removed by dry etching or wet etching, so that the thickness of the insulating layer at the opening position decreases in sequence along a direction toward the opening, thereby forming an inverted trapezoidal opening.
[0017] Optionally, depositing polysilicon in the second filling space so that the polysilicon fills the entire second filling space includes:
[0018] The polysilicon is deposited in the second filling space by using a furnace tube, so that the polysilicon fills the entire second filling space.
[0019] Optionally, the barrier layer is a fluid material.
[0020] Optionally, filling the first filling space with a barrier layer includes:
[0021] Filling the first filling space with a fluid material so that the fluid material fills the entire first filling space;
[0022] The fluid material is etched to a level below the shoulder of the trench, so that the insulating layer at the opening of the trench is exposed.
[0023] Optionally, the fluid material is photoresist; and removing the barrier layer to form a second filling space having the inverted trapezoidal opening comprises:
[0024] The remaining photoresist in the first filling space is stripped off by combining an ashing process and a wet stripping process to form the second filling space having the inverted trapezoidal opening.
[0025] Optionally, when the depth of the trench is greater than 2.2 μm and the filling aspect ratio of the polysilicon is greater than 15, the thickness of the photoresist ranges from 2000Å to 40000Å, including the values at both ends.
[0026] Optionally, the etching depth ranges from 2000Å to 6000Å below the substrate surface, including both end values.
[0027] To achieve the above objectives, the present application also provides an SGT device, including: a source polysilicon structure prepared by the above-mentioned method for improving SGT source polysilicon filling.
[0028] The present application provides a method for improving SGT source polysilicon filling, comprising: providing a substrate with a groove; depositing an insulating layer on the sidewall and bottom of the groove to form a first filling space; filling a barrier layer in the first filling space; the height of the barrier layer is lower than the shoulder of the groove, so that the insulating layer at the opening position of the groove is exposed; removing part of the insulating layer at the opening position, so that the thickness of the insulating layer at the opening position decreases successively along the direction toward the opening, forming an inverted trapezoidal opening; removing the barrier layer to form a second filling space with the inverted trapezoidal opening; depositing polysilicon in the second filling space, so that the polysilicon fills the entire second filling space, forming a source polysilicon structure.
[0029] Obviously, the present application expands the opening before the trench is filled, while ensuring that the thickness and structure of the side wall and bottom film layer remain unchanged before the polysilicon is filled, to form an inverted trapezoidal opening similar to a funnel. The funnel-like morphology improves the filling capacity of undoped / doped SGT polysilicon, and there is no premature sealing seam phenomenon after polysilicon filling, which solves the polysilicon filling problem of high aspect ratio trenches and eliminates the adverse effects of polysilicon filling on device performance, thereby improving the performance and reliability of semiconductor devices. At the same time, the film layer on the side wall and bottom of the trench is protected by filling the barrier layer, which is beneficial to the improvement of subsequent process stability and device capabilities. The present application also provides an SGT device with the above-mentioned beneficial effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0031] Figure 1 A schematic diagram of a seam produced after polysilicon deposition;
[0032] Figure 2 is a schematic diagram of the arrival angle of the groove surface;
[0033] Figure 3 This is a schematic diagram of the closing morphology after SACVD deposition;
[0034] Figure 4 Schematic diagram of the morphology after polysilicon etching;
[0035] Figure 5 Schematic diagram of a polysilicon filling problem causing poor lead-out;
[0036] Figure 6 A flow chart of a method for improving SGT source polysilicon filling provided in an embodiment of the present application;
[0037] Figure 7 is a cross-sectional view of the structure after the oxide layer is deposited;
[0038] Figure 8 This is the cross-sectional view of the structure after gluing;
[0039] Fig. 9 is a cross-sectional view of the structure after photoresist etching;
[0040] Fig.10 Schematic diagram of the funnel-like morphology that disappears after etching;
[0041] Fig.11 This is the cross-sectional view of the structure after debonding;
[0042] Fig.12 This is a cross-sectional view of a problem-free structure after polysilicon deposition.
[0043] The following are the descriptions of the reference numerals:
[0044] 1-Silicon substrate; 2-Oxide layer or nitride layer; 3-Photoresist; 4-Polysilicon; 5-Gate. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0046] Currently, the demand for semiconductor integration is getting higher and higher, and the process feature size is getting smaller and smaller. As a result, the trench size and the gap between filling materials are getting smaller and smaller, resulting in a greatly increased aspect ratio and difficulty of deep trench filling.
[0047] The thickness of the deposited film by SACVD (Sub-Atmospheric Pressure Chemical Vapor Deposition) is strongly correlated with the arrival angle on the wafer surface. The arrival angle on the surface of the SGT groove is as follows: Figure 2As shown, angle A has the largest arrival angle of 270°, so more source material will be deposited, while angle B has an arrival angle of only 180°, so less source material will be deposited, thus forming the following Figure 3 For a high aspect ratio trench with a relatively small size and a relatively deep trench, the trench shoulder closing will greatly affect the subsequent deposition of polysilicon 4, resulting in the formation of a polysilicon 4 in the middle of the trench. Figure 1 The seams shown affect the subsequent Figure 4 The polysilicon 4 etching process depth uniformity and HDP (High-Density Plasma) deposition aspect ratio shown in the figure result in Figure 5 The device shown has problems such as short circuit between gate 5 (Gate, G) and source (Source, S) and poor lead-out of source polysilicon, which seriously affect the performance and reliability of the device. Therefore, the present application provides a method for improving the filling of SGT source polysilicon, by expanding the opening before trench filling to form an inverted trapezoidal opening similar to a funnel, thereby improving the filling capacity of undoped / doped SGT polysilicon, and there is no premature sealing seam phenomenon after polysilicon filling, which solves the polysilicon filling problem of high aspect ratio trenches, eliminates the adverse effects of polysilicon filling on device performance, and thus improves the performance and reliability of semiconductor devices.
[0048] Please refer to Figure 1 , Figure 1 A flow chart of a method for improving SGT source polysilicon filling provided in an embodiment of the present application, the method may include:
[0049] S101: providing a substrate having a groove.
[0050] This embodiment does not limit the specific type of substrate, and the specific type of substrate can be determined according to actual needs, for example, the substrate can be a silicon substrate. This embodiment does not limit the specific method of forming the groove, as long as it can ensure that an inwardly recessed filling space can be formed on the substrate surface.
[0051] S102: depositing an insulating layer on the sidewall and bottom of the trench to form a first filling space.
[0052] It should be noted that the first filling space is the remaining filling space in the trench after the insulating layer is deposited on the sidewall and bottom of the trench, that is, the sidewall and bottom of the first filling space are covered with the insulating layer.
[0053] The present embodiment does not limit the specific type of the insulating layer, and may be any dielectric layer with insulating properties. For example, the insulating layer may be an oxide layer or a nitride layer. The oxide layer may include but is not limited to SiO 2(silicon dioxide) layer, and the nitride layer may include but is not limited to a SiN (silicon nitride) layer. This embodiment does not limit the specific method of depositing the insulating layer, and a corresponding deposition method may be selected according to the specific type of the insulating layer. For example, when the insulating layer is an oxide layer, SACVD may be used to deposit the oxide layer on the sidewall and bottom of the trench to form a first filling space; when the insulating layer is a nitride layer, a furnace tube may be used to deposit the nitride layer on the sidewall and bottom of the trench to form a first filling space.
[0054] Furthermore, in this embodiment, an insulating layer can be deposited on the sidewall and bottom of the trench, and on the non-trench area of the substrate surface, so as to provide an insulating layer for other structures subsequently formed on the substrate surface.
[0055] S103: filling a barrier layer in the first filling space; the height of the barrier layer is lower than the shoulder of the trench, so that the insulating layer at the opening position of the trench is exposed.
[0056] It should be noted that in this embodiment, a barrier layer whose height is lower than the shoulder of the groove is filled in the first filling space having an insulating layer on the sidewall and the bottom. In the subsequent process of removing part of the insulating layer at the opening position to form an inverted trapezoidal opening, the barrier layer can be used to protect the oxide layer on the sidewall and the bottom of the groove and keep it unchanged, thereby avoiding affecting the device performance.
[0057] This embodiment does not limit the specific type of the barrier layer, as long as it can protect the insulating layer at the sidewall and bottom of the trench from being damaged during the subsequent formation of the inverted trapezoidal opening. Further, in order to facilitate filling the first empty space, this embodiment can select a material with good fluidity as the barrier layer, that is, the barrier layer can be a fluid material; the fluid material can include but is not limited to photoresist.
[0058] The present embodiment does not limit the specific method of filling the barrier layer in the first filling space, as long as it is ensured that a barrier layer with a height lower than the shoulder of the groove can be formed in the first filling space so that the insulating layer at the opening position of the groove is exposed. For example, a fluid material can be filled in the first filling space so that the fluid material fills the entire first filling space; the fluid material is etched to a height lower than the shoulder of the groove so that the insulating layer at the opening position of the groove is exposed.
[0059] This embodiment does not limit the specific thickness of the photoresist, and the specific thickness of the photoresist can be determined according to actual conditions. For example, when the depth of the groove is greater than 2.2 μm and the filling aspect ratio of polysilicon is greater than 15, the thickness of the photoresist can range from 2000Å to 40000Å, including the values at both ends. It should be noted that the thickness of the photoresist can be appropriately thinned according to the specific depth of the groove.
[0060] S104: removing part of the insulating layer at the opening position, so that the thickness of the insulating layer at the opening position decreases in sequence along a direction toward the opening, thereby forming an inverted trapezoidal opening.
[0061] It should be noted that after the barrier layer with a height lower than the shoulder of the groove is filled in the first filling space, the insulating layer at the opening position of the groove will be exposed. By removing part of the insulating layer at the opening position, the thickness of the insulating layer at the opening position is gradually reduced along the direction toward the opening, and an inverted trapezoidal opening can be formed at the opening position of the first filling space.
[0062] This embodiment does not limit the specific method of removing the insulating layer, as long as the insulating layer can be removed, for example, dry etching or wet etching can be used to remove part of the insulating layer at the opening position, so that the thickness of the insulating layer at the opening position decreases in the direction toward the opening, forming an inverted trapezoidal opening. It should be noted that dry etching is an anisotropic etching method, and wet etching is an isotropic etching method.
[0063] This embodiment does not limit the specific thickness of the removed insulating layer, and the specific size of the inverted trapezoidal opening can be determined according to the actual size of the groove, thereby determining the specific thickness of the removed insulating layer.
[0064] S105: removing the barrier layer to form a second filling space having an inverted trapezoidal opening.
[0065] It should be noted that the sidewalls and bottom of the second filling space formed after removing the barrier layer have an insulating layer, and the thickness of the insulating layer at the opening position decreases gradually in the direction toward the opening, so that the second filling space has an inverted trapezoidal opening.
[0066] This embodiment does not limit the specific method of removing the barrier layer, and the corresponding removal method can be selected according to the specific type of the barrier layer. For example, when the fluid material is photoresist, an ashing process and a wet stripping process can be combined to strip the remaining photoresist in the first filling space to form a second filling space with an inverted trapezoidal opening. It should be noted that the ashing process and the wet stripping process used in this embodiment can be used to strip the remaining photoresist in the first filling space to avoid contaminating subsequent equipment.
[0067] S106: depositing polysilicon in the second filling space, so that the polysilicon fills the entire second filling space, forming a source polysilicon structure.
[0068] It should be noted that, since an inverted trapezoidal opening similar to a funnel is formed before filling the polysilicon, it can prevent the polysilicon from closing prematurely, which is beneficial to the deposition of polysilicon in the trench.
[0069] This embodiment does not limit the specific method of depositing polysilicon, as long as the polysilicon can fill the entire second filling space, for example, a furnace tube can be used to deposit polysilicon in the second filling space, so that the polysilicon fills the entire second filling space. Furthermore, this embodiment can also deposit polysilicon in the second filling space, so that the polysilicon fills the entire second filling space and covers the non-groove area on the substrate surface.
[0070] Based on the above embodiments, the present application expands the opening before the trench is filled, while ensuring that the thickness and structure of the sidewall and bottom film layers before polysilicon filling remain unchanged, to form an inverted trapezoidal opening similar to a funnel. The funnel-like morphology improves the filling capacity of undoped / doped SGT polysilicon, and there is no premature sealing seam phenomenon after polysilicon filling, which solves the polysilicon filling problem of high aspect ratio trenches and eliminates the adverse effects of polysilicon filling on device performance, thereby improving the performance and reliability of semiconductor devices. At the same time, the film layers on the sidewalls and bottom of the trench are protected by filling the barrier layer, which is conducive to the improvement of subsequent process stability and device capabilities.
[0071] An embodiment of the present application further provides an SGT device, which may include: a source polysilicon structure prepared by the above-mentioned method for improving SGT source polysilicon filling.
[0072] Based on the above embodiments, the source polysilicon structure in the SGT device of the present application is prepared by the above method for improving the filling of SGT source polysilicon, and also has the above beneficial effects. The above method for improving the filling of SGT source polysilicon, under the premise of ensuring that the thickness and structure of the side wall and bottom film layer before polysilicon filling remain unchanged, expands the opening before the trench is filled to form an inverted trapezoidal opening similar to a funnel. The undoped / doped SGT polysilicon filling capacity is improved by the funnel-like morphology, and there is no premature sealing seam phenomenon after polysilicon filling, which solves the polysilicon filling problem of high aspect ratio trenches and eliminates the adverse effects of polysilicon filling on device performance, thereby improving the performance and reliability of semiconductor devices. At the same time, the film layer on the sidewall and bottom of the trench is protected by filling the barrier layer, which is beneficial to the improvement of subsequent process stability and device capabilities.
[0073] The following is a specific example to illustrate the above method of improving SGT source polysilicon filling. Please refer to Figures 7 to 12 , the process is as follows:
[0074] Step 1: Provide a silicon substrate 1 with a groove, and deposit an oxide layer or a nitride layer 2 on the sidewall and bottom of the groove, such as Figure 7 As shown;
[0075] Step 2: Select photoresist 3 with good fluidity to fill the grooves. The effect is as follows: Figure 8As shown; when the trench depth is greater than 2.2μm and the polysilicon 4 filling aspect ratio is greater than 15, the photoresist 3 thickness selection range is: 2000Å-40000Å (including the values at both ends), and it can be appropriately thinned according to the trench depth.
[0076] Step 3: Etch the photoresist 3 to below the groove shoulder, exposing the groove end position. Fig. 9 As shown; etching depth range: 2000Å-6000Å below the surface of the silicon substrate 1 (including the values at both ends).
[0077] Step 4: Use anisotropic dry etching or isotropic wet etching to etch away the excess oxide layer or nitride layer 2 exposed outside to form an inverted trapezoidal opening similar to a funnel. The effect is as follows: Fig.10 As shown. The oxide layer 2 on the sidewall and bottom of the trench is protected by the photoresist 3 and remains unchanged, which does not affect the device performance;
[0078] Step 5: Stripping: Use a combination of ashing and wet stripping processes to strip the remaining photoresist 3 in the grooves. Fig.11 As shown, so as not to contaminate subsequent equipment;
[0079] Step 6: Polysilicon 4 deposition: Polysilicon 4 is deposited in the trench. The effect is as follows: Fig.12 As shown, the funnel-like morphology enlarges the opening to prevent the polysilicon 4 from closing prematurely, which is beneficial to the deposition of the polysilicon 4 in the trench.
[0080] Specific examples are used herein to illustrate the principles and implementation methods of the present application, and the embodiments are in a progressive relationship, each embodiment focuses on the differences from other embodiments, and the same and similar parts between the embodiments can be referred to each other. The description of the above embodiments is only used to help understand the method and core ideas of the present application. For ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
[0081] It should also be noted that, in this specification, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements.
Claims
1. A method for improving SGT source polysilicon filling, characterized in that: include: providing a substrate having a groove; Depositing an insulating layer on the sidewall and bottom of the trench to form a first filling space; Filling a barrier layer in the first filling space; the barrier layer has a height lower than the shoulder of the groove, so that the insulating layer at the opening position of the groove is exposed; Removing part of the insulating layer at the opening position, so that the thickness of the insulating layer at the opening position decreases in sequence along a direction toward the opening, forming an inverted trapezoidal opening; removing the barrier layer to form a second filling space having the inverted trapezoidal opening; Polysilicon is deposited in the second filling space so that the polysilicon fills the entire second filling space to form a source polysilicon structure.
2. The method for improving SGT source polysilicon filling according to claim 1, characterized in that: When the insulating layer is an oxide layer, depositing the insulating layer on the sidewall and the bottom of the trench to form a first filling space includes: Depositing the oxide layer on the sidewall and bottom of the trench by SACVD to form the first filling space; When the insulating layer is a nitride layer, depositing the insulating layer on the sidewall and the bottom of the trench to form a first filling space includes: The nitride layer is deposited on the sidewall and bottom of the trench by using a furnace tube to form the first filling space.
3. The method for improving SGT source polysilicon filling according to claim 1, characterized in that: The step of removing a portion of the insulating layer at the opening position so that the thickness of the insulating layer at the opening position decreases in a direction toward the opening to form an inverted trapezoidal opening comprises: A portion of the insulating layer at the opening position is removed by dry etching or wet etching, so that the thickness of the insulating layer at the opening position decreases in sequence along a direction toward the opening, thereby forming an inverted trapezoidal opening.
4. The method for improving SGT source polysilicon filling according to claim 1, characterized in that: The step of depositing polysilicon in the second filling space so that the polysilicon fills the entire second filling space includes: The polysilicon is deposited in the second filling space by using a furnace tube, so that the polysilicon fills the entire second filling space.
5. The method for improving SGT source polysilicon filling according to any one of claims 1 to 4, characterized in that: The barrier layer is a fluid material.
6. The method for improving SGT source polysilicon filling according to claim 5, characterized in that: The step of filling the first filling space with a barrier layer comprises: Filling the first filling space with a fluid material so that the fluid material fills the entire first filling space; The fluid material is etched to a level below the shoulder of the trench, so that the insulating layer at the opening of the trench is exposed.
7. The method for improving SGT source polysilicon filling according to claim 6, characterized in that: The fluid material is photoresist; The step of removing the barrier layer to form a second filling space having the inverted trapezoidal opening comprises: The remaining photoresist in the first filling space is stripped off by combining an ashing process and a wet stripping process to form the second filling space having the inverted trapezoidal opening.
8. The method for improving SGT source polysilicon filling according to claim 7, characterized in that: When the depth of the trench is greater than 2.2 μm and the filling aspect ratio of the polysilicon is greater than 15, the thickness of the photoresist ranges from 2000Å to 40000Å, including the values at both ends.
9. The method for improving SGT source polysilicon filling according to claim 6, characterized in that: The etching depth ranges from 2000Å to 6000Å below the substrate surface, inclusive.
10. An SGT device, characterized in that: include: A source polysilicon structure prepared by the method for improving SGT source polysilicon filling according to any one of claims 1 to 9.
Citation Information
Cited By
Semiconductor device and manufacturing method
CN121310570A