Method for preparing silicon-copper composite nanowire negative electrode material by utilizing photovoltaic silicon cutting waste

By using photovoltaic silicon cutting waste in lithium batteries for metal-assisted chemical etching and improved molten salt electrolysis, the silicon-copper composite nanowire structure is formed, which solves the problems of poor conductivity and unstable electrochemical performance of silicon negative electrode materials, and improves the The performance and life of lithium-ion batteries and reduce production costs and environmental pollution.

CN118969994AActive Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411031805.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The poor conductivity of silicon negative electrode materials in existing lithium batteries, their own volume expansion and unstable electrochemical performance, resulting in low charge and discharge efficiency and short life of lithium-ion batteries.

Method used

Photovoltaic silicon cutting waste is used to introduce nano-scale copper particles through metal-assisted chemical etching, and combined with the improved molten salt electrolysis method, a silicon-copper composite nanowire structure is formed to achieve structural modification of the silicon material and uniformity of the electrolytic process.

Benefits of technology

It significantly improves the conductivity and electrochemical performance of lithium-ion batteries, alleviates the volume expansion problem of lithium-ion batteries during charging and discharging, extends battery life, and reduces production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969994A_ABST
    Figure CN118969994A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a silicon-copper composite nanowire negative electrode material from photovoltaic silicon cutting waste, and belongs to the technical field of silicon waste resource recycling. The preparation method comprises the following steps: carrying out two-step metal-assisted chemical etching on a silicon material through copper salt to uniformly introduce nano-micron copper particles into the silicon material, carrying out controllable oxidation on an etching product, and carrying out tabletting sintering to form an electrolytic precursor; the upper surface and the lower surface of the electrolytic precursor are attached to a sheet-shaped current collector and placed on a hook-shaped cathode current collector for two-step constant-current molten salt electrolysis, electrolytic reduction is carried out with low current density to achieve reduction of copper oxide and silicon oxide, side reaction is avoided, and the silicon-copper composite nanowire negative electrode material is obtained. The silicon-copper composite nanowire negative electrode material not only has a smaller diameter and a larger length-diameter ratio, but also remarkably improves the conductivity and the surface area, and is beneficial to forming a stable solid electrolyte membrane layer in the lithium de-intercalation process of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a silicon-copper composite nanowire negative electrode material by utilizing photovoltaic silicon cutting waste, and belongs to the technical field of silicon waste resource recycling. Background Art

[0002] With the booming development of the photovoltaic industry, the demand for silicon wafers in solar photovoltaic panels has increased year by year. However, silicon wafers are obtained by wire cutting of silicon ingots, and 30-40% silicon debris (silicon waste) will be generated during the wire cutting process. Silicon waste has a flaky structure, a low impurity content and its surface is very easily oxidized to form an oxide layer.

[0003] With the rapid development of the energy storage industry, the commercially available graphite-based lithium battery negative electrode materials have low theoretical specific capacity (372 mAhg -1 ) has gradually failed to meet people's demand for long-lasting and long-life lithium batteries. Silicon materials have a high theoretical specific capacity (4200mAhg -1 ), the lithium insertion potential is low. However, during the charge and discharge process, the silicon negative electrode will expand its own volume (about 300%) due to the deintercalation of lithium, which can easily cause the breakage and pulverization of the active material, leading to the occurrence of side reactions, and causing the solid electrolyte membrane to rupture and regenerate repeatedly, continuously consuming the limited electrolyte in the lithium battery. In addition, the silicon negative electrode has poor conductivity, which limits the current conduction efficiency of the lithium battery during the charge and discharge process and reduces the battery's rate performance; at the same time, the lithium ion migration rate in the lithium battery with pure silicon as the negative electrode is slow, resulting in an increase in the internal resistance of the battery during the charge and discharge process, affecting the battery's charging speed and capacity retention rate. These problems are the main reasons for the unstable electrochemical performance of silicon negative electrode materials. Therefore, it is very important to find a method to modify the structure of the silicon negative electrode.

[0004] In the prior art, direct molten salt electrolysis reduction of silicon dioxide is prone to incomplete electro-deoxidation, easy to produce impurities and low reduction efficiency. Therefore, in order to improve the efficiency of electro-deoxidation, researchers adopt the method of electrolyzing silicon dioxide by adding metal oxides together, but the batch structure modification of silicon-metal materials prepared by this method is incomplete, and it is easy to form metal impurities with larger particle size, which is easy to reduce the charge and discharge capacity of lithium-ion batteries; researchers also plate metal oxides on the surface of silicon dioxide through a series of complex reactions. This method has a long operation process and is not conducive to industrial production. At the same time, the existing electrolysis equipment generally only conducts the precursor along a single horizontal or vertical direction. In this way, as the electrolysis process proceeds, when silicon dioxide is reduced to silicon, the poor conductivity of silicon easily causes the current conduction efficiency of the precursor to be low, thereby reducing the driving force of electrolytic reduction, greatly reducing the rate of electro-deoxidation, resulting in the inability to completely electrolyze part of the silicon dioxide, and easily introducing side reactions, resulting in impure electrolysis products. Using molten salt electrolytic silicon with impure electrolysis products as silicon negative electrode material has the problems of poor conductivity, volume expansion during lithium insertion and extraction, and poor electrochemical performance of silicon negative electrode material. Summary of the invention

[0005] In view of the fact that the silicon reduced by molten salt electrolysis is impure and used as silicon negative electrode material, it has poor conductivity, its own volume expansion during lithium insertion and extraction, and poor electrochemical performance of silicon negative electrode materials. The present invention proposes a method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste. The present invention adopts a metal-assisted chemical etching method to introduce nano-micron structure copper particles into the silicon material, and after controllably oxidizing it, the precursor is subjected to two-step constant current electrolysis in the axial and radial directions through an improved molten salt electrolysis device. Because the precursor and the current collector are in uniform contact, the current density passing through the precursor during the molten salt electrolysis process is relatively uniform, and the constant current electrolysis can accurately control the rate of the electrolysis reaction, so that the electric deoxidation reaction is carried out more uniformly, reducing the occurrence of side reactions during the electrolysis process. During the electrolysis process, copper oxide and silicon oxide are continuously reduced to copper and silicon. The reduced copper enhances the conductivity of the electrolysis precursor, promotes the nucleation process of silicon, and generates silicon-copper alloy nanowires, thereby improving the lithium ion transmission rate of lithium-ion batteries during the charging and discharging process. The silicon-copper composite nanowire negative electrode material of the present invention can greatly improve the conductivity of the silicon negative electrode material during the lithium insertion and extraction process of a lithium ion battery, alleviate its own volume expansion, and fully improve the electrochemical performance of the silicon negative electrode.

[0006] The present invention performs two-step metal-assisted chemical etching on silicon material through copper salt, so that nanometer-micrometer-level copper particles are uniformly introduced into the silicon material, and the etching product is controllably oxidized and then pressed and sintered to form an electrolytic precursor; the upper and lower surfaces of the electrolytic precursor are bonded to a sheet-like current collector and placed on a hook-shaped cathode current collector to perform two-step constant-current molten salt electrolysis, and electrolytic reduction is performed at a relatively low current density to achieve reduction of copper oxide and silicon oxide, thereby avoiding the occurrence of side reactions, and obtaining a silicon-copper composite nanowire negative electrode material.

[0007] A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0008] (1) adding photovoltaic silicon cutting waste to a copper salt solution and mixing evenly, adding a reducing agent, and performing reduction chemical deposition, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste;

[0009] (2) adding the silicon waste material deposited with copper nanoparticles into an etchant for metal-assisted chemical etching so that the nanometer-scale copper particles are uniformly introduced into the silicon waste material to obtain a nanometer-scale copper / silicon composite; the etchant is HF-oxidant-organic solvent;

[0010] (3) placing the nano-micron copper / silicon composite in an air atmosphere for controllable oxidation treatment to obtain a controllable oxidation product, mixing the controllable oxidation product, a binder and a pore-forming agent, and pressing the tablets, and sintering under a protective atmosphere to obtain a molten salt electrolysis precursor;

[0011] (4) The upper and lower surfaces of the molten salt electrolysis precursor are bonded to the sheet current collector and then suspended on a hook-shaped cathode current collector as the cathode. A graphite crucible is used as the anode. Metal halide molten salt is added to the graphite crucible. A first constant current molten salt electrolysis reduction and a second constant current molten salt electrolysis reduction are performed in sequence under a protective atmosphere to obtain a silicon-copper composite nanowire negative electrode material.

[0012] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent and a binder. Based on the mass of the lithium battery silicon negative electrode material as 100 parts, the silicon-copper composite nanowire negative electrode material accounts for 60 to 80 parts, the conductive agent accounts for 10 to 20 parts, and the binder accounts for 10 to 20 parts. Preferably, the conductive agent is acetylene black, graphene, conductive carbon black, polyaniline, polypyrrole or carbon nanotubes; the binder is polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), sodium alginate, polyacrylic acid (PAA), polyethyleneimine (PEI) or polyetheretherketone (PEEK).

[0013] The present invention adopts molten salt electrolysis to structurally modify silicon material by controlled oxidation two-step copper-assisted chemical etching, and finally successfully modifies the flaky morphology of silicon waste into a silicon-copper nanowire composite structure, effectively improving the electrochemical performance of silicon negative electrode materials during the charge and discharge cycle of lithium-ion batteries.

[0014] The beneficial effects of the present invention are:

[0015] (1) The present invention transforms the sheet structure of silicon waste into a silicon-copper composite nanowire structure without generating any by-products. The silicon-copper composite nanowire structure greatly alleviates the problem of spontaneous volume expansion of sheet silicon waste during charging and discharging, thereby improving the electrochemical performance of lithium batteries.

[0016] (2) The present invention ingeniously introduces metallic copper to achieve uniform etching of the porous structure on the surface of the silicon waste and embedding the metallic copper into the interior of the silicon waste. After the etched silicon material is controllably oxidized, the copper oxide is uniformly distributed inside the silicon oxide material. During molten salt electrolysis, the copper oxide inside the silicon waste is first reduced to nano-micron structure copper, which in turn promotes the nucleation of the reduced silicon. After reaching a certain precipitation point, silicon-copper alloy nanowires with a small diameter and a large aspect ratio grow, which are helpful to form a stable solid electrolyte film layer during the lithium-ion battery lithium-ion battery deintercalation process, avoid repeated consumption of lithium ions and improve the conductivity of the lithium-ion battery cycle process, thereby improving the rate performance of the lithium battery; accelerating the migration rate of lithium ions during the lithium-ion battery deintercalation process, reducing the charge transfer resistance, thereby extending the life of the lithium battery and enhancing the safety of the use process; at the same time, the generated copper enhances the conductivity of the electrolytic precursor, ensuring that the precursor is completely electrolyzed during the electrolysis process;

[0017] (3) The present invention makes use of the flaky structure of silicon waste to reduce the accumulation of silicon waste and its pollution to the environment. By recycling silicon waste, the demand for new silicon materials can be reduced, resources can be saved, and production costs can be reduced. The constant current electrolysis is used to obtain silicon-copper alloy nanowires with high purity, which significantly improves the conductivity and surface area of ​​the material and effectively alleviates the volume expansion phenomenon of the material. In addition, the preparation process of silicon-copper alloy nanowires of the present invention is short and the energy consumption is low, which makes it easier to achieve continuous low-cost large-scale industrial production.

[0018] (4) In the present invention, during the molten salt electrolysis process, the precursor is placed on a hook-shaped current collector with a sheet-shaped current collector attached thereto; the design of the sheet-shaped current collector can maintain a uniform distribution of current in the electrolytic precursor during the electrolysis process, improve the electrolysis efficiency, and help form uniform silicon-copper composite nanowires. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of molten salt electrolysis of the present invention; wherein, 1-anode, 2-stainless steel rod, 3-cathode current collector, 4-molten salt, 5-electrolysis precursor; 6-sheet cathode current collector;

[0020] Figure 2 This is a SEM image of the powdered waste silicon powder in Example 1;

[0021] Figure 3 This is a mechanism diagram of metal-assisted chemical etching in Example 1;

[0022] Figure 4 This is a SEM image of the nano-micron copper / silicon composite obtained by metal-assisted chemical etching in Example 1;

[0023] Figure 5 is the XRD pattern of the controlled oxidation product and the silicon-copper composite nanowire in Example 1;

[0024] Figure 6 is a SEM image of the silicon-copper composite nanowires in Example 1;

[0025] Figure 7 This is a test diagram of the cycle performance of the lithium battery negative electrode prepared with the silicon-copper composite nanowire structure of Example 1 and the lithium battery negative electrode of Comparative Example 1. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0027] Summary of the Invention

[0028] A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0029] (1) adding photovoltaic silicon cutting waste to a copper salt solution and mixing evenly, adding a reducing agent, and performing reduction chemical deposition, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste;

[0030] (2) adding the silicon waste material deposited with copper nanoparticles into an etchant for metal-assisted chemical etching so that the nanometer-scale copper particles are uniformly introduced into the silicon waste material to obtain a nanometer-scale copper / silicon composite; the etchant is HF-oxidant-organic solvent;

[0031] (3) placing the nano-micron copper / silicon composite in an air atmosphere for controllable oxidation treatment to obtain a controllable oxidation product, mixing the controllable oxidation product, a binder and a pore-forming agent, and pressing the tablets, and sintering under a protective atmosphere to obtain a molten salt electrolysis precursor;

[0032] (4) The upper and lower surfaces of the molten salt electrolysis precursor are bonded to the sheet current collector and then suspended on a hook-shaped cathode current collector as a cathode, a graphite crucible is used as an anode, a metal halide molten salt is added to the graphite crucible, and a first constant current molten salt electrolysis reduction and a second constant current molten salt electrolysis reduction are sequentially performed under a protective atmosphere to obtain a silicon-copper composite nanowire negative electrode material;

[0033] Preferably, the particle size of the photovoltaic silicon cutting waste in step (1) is 0.5 to 10 μm. Controlling the particle size of the photovoltaic silicon cutting waste can increase the specific surface area of ​​the silicon material, facilitate the subsequent copper-assisted chemical etching reaction and electrolysis process, and improve the performance of the final product;

[0034] Preferably, the copper salt in step (1) is one or more of Cu(NO3)2, CuCl2, CuSO4, Cu(C2H3O2)2, CuO, Cu(OH)2, CuCO3, Cu(CN)2, and CuF2, and the copper salt solution contains Cu 2+ The concentration is 0.005-1 mol / L; the reducing agent is one or more of HF, sodium borohydride, ascorbic acid, hydrazine, and formaldehyde, and the added molar amount of the reducing agent is Cu 2+ 1 to 60 times;

[0035] Preferably, the oxidant in the etchant in step (2) is one or more of H2O2, HClO3, KMnO4, HNO3, Br2, concentrated H2SO4, C2H4O3, the organic solvent is one or more of acetone, methanol, ethanol, tetrahydrofuran, benzene, the reducing agent concentration is 0.1 to 22 mol / L, and the oxidant concentration is 0.1 to 5 mol / L;

[0036] Preferably, the temperature of the metal-assisted chemical etching in step (2) is 15 to 80° C., and the time is 1 to 400 min;

[0037] Preferably, the temperature of the controlled oxidation treatment in step (3) is 300-1000° C., and the time is 2-10 hours; the mass ratio of the controlled oxidation product, the binder and the pore-forming agent is 100:20-50:10-50; the tableting pressure is 5-30 MPa, and the holding time is 1-10 minutes; the sintering temperature is 300-800° C., and the time is 2-5 hours;

[0038] Preferably, the binder in step (3) is one or more of epoxy resin, silicone, starch, chitosan, polyamide, acrylate, phenolic resin, polyimide, polyvinyl alcohol, polyvinyl butyral, the pore-forming agent is one or more of halogen salt, NH4NO3, (NH4)2SO4, (NH4)2CO3, NH4HCO3; the protective atmosphere is nitrogen, argon or helium;

[0039] Preferably, the sheet current collector in step (4) is platinum, tungsten, molybdenum or zirconium, the hook-shaped cathode current collector is a platinum hook, tungsten hook, molybdenum hook or zirconium hook corresponding to the sheet current collector, the metal halide molten salt is NaCl-CaCl2 molten salt, NaCl-KCl-MgCl2 molten salt, CaF2-NaF-MgF2 molten salt, NaCl-CaCl2-LiF molten salt, NaCl-CaCl2-LiCl molten salt, KCl-CaCl2 molten salt, NaCl-KCl molten salt, NaCl-CaCl2-CaF2 molten salt, NaCl molten salt, CaCl2 molten salt, CaCl2-KCl-MgCl2 molten salt, LiF-BeF2 molten salt or NaF-ZrF4 molten salt, and the protective atmosphere is nitrogen, argon or helium;

[0040] Preferably, the temperature of the first constant current molten salt electrolytic reduction in step (4) is 700-1000° C., the current is 0.5-3A, and the time is 1-6h;

[0041] Preferably, the temperature of the second constant current molten salt electrolytic reduction in step (4) is 700-1000° C., the current of the second constant current molten salt electrolytic reduction is 0.3-0.5A lower than the current of the first constant current molten salt electrolytic reduction, and the time is 1-6h;

[0042] In the present invention, the cathode system of molten salt electrolysis is improved, a sheet current collector in good contact with the precursor is added to the cathode hook current collector, and it is ensured that the electrolysis precursor, the hook cathode current collector, and the sheet current collector are in good contact. When electrolysis is carried out under an inert atmosphere, a DC power supply is introduced, and a part of the electrons are transmitted to the sheet cathode current collector, and the other part of the electrons are transmitted to the hook cathode current collector; at this time, the surface of the precursor in contact with the sheet current collector obtains electrons and begins to be reduced. Secondly, because the electrons transmitted through the surface of the cathode hook current collector are in contact with the center position inside the precursor, the center position of the precursor also begins to be electrolytically reduced from the radial direction. Thereafter, the electrolytic reduction reaction reacts simultaneously from the center position of the precursor to the radial direction and the axial direction in contact with the sheet current collector, so the electro-deoxidation is sufficient and the reduction rate is fast. The current in this process is constant and the introduction of the sheet current collector can ensure the uniformity of the current density of the electrolytic precursor during the electrolysis process, avoid the occurrence of side reactions, and ensure the introduction of no electrolysis by-products. In addition, in the silicon material after the two-step copper-assisted chemical etching with controlled oxidation, the theoretical decomposition voltage of copper oxide is lower than that of silicon waste after controlled oxidation. Therefore, at the beginning of electrolysis, the copper oxide in the precursor is first reduced by electrons to form copper. The generation of copper increases the conductivity of the precursor. Combined with the excellent electrical deoxidation characteristics of the precursor in the axial and radial directions, the electrical deoxidation effect of the precursor is more sufficient and the electrolysis efficiency is higher. The oxygen ions separated from the precursor can easily combine with the anode graphite crucible through the molten salt to form CO or CO2 overflowing from the surface of the molten salt, avoiding the generation of carbonate impurities. After etching and oxidation of the silicon material assisted by the copper salt two-step method, nano-particle copper is successfully introduced into the silicon waste. After controlled oxidation, copper and silicon are oxidized respectively. At the beginning of electrolysis, the copper oxide inside the pores of the controllably oxidized silicon material is first reduced to copper. As the electrolysis proceeds, the controllably oxidized silicon material gradually reduces to silicon by gaining electrons. At this time, the nano-micron copper particles promote the nucleation of the reduced silicon inside the oxidized silicon material. When the reduced silicon reaches a certain concentration, it catalyzes the growth of silicon-copper alloy nanowires. Because the copper particles introduced by metal-assisted chemical etching are small in size, silicon-copper alloy nanowires with a small diameter and a high aspect ratio are grown under the catalytic action of copper, which facilitates the formation of a stable solid electrolyte membrane in the process of lithium-ion battery deintercalation and extraction, fully alleviates the volume expansion phenomenon of lithium-ion battery during charging and discharging, and is conducive to improving the electrochemical performance of lithium-ion battery.

[0043] Conventional molten salt electrolysis uses SiO2 powder as an electrolysis precursor, and the introduced metal oxide generally adheres to the surface of the SiO2 powder, causing the oxygen ions released by electrolysis to easily combine with SiO2 and molten salt to form silicate impurities, resulting in impure electrolysis products and affecting the electrochemical performance of lithium batteries. Compared with conventional SiO2 electrolysis, the present invention etches silicon waste with copper salt and uniformly introduces metal copper particles into the silicon material. After the silicon material etched by copper salt is controllably oxidized, the electrolysis device of the present invention is used to simultaneously cause the electrolysis precursor to undergo an electro-deoxidation reduction reaction in the radial and axial directions, which helps to accelerate the electro-deoxidation rate, reduce the electrolysis time, achieve energy saving, and realize the purpose of batch preparation of silicon-copper alloy nanowires.

[0044] Example 1: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0045] (1) Add vacuum-dried photovoltaic silicon cutting waste (particle size of 0.5 to 6 μm) to a 0.2 mol / L Cu(NO3)2 solution and mix evenly, add a reducing agent (HF solution with a concentration of 20 mol / L), and perform reduction chemical deposition for 60 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, separate the solid and the liquid, wash the solid with deionized water, and vacuum dry; the molar amount of the reducing agent (HF) added is Cu in the Cu(NO3)2 solution 2+ 20 times;

[0046] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-H2O2-anhydrous ethanol), performing metal-assisted chemical etching at a temperature of 25° C. for 60 min to uniformly introduce the nano-micron-sized copper particles into the silicon waste material, performing solid-liquid separation, washing the solid with deionized water, and vacuum drying to obtain a nano-micron-sized copper / silicon composite; the HF concentration in the etchant is 4.5 mol / L, and the H2O2 concentration is 0.5 mol / L;

[0047] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 900°C for 5 hours to obtain a controllable oxidation product, the controllable oxidation product, a binder (polyvinyl alcohol) and a pore-forming agent (ammonium bicarbonate) are mixed and pressed into a sheet at a pressure of 15 MPa for 3 minutes, and then placed in an argon atmosphere (argon flow rate of 15 mL / min) and sintered at a temperature of 600°C for 3 hours to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controllable oxidation product, the binder (polyvinyl alcohol) and the pore-forming agent (ammonium bicarbonate) is 100:30:30;

[0048] (4) Figure 1As shown in the figure, the upper and lower surfaces of the molten salt electrolysis precursor are attached to the molybdenum sheet current collector and then suspended on the molybdenum hook cathode current collector (the electrolysis precursor, the molybdenum hook current collector, and the molybdenum sheet current collector are in good contact), and a graphite crucible is used as the anode. NaCl-CaCl2 molten salt (the molar ratio of NaCl and CaCl2 is 4:6) is added to the graphite crucible, and the first constant current molten salt electrolysis reduction and the second constant current molten salt electrolysis reduction are carried out in sequence under an argon atmosphere (argon flow rate is 20 mL / min), and the cathode current collector is taken from the molten salt. The electrolysis product was washed with deionized water, and then pickled with HCl-HF mixed acid solution (HCl concentration was 0.5 mol / L, HF concentration was 0.5 mol / L) for 2 h to obtain a silicon-copper composite nanowire negative electrode material; the first constant current molten salt electrolysis reduction temperature was 700 ° C, the current was 1.5 A, and the time was 2 h; the second constant current molten salt electrolysis reduction temperature was 700 ° C, the current was 1.1 A, and the time was 2 h;

[0049] The SEM image of photovoltaic silicon cutting waste in this embodiment is shown in Figure 2 ,from Figure 2 It can be seen that photovoltaic silicon cutting waste exists in the form of irregular nano-micron flake structures, and the distribution between the flake structures is relatively loose and there are significant gaps. This structure facilitates further etching in the solution.

[0050] The mechanism diagram of copper-assisted chemical etching in this embodiment is shown in Figure 3 , Figure 3 The left side of the figure shows the process of copper deposition on the surface of silicon waste. When the HF solution comes into contact with the silicon waste, the HF solution first dissolves the natural oxide layer on the surface of the silicon waste, then exposes the pure silicon on the surface. Finally, the HF solution oxidizes some silicon atoms on the surface of the silicon waste into tetravalent silicon ions and releases electrons. These electrons react with the Cu in the solution. 2+ The combination reduces it to nano-micron copper particles and attaches them to the surface of silicon waste; Figure 3 The middle right side shows the process of nano-micron copper particles etching into the silicon waste. Under the catalytic effect of nano-micron copper particles, hydrogen peroxide as an oxidant will accelerate the oxidation reaction to quickly form silicon dioxide on the surface of the silicon waste. At the same time, due to the presence of HF, the SiO2 generated on the surface of the silicon waste is quickly dissolved in the etchant, so that the nano-micron copper particles are gradually etched into the interior of the silicon waste.

[0051] The SEM image of the nano-micron copper / silicon composite obtained by copper-assisted chemical etching in this embodiment is shown in Figure 4 ,from Figure 4 It can be seen that after the two-step copper-assisted chemical etching, a uniform porous structure appeared on the surface of the silicon waste, indicating that the nano-micron copper particles were uniformly etched into the interior of the silicon waste;

[0052] The XRD patterns of the controlled oxidation products and silicon-copper composite nanowires in this example are shown in Figure 5 ,from Figure 5 It can be seen that after the silicon waste is subjected to two-step copper-assisted chemical etching and high-temperature oxidation pretreatment, the crystal peak of the silicon waste is converted into an amorphous peak of silicon oxide, indicating that most of the etched silicon material is oxidized. At the same time, the appearance of the copper oxide crystal peak also indicates that the copper is successfully oxidized. After the precursor is electrolyzed in two steps with a constant current using an improved molten salt electrolysis device, it is found that the amorphous silicon oxide peak disappears and the crystalline silicon peak reappears. In addition, the copper oxide peak also disappears and the copper-silicon alloy peak appears. No other miscellaneous peaks appear in this process, indicating that this electrolysis method has fewer side reactions.

[0053] The SEM image of the silicon-copper composite nanowires in this embodiment is shown in Figure 6 ,contrast Figure 2 and Figure 6 It can be seen that the method of this embodiment successfully converts waste silicon powder with flake structure into nanowire structure in batches;

[0054] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (conductive carbon black) and a binder (sodium alginate), and the mass of the lithium battery silicon negative electrode material is 100 parts, the silicon-copper composite nanowire negative electrode material accounts for 60 parts, the conductive agent (conductive carbon black) accounts for 20 parts, and the binder (sodium alginate) accounts for 20 parts;

[0055] In the glove box, the lithium battery silicon negative electrode material and lithium sheet (counter electrode) were assembled into a half-cell and charged and discharged at a current density of 500mA / g. The cycle performance of the lithium battery silicon negative electrode material was as follows: Figure 7 As shown, the first discharge specific capacity of the lithium battery silicon negative electrode material is 2206.8 mAh / g, the first coulomb efficiency can reach 85.6%, and the reversible specific capacity after 300 cycles is 930.4 mAh / g.

[0056] Comparative Example 1: The photovoltaic silicon cutting waste (particle size of 0.5-6 μm) vacuum-dried in Example 1 is directly used to prepare the lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of photovoltaic silicon cutting waste, a conductive agent (conductive carbon black) and a binder (sodium alginate), and the mass of the lithium battery silicon negative electrode material is 100 parts, the photovoltaic silicon cutting waste accounts for 60 parts, the conductive agent (conductive carbon black) accounts for 20 parts, and the binder (sodium alginate) accounts for 20 parts;

[0057] In the glove box, the lithium battery silicon negative electrode material and lithium sheet (counter electrode) were assembled into a half-cell and charged and discharged at a current density of 500mA / g. The cycle performance of the lithium battery silicon negative electrode material was as follows: Figure 7As shown, the first discharge specific capacity of the silicon negative electrode material of the lithium battery in this comparative example is 2732.1 mAh / g, the first coulombic efficiency can reach 75.5%, and the reversible specific capacity after 300 cycles is only 280.1 mAh / g; while the reversible specific capacity of Example 1 after 300 cycles is 650.3 mAh / g higher than that of the comparative example, so the long cycle performance of Example 1 is much greater than the long cycle performance of waste silicon powder (flake).

[0058] Example 2: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0059] (1) Add vacuum-dried photovoltaic silicon cutting waste (particle size of 1 to 3 μm) to a 0.3 mol / L CuSO4 solution and mix well, add a reducing agent (sodium borohydride solution with a concentration of 3 mol / L), and perform reduction chemical deposition for 90 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, separate the solid and the liquid, wash the solid with deionized water, and vacuum dry; the molar amount of the reducing agent (sodium borohydride) added is 1:100 of the Cu in the CuSO4 solution. 2+ 25 times of

[0060] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-HNO3-acetone), performing metal-assisted chemical etching at a temperature of 30°C for 120 min to uniformly introduce the nano-micron-sized copper particles into the silicon waste material, performing solid-liquid separation, washing the solid with deionized water, and vacuum drying to obtain a nano-micron-sized copper / silicon composite; the HF concentration in the etchant is 5.0 mol / L, and the HNO3 concentration is 1.0 mol / L;

[0061] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 800°C for 6 hours to obtain a controllable oxidation product, the controllable oxidation product, a binder (polyvinyl butyral) and a pore-forming agent (ammonium chloride) are mixed and pressed at a pressure of 18 MPa for 4 minutes, and then placed in a nitrogen atmosphere (nitrogen flow rate of 20 mL / min) and sintered at a temperature of 650°C for 3.5 hours to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controlled oxidation product, the binder (polyvinyl butyral) and the pore-forming agent (ammonium chloride) is 100:35:25;

[0062] (4) Figure 1As shown, the upper and lower surfaces of the molten salt electrolysis precursor are attached to the tungsten sheet current collector and then suspended on the tungsten hook cathode current collector (the electrolysis precursor, the tungsten hook current collector, and the tungsten sheet current collector are in good contact), and a graphite crucible is used as the anode. NaCl-KCl-MgCl2 molten salt (the molar ratio of NaCl, KCl and MgCl2 is 5:3:2) is added into the graphite crucible, and the first constant current molten salt electrolysis reduction and the second constant current molten salt electrolysis reduction are carried out in sequence under a nitrogen atmosphere (nitrogen flow rate is 25 mL / min), and the cathode current collector is reduced from The electrolytic product was taken out from the molten salt, cooled naturally to room temperature under a nitrogen atmosphere, and the electrolysis product was washed with deionized water, and then pickled with an HCl-HF mixed acid solution (the HCl concentration in the HCl-HF mixed acid solution was 1 mol / L and the HF concentration was 0.5 mol / L) for 1 h to obtain a silicon-copper composite nanowire negative electrode material; the first constant current molten salt electrolysis reduction temperature was 800° C., the current was 1.8 A, and the time was 1.5 h; the second constant current molten salt electrolysis reduction temperature was 800° C., the current was 1.5 A, and the time was 2.5 h;

[0063] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (conductive carbon black) and a binder (sodium alginate), and the mass of the lithium battery silicon negative electrode material is 100 parts, the silicon-copper composite nanowire negative electrode material accounts for 60 parts, the conductive agent (conductive carbon black) accounts for 20 parts, and the binder (sodium alginate) accounts for 20 parts;

[0064] In a glove box, lithium battery silicon negative electrode material and lithium sheet (counter electrode) were assembled into a half-cell and charged and discharged at a current density of 500mA / g. The first discharge specific capacity of the lithium battery silicon negative electrode material was 2160.5mAh / g, the first coulombic efficiency could reach 83.60%, and the reversible specific capacity after 300 cycles was 980.6mAh / g.

[0065] Example 3: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0066] (1) Add vacuum-dried photovoltaic silicon cutting waste (particle size of 1 to 5 μm) to a 0.25 mol / L CuCl2 solution and mix well, add a reducing agent (a 13 mol / L formaldehyde solution), and perform reduction chemical deposition for 90 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, separate the solid and the liquid, wash the solid with deionized water, and vacuum dry; the molar amount of the reducing agent (formaldehyde solution) added is 1:100 of the Cu in the CuCl2 solution. 2+ 15 times of

[0067] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-H2O2-anhydrous ethanol), performing metal-assisted chemical etching at a temperature of 40° C. for 90 min to uniformly introduce the nano-micron-sized copper particles into the silicon waste material, performing solid-liquid separation, washing the solid with deionized water, and vacuum drying to obtain a nano-micron-sized copper / silicon composite; the HF concentration in the etchant is 6 mol / L, and the H2O2 concentration is 1.5 mol / L;

[0068] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 850° C. for 5 h to obtain a controllable oxidation product, the controllable oxidation product, a binder (phenolic resin) and a pore-forming agent (ammonium sulfate) are mixed and pressed into a sheet at a pressure of 20 MPa for 3 min, and then placed in an argon atmosphere (argon flow rate of 25 mL / min) and sintered at a temperature of 750° C. for 4 h to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controlled oxidation product, the binder (phenolic resin) and the pore-forming agent (ammonium sulfate) is 100:40:30;

[0069] (4) Figure 1 As shown in the figure, the upper and lower surfaces of the molten salt electrolysis precursor are attached to the platinum sheet current collector and then suspended on the platinum hook cathode current collector (the electrolysis precursor, the platinum hook current collector and the platinum sheet current collector have good contact), a graphite crucible is used as the anode, NaCl-CaCl2-CaF2 molten salt (the molar ratio of NaCl, CaCl2 and CaF2 is 6:3:1) is added into the graphite crucible, and the first constant current molten salt electrolysis reduction and the second constant current molten salt electrolysis reduction are carried out in sequence under an argon atmosphere (argon flow rate is 30 mL / min), and the cathode collector The fluid is taken out from the molten salt and naturally cooled to room temperature under an argon atmosphere. The electrolysis product is washed with deionized water and then pickled with an HCl-HF mixed acid solution (the HCl concentration in the HCl-HF mixed acid solution is 1.5 mol / L and the HF concentration is 0.5 mol / L) for 2 hours to obtain a silicon-copper composite nanowire negative electrode material; the first constant current molten salt electrolysis reduction temperature is 850°C, the current is 1.5A, and the time is 2 hours; the second constant current molten salt electrolysis reduction temperature is 800°C, the current is 1A, and the time is 2 hours;

[0070] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (graphene) and a binder (sodium alginate), and the mass of the lithium battery silicon negative electrode material is 100 parts, the silicon-copper composite nanowire negative electrode material accounts for 70 parts, the conductive agent (graphene) accounts for 15 parts, and the binder (sodium alginate) accounts for 15 parts;

[0071] In a glove box, lithium battery silicon negative electrode material and lithium sheet (counter electrode) were assembled into a half-cell and charged and discharged at a current density of 500mA / g. The first discharge specific capacity of the lithium battery silicon negative electrode material was 2463.6mAh / g, the first coulombic efficiency could reach 84.86%, and the reversible specific capacity after 300 cycles was 1056.3mAh / g.

[0072] Example 4: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0073] (1) Adding vacuum-dried photovoltaic silicon cutting waste (particle size of 0.5 to 7 μm) to a 0.4 mol / L Cu(C2H3O2)2 solution and mixing evenly, adding a reducing agent (a 10 mol / L hydrazine solution) and performing reduction chemical deposition for 150 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, and then separating the solid from the liquid, washing the solid with deionized water, and vacuum drying; the molar amount of the reducing agent (hydrazine solution) is 1:100 of the Cu in the Cu(C2H3O2)2 solution. 2+ 30 times;

[0074] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-KMnO4-tetrahydrofuran), performing metal-assisted chemical etching at a temperature of 50° C. for 120 min to uniformly introduce the nano-micron copper particles into the silicon waste material, performing solid-liquid separation, washing the solid with deionized water, and vacuum drying to obtain a nano-micron copper / silicon composite; the HF concentration in the etchant is 6.5 mol / L, and the KMnO4 concentration is 2 mol / L;

[0075] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 900°C for 6 hours to obtain a controllable oxidation product, the controllable oxidation product, a binder (chitosan) and a pore-forming agent (ammonium nitrate) are mixed and pressed into a sheet at a pressure of 23 MPa for 5 minutes, and then placed in a helium atmosphere (helium flow rate of 20 mL / min) and sintered at a temperature of 700°C for 3 hours to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controllable oxidation product, the binder (chitosan) and the pore-forming agent (ammonium nitrate) is 100:35:30;

[0076] (4) Figure 1As shown, the upper and lower surfaces of the molten salt electrolysis precursor are attached to the zirconium sheet current collector and then suspended on the zirconium hook cathode current collector (the electrolysis precursor, the zirconium hook current collector, and the zirconium sheet current collector are in good contact), and a graphite crucible is used as the anode. NaCl-CaCl2-LiF molten salt (the molar ratio of NaCl, CaCl2 and LiF is 5:4:1) is added to the graphite crucible, and the first constant current molten salt electrolysis reduction and the second constant current molten salt electrolysis reduction are carried out in sequence under a helium atmosphere (helium flow rate is 25 mL / min), and the cathode current collector is reduced from the molten salt to the cathode current collector. The electrolytic product was taken out, cooled naturally to room temperature under an argon atmosphere, and washed with deionized water, and then pickled with a H2SO4-HF mixed acid solution (the H2SO4 concentration in the H2SO4-HF mixed acid solution was 1 mol / L and the HF concentration was 0.5 mol / L) for 1 h to obtain a silicon-copper composite nanowire negative electrode material; the first constant current molten salt electrolysis reduction temperature was 750°C, the current was 1.6A, and the time was 1.5h; the second constant current molten salt electrolysis reduction temperature was 800°C, the current was 1.2A, and the time was 3h;

[0077] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (carbon nanotubes) and a binder (carboxymethyl cellulose), and based on 100 parts of the lithium battery silicon negative electrode material, the silicon-copper composite nanowire negative electrode material accounts for 70 parts, the conductive agent (carbon nanotubes) accounts for 15 parts, and the binder (carboxymethyl cellulose) accounts for 15 parts;

[0078] In a glove box, lithium battery silicon negative electrode material and lithium sheet (counter electrode) were assembled into a half-cell and charged and discharged at a current density of 500mA / g. The first discharge specific capacity of the lithium battery silicon negative electrode material was 2362.8mAh / g, the first coulombic efficiency could reach 82.9%, and the reversible specific capacity after 300 cycles was 920.4mAh / g.

[0079] Example 5: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0080] (1) Adding vacuum-dried photovoltaic silicon cutting waste (particle size of 1 to 8 μm) to a 0.5 mol / L Cu(C2H3O2)2 solution and mixing them evenly, adding a reducing agent (3 mol / L ascorbic acid solution) to perform reduction chemical deposition for 180 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, and then separating the solid from the liquid, washing the solid with deionized water, and vacuum drying; the molar amount of the reducing agent (ascorbic acid) added is 1:100 molar mass of Cu in the Cu(C2H3O2)2 solution. 2+ 20 times;

[0081] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-C2H4O3-methanol), performing metal-assisted chemical etching at a temperature of 60° C. for 90 min to uniformly introduce the nano-micron-sized copper particles into the silicon waste material, performing solid-liquid separation, washing the solid with deionized water, and vacuum drying to obtain a nano-micron-sized copper / silicon composite; the HF concentration in the etchant is 7 mol / L, and the C2H4O3 concentration is 2.5 mol / L;

[0082] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 950° C. for 4 h to obtain a controllable oxidation product, the controlled oxidation product, a binder (polyimide) and a pore-forming agent (ammonium carbonate) are mixed and pressed into a sheet at a pressure of 25 MPa for 3 min, and then placed in a nitrogen atmosphere (nitrogen flow rate of 25 mL / min) and sintered at a temperature of 780° C. for 3.5 h to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controlled oxidation product, the binder (polyimide) and the pore-forming agent (ammonium carbonate) is 100:28:32;

[0083] (4) Figure 1 As shown, the upper and lower surfaces of the molten salt electrolysis precursor are attached to the tungsten sheet current collector and then suspended on the tungsten hook cathode current collector (the electrolysis precursor, the tungsten hook current collector, and the tungsten sheet current collector are in good contact), and a graphite crucible is used as the anode. NaCl-CaCl2-LiCl molten salt (the molar ratio of NaCl, CaCl2 and LiCl is 6:3:1) is added to the graphite crucible, and the first constant current molten salt electrolysis reduction and the second constant current molten salt electrolysis reduction are carried out in sequence under an argon atmosphere (argon flow rate is 30 mL / min), and the cathode current collector is The product was taken out from the molten salt, cooled naturally to room temperature under an argon atmosphere, and the electrolysis product was washed with deionized water, and then pickled with a HNO3-HF mixed acid solution (the HNO3 concentration in the HNO3-HF mixed acid solution was 1 mol / L and the HF concentration was 0.6 mol / L) for 2 h to obtain a silicon-copper composite nanowire negative electrode material; the first constant current molten salt electrolysis reduction temperature was 800°C, the current was 1.4A, and the time was 2 h; the second constant current molten salt electrolysis reduction temperature was 850°C, the current was 1.0A, and the time was 2.5 h;

[0084] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (conductive carbon black) and a binder (sodium alginate), and based on 100 parts of the lithium battery silicon negative electrode material, the silicon-copper composite nanowire negative electrode material accounts for 80 parts, the conductive agent (acetylene black) accounts for 10 parts, and the binder (polyacrylic acid) accounts for 10 parts;

[0085] In a glove box, lithium battery silicon negative electrode materials and lithium sheets (counter electrodes) were assembled into half-cells and charged and discharged at a current density of 500mA / g. The first discharge specific capacity of the lithium battery silicon negative electrode material was 2538.7mAh / g, the first coulombic efficiency could reach 83.5%, and the reversible specific capacity after 300 cycles was 908.8mAh / g.

[0086] Example 6: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows: a sodium borohydride solution with a concentration of 3 mol / L

[0087] (1) Adding vacuum-dried photovoltaic silicon cutting waste (particle size of 0.5 to 8.5 μm) to a 0.6 mol / L CuCl2 solution and mixing them evenly, adding a reducing agent (HF solution with a concentration of 15 mol / L and sodium borohydride solution with a concentration of 3 mol / L) to perform reduction chemical deposition for 180 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, and then separating the solid from the liquid, washing the solid with deionized water, and vacuum drying; the molar amounts of the reducing agents (HF and sodium borohydride) added are: Cu in the CuCl2 solution: 2+ 40 times and 20 times;

[0088] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-HClO3-tetrahydrofuran), performing metal-assisted chemical etching at a temperature of 70°C for 180 min to uniformly introduce the nano-micron-sized copper particles into the silicon waste material, performing solid-liquid separation, washing the solid with deionized water, and vacuum drying to obtain a nano-micron-sized copper / silicon composite; the HF concentration in the etchant is 7.5 mol / L, and the HClO3 concentration is 0.5 mol / L;

[0089] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 900°C for 6 hours to obtain a controllable oxidation product, the controllable oxidation product, a binder (acrylate) and a pore-forming agent (LiCl) are mixed and pressed into a sheet at a pressure of 15 MPa for 6 minutes, and then placed in a nitrogen atmosphere (nitrogen flow rate of 35 mL / min) and sintered at a temperature of 680°C for 4 hours to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controlled oxidation product, the binder (acrylate) and the pore-forming agent (LiCl) is 100:30:35;

[0090] (4) Figure 1As shown, the upper and lower surfaces of the molten salt electrolysis precursor are bonded to the zirconium sheet current collector and then suspended on the zirconium hook cathode current collector (the electrolysis precursor, the zirconium hook current collector, and the zirconium sheet current collector are in good contact), a graphite crucible is used as the anode, KCl-CaCl2 molten salt (the molar ratio of KCl and CaCl2 is 4:6) is added to the graphite crucible, and the first constant current molten salt electrolysis reduction and the second constant current molten salt electrolysis reduction are carried out in sequence under a nitrogen atmosphere (nitrogen flow rate is 40 mL / min), the cathode current collector is taken out of the molten salt, and naturally cooled to room temperature under an argon atmosphere. The electrolysis product was washed with deionized water, and then pickled with H2SO4-HCl-HF mixed acid solution (the H2SO4 concentration in the H2SO4-HCl-HF mixed acid solution was 1 mol / L, the HCl concentration was 1 mol / L, and the HF concentration was 0.5 mol / L) for 1.5 h to obtain a silicon-copper composite nanowire negative electrode material; the first constant current molten salt electrolysis reduction temperature was 850°C, the current was 1.3A, and the time was 2 h; the second constant current molten salt electrolysis reduction temperature was 800°C, the current was 0.9A, and the time was 2.5 h;

[0091] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (polypyrrole) and a binder (sodium alginate), and the mass of the lithium battery silicon negative electrode material is 100 parts, the silicon-copper composite nanowire negative electrode material accounts for 80 parts, the conductive agent (conductive carbon black) accounts for 10 parts, and the binder (styrene-butadiene rubber) accounts for 10 parts;

[0092] In a glove box, lithium battery silicon negative electrode material and lithium sheet (counter electrode) were assembled into a half-cell and charged and discharged at a current density of 500mA / g. The first discharge specific capacity of the lithium battery silicon negative electrode material was 2386.7mAh / g, the first coulombic efficiency could reach 84.2%, and the reversible specific capacity after 300 cycles was 890.7mAh / g.

[0093] Example 7: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0094] (1) Adding vacuum-dried photovoltaic silicon cutting waste (particle size of 3 to 9 μm) to a 0.7 mol / L CuSO4 solution and mixing them evenly, adding a reducing agent (HF solution with a concentration of 10 mol / L and hydrazine solution with a concentration of 8 mol / L) to perform reduction chemical deposition for 240 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, and then separating the solid from the liquid, washing the solid with deionized water, and vacuum drying; the molar amounts of the reducing agents (HF and hydrazine) added are: Cu in the CuSO4 solution: 2+ 50 times and 15 times;

[0095] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-HNO3-methanol), performing metal-assisted chemical etching at a temperature of 75°C for 300 min to uniformly introduce the nano-micron-sized copper particles into the silicon waste material, separating the solid from the liquid, washing the solid with deionized water, and vacuum drying to obtain a nano-micron-sized copper / silicon composite; the HF concentration in the etchant is 8 mol / L, and the HNO3 concentration is 0.5 mol / L;

[0096] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 700°C for 7 hours to obtain a controllable oxidation product, the controllable oxidation product, a binder (epoxy resin) and a pore-forming agent (ammonium chloride) are mixed and pressed into a sheet at a pressure of 18 MPa for 6 minutes, and then placed in a helium atmosphere (helium flow rate of 25 mL / min) and sintered at a temperature of 650°C for 3 hours to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controlled oxidation product, the binder (epoxy resin) and the pore-forming agent (ammonium chloride) is 100:35:25;

[0097] (4) Figure 1 As shown in the figure, the upper and lower surfaces of the molten salt electrolysis precursor are attached to the platinum sheet current collector and then suspended on the platinum hook cathode current collector (the electrolysis precursor, platinum hook current collector, and platinum sheet current collector have good contact), and the graphite crucible is used as the anode to mix NaCl-KCl

[0098] Molten salt (NaCl and KCl in a molar ratio of 7:3) was added to a graphite crucible, and a first constant current molten salt electrolytic reduction and a second constant current molten salt electrolytic reduction were performed in sequence under a helium atmosphere (helium flow rate was 30 mL / min), the cathode current collector was taken out of the molten salt, and naturally cooled to room temperature under an argon atmosphere, the electrolysis product was washed with deionized water, and then pickled with an HCl-HF mixed acid solution (HCl concentration in the HCl-HF mixed acid solution was 1.5 mol / L, and HF concentration was 1 mol / L) for 2.5 h to obtain a silicon-copper composite nanowire negative electrode material; the temperature of the first constant current molten salt electrolytic reduction was 800° C., the current was 1.7 A, and the time was 1.5 h; the temperature of the second constant current molten salt electrolytic reduction was 800° C., the current was 1.3 A, and the time was 2 h;

[0099] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (polyaniline) and a binder (polyvinylidene fluoride), and based on 100 parts of the lithium battery silicon negative electrode material, the silicon-copper composite nanowire negative electrode material accounts for 70 parts, the conductive agent (polyaniline) accounts for 15 parts, and the binder (polyvinylidene fluoride) accounts for 15 parts;

[0100] In a glove box, lithium battery silicon negative electrode materials and lithium sheets (counter electrodes) were assembled into half-cells and charged and discharged at a current density of 500mA / g. The first discharge specific capacity of the lithium battery silicon negative electrode material was 2316.4mAh / g, the first coulombic efficiency could reach 82.3%, and the reversible specific capacity after 300 cycles was 916.3mAh / g.

[0101] Example 8: A method for preparing a silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, the specific steps are as follows:

[0102] (1) Adding vacuum-dried photovoltaic silicon cutting waste (particle size of 0.5 to 9.5 μm) to a 0.8 mol / L Cu(NO3)2 solution and mixing them evenly, adding a reducing agent (an HF solution with a concentration of 8 mol / L and an ascorbic acid solution with a concentration of 3 mol / L) to perform reduction chemical deposition for 300 min, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste, and then separating the solid from the liquid, washing the solid with deionized water, and vacuum drying; the molar amounts of the reducing agent (HF and ascorbic acid) added are respectively: Cu in the CuSO4 solution: Cu 2+; Cu 3+; Cu 4+; Cu 5+; Cu 6+; Cu 7+; Cu 8+; Cu 9+; Cu 10+; Cu 11+; Cu 12+; Cu 13+; Cu 14+; Cu 15+; Cu 16+; Cu 17+; Cu 18+; Cu 19+; Cu 20+; Cu 21+; Cu 22+; Cu 23+; Cu 24+; Cu 25+; Cu 26+; Cu 27+; Cu 28+; Cu 29+; Cu 20+; Cu 29+; Cu 20+; Cu 28+; Cu 29+; Cu 28+; Cu 29+; Cu 24+; Cu 26+; Cu 28+; Cu 29 ...9+; Cu 24+; Cu 26+; Cu 28+; Cu 29+; Cu 29+; Cu 2 2+ 55 times and 10 times;

[0103] (2) adding the silicon waste material with copper nanoparticles deposited thereon into an etchant (HF-H2O2-tetrahydrofuran), performing metal-assisted chemical etching at a temperature of 80° C. for 360 min to uniformly introduce the nano-micron-sized copper particles into the silicon waste material, performing solid-liquid separation, washing the solid with deionized water, and vacuum drying to obtain a nano-micron-sized copper / silicon composite; the HF concentration in the etchant is 10 mol / L, and the H2O2 concentration is 1.5 mol / L;

[0104] (3) The nano-micron copper / silicon composite is placed in an air atmosphere and subjected to a controllable oxidation treatment at a temperature of 800°C for 6 hours to obtain a controllable oxidation product, the controllable oxidation product, a binder (acrylate) and a pore-forming agent (ammonium sulfate) are mixed and pressed into a sheet at a pressure of 20 MPa for 3 minutes, and then placed in an argon atmosphere (argon flow rate of 25 mL / min) and sintered at a temperature of 600°C for 4 hours to obtain a circular sheet-shaped molten salt electrolysis precursor; the mass ratio of the controllable oxidation product, the binder (acrylate) and the pore-forming agent (ammonium sulfate) is 100:38:30;

[0105] (4) Figure 1As shown, the upper and lower surfaces of the molten salt electrolysis precursor are bonded to the molybdenum sheet current collector and then suspended on the molybdenum hook cathode current collector (the electrolysis precursor, the molybdenum hook current collector, and the molybdenum sheet current collector are in good contact), a graphite crucible is used as the anode, and a CaCl2-KCl-MgCl2 molten salt (the molar ratio of CaCl2, KCl and MgCl2 is 5:3:2) is added to the graphite crucible, and the first constant current molten salt electrolysis reduction and the second constant current molten salt electrolysis reduction are carried out in sequence under a nitrogen atmosphere (nitrogen flow rate is 35 mL / min), and the cathode current collector is The product was taken out from the molten salt, cooled naturally to room temperature under an argon atmosphere, the electrolysis product was washed with deionized water, and then pickled with an HCl-HF mixed acid solution (the HCl concentration in the HCl-HF mixed acid solution was 1 mol / L and the HF concentration was 0.5 mol / L) for 2 h to obtain a silicon-copper composite nanowire negative electrode material; the first constant current molten salt electrolysis reduction temperature was 850°C, the current was 1.5A, and the time was 1.5 h; the second constant current molten salt electrolysis reduction temperature was 850°C, the current was 1.1A, and the time was 2.5 h;

[0106] The silicon-copper composite nanowire negative electrode material can be used to prepare a lithium battery silicon negative electrode material: the lithium battery silicon negative electrode material is composed of a silicon-copper composite nanowire negative electrode material, a conductive agent (graphene) and a binder (carboxymethyl cellulose), and based on 100 parts of the lithium battery silicon negative electrode material, the silicon-copper composite nanowire negative electrode material accounts for 70 parts, the conductive agent (graphene) accounts for 15 parts, and the binder (carboxymethyl cellulose) accounts for 15 parts;

[0107] In a glove box, lithium battery silicon negative electrode material and lithium sheet (counter electrode) were assembled into a half-cell and charged and discharged at a current density of 500mA / g. The first discharge specific capacity of the lithium battery silicon negative electrode material was 2318.4mAh / g, the first coulombic efficiency could reach 81.4%, and the reversible specific capacity after 300 cycles was 934.6mAh / g.

[0108] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste, characterized in that: The specific steps are as follows: (1) adding photovoltaic silicon cutting waste to a copper salt solution and mixing evenly, adding a reducing agent, and performing reduction chemical deposition, so that the copper ions in the copper salt solution are electronically reduced to copper nanoparticles and deposited on the surface of the silicon waste; (2) adding the silicon waste material deposited with copper nanoparticles into an etchant for metal-assisted chemical etching so that the nanometer-scale copper particles are uniformly introduced into the silicon waste material to obtain a nanometer-scale copper / silicon composite; the etchant is HF-oxidant-organic solvent; (3) placing the nano-micron copper / silicon composite in an air atmosphere for controllable oxidation treatment to obtain a controllable oxidation product, mixing the controllable oxidation product, a binder and a pore-forming agent, and pressing the tablets, and sintering under a protective atmosphere to obtain a molten salt electrolysis precursor; (4) The upper and lower surfaces of the molten salt electrolysis precursor are bonded to the sheet current collector and then suspended on a hook-shaped cathode current collector as the cathode. A graphite crucible is used as the anode. Metal halide molten salt is added to the graphite crucible. A first constant current molten salt electrolysis reduction and a second constant current molten salt electrolysis reduction are performed in sequence under a protective atmosphere to obtain a silicon-copper composite nanowire negative electrode material.

2. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: The particle size of the photovoltaic silicon cutting waste in step (1) is 0.5 to 10 μm.

3. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: Step (1) The copper salt is one or more of Cu(NO3)2, CuCl2, CuSO4, Cu(C2H3O2)2, CuO, Cu(OH)2, CuCO3, Cu(CN)2, and CuF2, and the copper salt solution contains Cu 2+ The concentration is 0.005-1 mol / L; the reducing agent is one or more of HF, sodium borohydride, ascorbic acid, hydrazine, and formaldehyde, and the added molar amount of the reducing agent is Cu 2+ 1 to 60 times of.

4. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: In step (2), the oxidant in the etchant is one or more of H2O2, HClO3, KMnO4, HNO3, Br2, concentrated H2SO4, C2H4O3, the organic solvent is one or more of acetone, methanol, ethanol, tetrahydrofuran, benzene, the reducing agent concentration is 0.1 to 22 mol / L, and the oxidant concentration is 0.1 to 5 mol / L.

5. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 4, characterized in that: The temperature of the metal-assisted chemical etching in step (2) is 15 to 80° C. and the time is 1 to 400 min.

6. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: The temperature of the controlled oxidation treatment in step (3) is 300-1000° C., and the time is 2-10 hours; the mass ratio of the controlled oxidation product, the binder and the pore-forming agent is 100:20-50:10-50; the tableting pressure is 5-30 MPa, and the pressure holding time is 1-10 minutes; the sintering temperature is 300-800° C., and the time is 2-5 hours.

7. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: In step (3), the binder is one or more of epoxy resin, silicone, starch, chitosan, polyamide, acrylate, phenolic resin, polyimide, polyvinyl alcohol, and polyvinyl butyral; the pore-forming agent is one or more of halogen salt, NH4NO3, (NH4)2SO4, (NH4)2CO3, and NH4HCO3; and the protective atmosphere is nitrogen, argon, or helium.

8. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: In step (4), the sheet current collector is platinum, tungsten, molybdenum or zirconium, the hook-shaped cathode current collector is a platinum hook, tungsten hook, molybdenum hook or zirconium hook corresponding to the sheet current collector, the metal halide molten salt is NaCl-CaCl2 molten salt, NaCl-KCl-MgCl2 molten salt, CaF2-NaF-MgF2 molten salt, NaCl-CaCl2-LiF molten salt, NaCl-CaCl2-LiCl molten salt, KCl-CaCl2 molten salt, NaCl-KCl molten salt, NaCl-CaCl2-CaF2 molten salt, NaCl molten salt, CaCl2 molten salt, CaCl2-KCl-MgCl2 molten salt, LiF-BeF2 molten salt or NaF-ZrF4 molten salt, and the protective atmosphere is nitrogen, argon or helium.

9. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: Step (4) The temperature of the first constant current molten salt electrolytic reduction is 700-1000° C., the current is 0.5-3A, and the time is 1-6h.

10. The method for preparing silicon-copper composite nanowire negative electrode material using photovoltaic silicon cutting waste according to claim 1, characterized in that: In step (4), the temperature of the second constant current molten salt electrolytic reduction is 700-1000° C., the current of the second constant current molten salt electrolytic reduction is 0.3-0.5A lower than the current of the first constant current molten salt electrolytic reduction, and the time is 1-6h.

Citation Information

Patent Citations

  • Method for preparing nanometer silicon based on introduction of metal into metallothermic reduction

    CN106495161A

  • Transition metal ammonia complex functionalized polydopamine, and preparation method and application thereof

    CN108484907A

  • Preparation method of silicon-based composite material for lithium ion power battery

    CN109755546A

  • Method for preparing boron-doped nano-metal / porous silicon-carbon composite negative electrode based on cut silicon wastes

    CN111799460A

  • Preparation method of porous silicon / metal / carbon nanomaterial composite negative electrode material of lithium ion battery

    CN115472813A