Negative electrode material and preparation method thereof, negative electrode plate and lithium ion battery
By embedding single crystal silicon into the sodium aluminosilicate core in a lithium-ion battery and coated with carbon and graft copolymer layers, the cycle stability and water reaction problems of silicon-based materials are solved, and the Coulomb efficiency and cycling performance of the battery are improved. .
Patent Information
- Application Number
- CN202411043369.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Silicon-based anode materials have problems such as poor circulation stability and prone to side reactions with water in lithium-ion batteries, resulting in reduced Coulombic efficiency and deterioration of circulation performance of lithium-ion batteries.
Single crystal silicon is embedded in the sodium aluminosilicate core, and the surface is coated with carbon cladding and graft copolymer cladding. The contact between single crystal silicon and water is blocked by the sodium aluminosilicate core, reducing volume expansion and improving Conductivity.
The first Coulomb efficiency and cyclic performance of the negative electrode material are improved, structural stability and conductivity are enhanced, and the water reaction problem of silicon-based materials during the slurry combination process is solved.
Smart Images

Figure CN118970001A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a negative electrode material and a preparation method thereof, a negative electrode sheet and a lithium ion battery. Background Art
[0002] With the development of electric vehicles and portable electrical appliances, the demand for high energy density lithium-ion batteries is also increasing. The theoretical specific capacity of traditional graphite as anode material in lithium-ion batteries is only 372mAh / g, which is difficult to meet market demand. The first gram capacity of silicon as anode material in lithium-ion batteries is 4200mAh / g. Compared with graphite as anode material, silicon as anode material has a higher lithium insertion platform. Therefore, silicon as anode material for lithium-ion batteries has gradually attracted widespread attention from researchers.
[0003] However, the volume expansion of silicon is as high as 300%. During the cycle, it will not only cause the silicon to separate from the surrounding conductive carbon network, forming "dead silicon", but also cause the silicon to peel off from the current collector. Secondly, the large volume expansion will also cause the SEI film on the surface to be continuously reorganized and destroyed, making the SEI film thicker and thicker, and constantly consuming the positive electrode's Li + , resulting in a decrease in the coulombic efficiency of lithium-ion batteries. Finally, the large volume expansion can easily lead to the pulverization of silicon materials in the later stages of the cycle, ultimately causing a sharp deterioration in the cycle performance of lithium-ion batteries.
[0004] Due to the above problems with silicon, academia and industry have shifted some of their attention to silicon oxide. Compared with nano-silicon, although silicon oxide sacrifices some capacity, its expansion is relatively small (about 100%), and the byproducts such as lithium oxide, lithium silicate, and lithium metasilicate generated during the charge and discharge process can provide a buffering effect, thereby greatly improving the cycle performance of the material. However, the conductivity of silicon oxide is relatively poor, and the first coulomb efficiency is low. Nitrogen-doped carbon coating for a high-performance SiO anode in lithium-ion batteries [J]. Electrochemistry Communications, 2013, 34: 98-101, the document discloses the preparation of nitrogen-doped carbon-coated SiO material by liquid phase mixing and high-temperature carbonization. The cycle performance of the material is relatively good, but its first coulomb efficiency is low, and the intrinsic electronic conductivity of the material is not improved. Improvement of irreversible behavior of SiO anodes for lithium ion batteries by a solid state reaction at high temperature[J].Journal of Power Sources,2016,311:159-166, the document discloses that SiO and lithium metal are reacted in a solid state and then carbon coated to prepare a high first-efficiency silicon-based negative electrode material. This method improves the first coulomb efficiency of the material, but its cycle performance is relatively poor. Since lithium metal is used as a reactant, the synthesis conditions are relatively harsh and there is a safety risk. At the same time, due to the pre-lithiation treatment of SiO, a large amount of lithium carbonate and lithium hydroxide exist on the surface of the pre-lithiation treated SiO, and the lithium silicate inside the pre-lithiation treated SiO will dissolve during air storage and during the aqueous slurry process, and further converted into lithium carbonate and lithium hydroxide. Lithium carbonate and lithium hydroxide are prone to gasification and reaction with the binder during the battery slurry process, resulting in poor cycle performance of the formed negative electrode material. Therefore, considering the urgent need for the application of high first-efficiency silicon negative electrode materials in battery cells, it is urgent to solve the above defects. Summary of the invention
[0005] The main purpose of the present invention is to provide a negative electrode material and a preparation method thereof, a negative electrode sheet and a lithium ion battery, so as to solve the problem in the prior art that silicon-based negative electrode materials are prone to side reactions with water during the slurry mixing process and have poor cycle stability.
[0006] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a negative electrode material is provided, which includes single crystal silicon, a sodium aluminosilicate core and a coating layer, wherein the single crystal silicon is embedded in the sodium aluminosilicate core, and the coating layer includes a carbon coating layer, and the carbon coating layer is coated on the surface of the sodium aluminosilicate core.
[0007] Furthermore, the thickness of the above-mentioned carbon coating layer is 10 to 100 nm; and / or, the coating layer also includes a graft copolymer coating layer formed by grafting poly 3,4-ethylenedioxythiophene as a side chain segment onto the main chain of a polyvinyl alcohol molecule, and the graft copolymer coating layer is arranged on the outer surface of the carbon coating layer, and / or, the thickness of the graft copolymer coating layer is 5 nm to 50 nm; and / or, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 33 to 44:46 to 57:3 to 5:2 to 5; and / or, the grain size of single crystal silicon is 0.5 nm to 5 nm; and / or, the mass ratio of the main chain of the polyvinyl alcohol molecule and the side chain segment of poly 3,4-ethylenedioxythiophene in the graft copolymer coating layer is 9 to 99:1.
[0008] Furthermore, the pH value of the negative electrode material is 7.5 to 10; and / or the residual alkali content on the surface of the negative electrode material is 20 to 150 ppm; and / or the powder resistivity of the negative electrode material is 0.5 Ω·cm to 1 Ω·cm.
[0009] According to another aspect of the present invention, there is provided a method for preparing the aforementioned negative electrode material, the method comprising: step S1, sintering a raw material comprising SiO and a carbon source in a first inert atmosphere to obtain carbon-coated SiO; step S2, mixing a raw material comprising carbon-coated SiO, sodium dihydrobis(2-methoxyethoxy)aluminate, and an organic solvent in a second inert atmosphere, and sequentially performing a pre-sodium reaction and solid-liquid separation to obtain pre-sodium carbon-coated SiO; step S3, calcining the pre-sodium carbon-coated SiO in a third inert atmosphere to obtain a negative electrode material; wherein the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to carbon-coated SiO is 5:3 to 25:32; during the calcination process, the calcination temperature is gradually increased.
[0010] Furthermore, in the above step S2, the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to the organic solvent is 2-4:6-8; and / or the temperature of the pre-sodium reaction is 40-60°C; and / or the insulation time of the pre-sodium reaction is 4-8h; and / or the second inert atmosphere is selected from any one or more of helium, neon and argon; and / or the organic solvent is a benzene organic solvent, preferably the benzene organic solvent is benzene and / or toluene; and / or the solid-liquid separation is a process of evaporating the solvent, and the evaporation temperature is 100-150°C.
[0011] Further, in the above step S1, the temperature of the sintering treatment is 600°C to 800°C; and / or, the holding time of the sintering treatment is 1h to 6h; preferably, the sintering treatment is carried out in the first kiln, and the rotation speed of the first kiln is 0.25r / min to 2r / min; and / or, the carbon source is an organic hydrocarbon gas, and preferably the organic hydrocarbon gas is selected from any one or more of alkanes, alkenes, and alkynes; further, the organic hydrocarbon gas is preferably selected from any one or more of methane, ethylene and acetylene; and / or, the volume ratio of the first inert atmosphere and the carbon source is 1 to 4:1; and / or, the total flow rate of the first inert atmosphere and the carbon source is 80L / h to 200L / h; and / or, the first inert atmosphere is selected from any one or more of nitrogen, helium, neon and argon.
[0012] Further, in the above step S3, the calcination treatment includes a first calcination treatment, a second calcination treatment and a third calcination treatment performed in sequence; and / or, the temperature of the first calcination treatment is 200°C to 400°C; and / or, the holding time of the first calcination treatment is 8h to 24h; and / or, the heating rate of the first calcination treatment is 1°C / min to 3°C / min; and / or, the temperature of the second calcination treatment is 450°C to 700°C; and / or, the holding time of the second calcination treatment is 8h to 24h; and / or , the heating rate of the second calcination treatment is 1°C / min to 3°C / min; and / or, the temperature of the third calcination treatment is 750°C to 900°C; and / or, the holding time of the third calcination treatment is 2h to 8h; and / or, the heating rate of the third calcination treatment is 1°C / min to 3°C / min; preferably, the calcination treatment is carried out in the second kiln, and the rotation speed of the second kiln is 2.5r / min to 5r / min; and / or, the third inert atmosphere is selected from any one or more of helium, neon and argon.
[0013] Furthermore, the preparation method further comprises: step S4, wherein a reaction system comprising a mixture of the raw materials of the calcined product in step S3, polyvinyl alcohol, 3,4-ethylenedioxythiophene, a grafting agent, a solvent, acetylacetone and hydrogen peroxide is subjected to polymerization reaction and high temperature treatment in sequence to obtain a negative electrode material; preferably, the molecular weight of the polyvinyl alcohol is 25000 to 120000, and / or the mass ratio of the polyvinyl alcohol to 3,4-ethylenedioxythiophene is 8 to 100:1; and / or the mass ratio of the grafting agent to 3,4-ethylenedioxythiophene is 0.2 to 1:1; and / or the calcined product in step S3 is The mass ratio of the product to polyvinyl alcohol is 95:99 to 1:5; and / or the mass ratio of hydrogen peroxide to 3,4-ethylenedioxythiophene is 1:2 to 4; and / or the pH value of the reaction system is 3 to 5, and / or the mass ratio of acetylacetone to 3,4-ethylenedioxythiophene is 1 to 2:1; and / or the polymerization reaction temperature is 10°C to 40°C, and / or the polymerization reaction time is 2h to 8h; and / or the high temperature treatment temperature is 60 to 80°C, and / or the high temperature treatment time is 8 to 24h; and / or the grafting agent is 3-boric acid thiophene; and / or the solvent is dimethyl sulfoxide.
[0014] According to another aspect of the present invention, a negative electrode sheet is provided, wherein the negative electrode sheet contains the negative electrode material mentioned above.
[0015] According to another aspect of the present invention, a lithium-ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the negative electrode sheet is the negative electrode sheet mentioned above.
[0016] By applying the technical solution of the present invention, the single crystal silicon in the negative electrode material is embedded in the sodium aluminosilicate core. On the one hand, the presence of the sodium aluminosilicate core helps to reduce the volume expansion of the single crystal silicon during the charge and discharge process; on the other hand, the single crystal silicon is a single substance of silicon and is easy to react with water. Since the sodium aluminosilicate core can exist stably in water, the sodium aluminosilicate core can prevent the direct contact between the single crystal silicon and water, thereby helping to reduce the erosion of the single crystal silicon by water during the homogenization process, and further solves the problem that the silicon-based negative electrode material is easy to react with water during the slurry process. In addition, the carbon coating layer in the negative electrode material is coated on the surface of the sodium aluminosilicate core, which helps to improve the conductivity and structural stability of the negative electrode material. Combining the above favorable factors, the negative electrode material of the present application has the characteristics of high initial efficiency, good cycle performance and good rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0018] Figure 1 The SEM image of the negative electrode material in Example 1 of the present application is shown;
[0019] Figure 2 The SEM image of the negative electrode material in Comparative Example 1 of the present application is shown;
[0020] Figure 3 The first charge and discharge curves of the negative electrode materials in Example 1 and Comparative Example 1 of the present application at a current density of 0.1C are shown;
[0021] Figure 4 The first charge and discharge curves of the negative electrode materials in Example 1 and Comparative Example 2 of the present application at a current density of 0.1C are shown; and
[0022] Figure 5 The cycle performance curves of the negative electrode materials in Example 1, Comparative Example 1, Comparative Example 2 and Example 5 of the present application at a current density of 1C / 1C are shown. DETAILED DESCRIPTION
[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0024] As analyzed in the background technology of this application, there are problems in the prior art that silicon-based negative electrode materials are prone to side reactions with water during the slurry mixing process and have poor cycle stability. In order to solve the above problems, this application provides a negative electrode material and a preparation method thereof, a negative electrode sheet and a lithium-ion battery.
[0025] In a typical embodiment of the present application, a negative electrode material is provided, which includes single crystal silicon, a sodium aluminosilicate core and a coating layer, wherein the single crystal silicon is embedded in the sodium aluminosilicate core, and the coating layer includes a carbon coating layer, and the carbon coating layer is coated on the surface of the sodium aluminosilicate core.
[0026] The single crystal silicon in the negative electrode material is embedded in the sodium aluminosilicate core. On the one hand, the presence of the sodium aluminosilicate core helps to reduce the volume expansion of the single crystal silicon during the charge and discharge process; on the other hand, the single crystal silicon is a single silicon substance and is easy to react with water. Since the sodium aluminosilicate core can exist stably in water, the sodium aluminosilicate core can prevent the direct contact between the single crystal silicon and water, thereby helping to reduce the erosion of water on the single crystal silicon during the slurry process, and further solves the problem that the silicon-based negative electrode material is easy to react with water during the slurry process. In addition, the carbon coating layer in the negative electrode material is coated on the surface of the sodium aluminosilicate core, which helps to improve the conductivity and structural stability of the negative electrode material. Combining the above favorable factors, the negative electrode material of the present application has the characteristics of high initial efficiency, good cycle performance and good rate performance.
[0027] In one embodiment of the present application, the thickness of the above-mentioned carbon coating layer is 10 to 100 nm; and / or, the coating layer also includes a graft copolymer coating layer formed by grafting poly 3,4-ethylenedioxythiophene as a side chain segment onto the main chain of a polyvinyl alcohol molecule, and the graft copolymer coating layer is arranged on the outer surface of the carbon coating layer, and / or, the thickness of the graft copolymer coating layer is 5 to 50 nm; and / or, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 33 to 44:46 to 57:3 to 5:2 to 5; and / or, the grain size of single crystal silicon is 0.5 nm to 5 nm; and / or, the mass ratio of the main chain of the polyvinyl alcohol molecule and the side chain segment of poly 3,4-ethylenedioxythiophene in the graft copolymer coating layer is 9 to 99:1.
[0028] The thickness of the carbon coating layer is preferably controlled within the above range, which helps to further improve the conductivity and structural stability of the negative electrode material; a graft copolymer coating layer formed by grafting poly 3,4-ethylenedioxythiophene as a branch chain segment on the main chain of polyvinyl alcohol molecule is arranged on the carbon coating layer, which helps to improve the conductivity of the negative electrode material. The main chain of the polyvinyl alcohol molecule and the branch chain segment of poly 3,4-ethylenedioxythiophene in the graft copolymer coating layer are grafted by a grafting agent to form a graft copolymer. Therefore, the graft copolymer coating layer has both the rigidity of the branch chain segment of poly 3,4-ethylenedioxythiophene and the flexibility of the main chain of polyvinyl alcohol molecule, which can effectively buffer the volume expansion of the negative electrode material during charging and discharging, maintain the interface stability of the negative electrode material, and thus improve the cycle performance of the negative electrode material. The thickness of the graft copolymer coating layer is preferably controlled within the above range, which helps to further improve the conductivity and interface stability of the negative electrode material. The presence of the sodium aluminosilicate core helps to reduce the volume expansion of the single crystal silicon during the charge and discharge process, and reduces the erosion of the single crystal silicon by water during the homogenization process. The co-existence of the carbon coating layer and the graft copolymer coating layer helps to further reduce the volume expansion of the single crystal silicon. It is preferred to control the mass ratio of the single crystal silicon, the sodium aluminosilicate core, the carbon coating layer and the graft copolymer coating layer within the above range, which not only helps to reduce the volume expansion of the negative electrode material during the charge and discharge process, but also helps to improve the first effect and cycle performance of the negative electrode material. It is preferred to control the grain size of the single crystal silicon within the above range, which helps to reduce the volume expansion of the negative electrode material, thereby improving the cycle stability of the negative electrode material. If the mass ratio of the polyvinyl alcohol main chain and the poly(3,4-ethylenedioxythiophene) side chain segments is too small, the formed graft copolymer coating layer will be too rigid and the graft copolymer coating layer will be easily broken; if the mass ratio of the polyvinyl alcohol main chain and the poly(3,4-ethylenedioxythiophene) side chain segments is too large, the formed graft copolymer coating layer will be too flexible, which is not conducive to reducing the volume expansion of the negative electrode material. It is preferred to control the mass ratio of the polyvinyl alcohol main chain and the poly(3,4-ethylenedioxythiophene) side chain segments within the above range, which helps to take into account the rigidity of the poly(3,4-ethylenedioxythiophene) side chain segments and the flexibility of the polyvinyl alcohol main chain, thereby helping to buffer the volume expansion of the negative electrode material during charging and discharging, while improving the stability and conductivity of the negative electrode material interface.
[0029] In one embodiment of the present application, the pH value of the negative electrode material is 7.5-10; and / or the surface residual alkali content of the negative electrode material is 20-150 ppm; and / or the powder resistivity of the negative electrode material is 0.5Ω·cm-1Ω·cm.
[0030] The negative electrode material with the above pH value and surface residual alkali amount helps to reduce the gas production of the negative electrode material during the homogenization process as much as possible, thereby improving the structural stability of the negative electrode material. The negative electrode material with the above conductivity helps to improve the first efficiency and rate performance of the negative electrode material.
[0031] In another typical embodiment of the present application, a method for preparing the aforementioned negative electrode material is provided, the preparation method comprising: step S1, sintering a raw material including SiO and a carbon source in a first inert atmosphere to obtain carbon-coated SiO; step S2, mixing a raw material including carbon-coated SiO, sodium dihydrobis(2-methoxyethoxy)aluminate, and an organic solvent in a second inert atmosphere, and then sequentially performing a pre-sodium reaction and solid-liquid separation to obtain pre-sodium carbon-coated SiO; step S3, calcining the pre-sodium carbon-coated SiO in a third inert atmosphere to obtain a negative electrode material; wherein the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to carbon-coated SiO is 5:3 to 25:32; during the calcination process, the calcination temperature gradually increases.
[0032] Sodium dihydrogen bis(2-methoxyethoxy)aluminate can be reduced to single crystal silicon with SiO, and can also react with SiO to form sodium silicate. The present application controls the mass ratio of sodium dihydrogen bis(2-methoxyethoxy)aluminate to carbon-coated SiO within the above range and the temperature of the calcination treatment is a gradually increasing process, thereby taking into account the process of sodium dihydrogen bis(2-methoxyethoxy)aluminate being reduced to single crystal silicon with SiO and reacting with SiO to form sodium silicate. In step S1, SiO and a carbon source are sintered to coat a carbon coating layer on the surface of SiO to form carbon-coated SiO. The carbon coating layer helps to reduce the direct contact rate between SiO and sodium dihydrogen bis(2-methoxyethoxy)aluminate during the pre-sodium process, thereby helping to control the growth rate of single crystal silicon grains. In step S2, sodium dihydrobis(2-methoxyethoxy)aluminate is used to pre-sodiumize the carbon-coated SiO, which is beneficial to control the pre-sodium reaction speed, thereby controlling the grain size of the single crystal silicon, and removing the solvent after the pre-sodium reaction by solid-liquid separation to obtain pre-sodium carbon-coated SiO. In step S3, as the temperature of the calcination treatment gradually increases, the unreacted part of the sodium dihydrobis(2-methoxyethoxy)aluminate in the pre-sodium reaction at low temperature melts and enters the interior of the carbon-coated SiO through the pores of the carbon coating, thereby reducing part of the SiO to single crystal silicon. At medium temperature, a large amount of sodium ions in sodium dihydrobis(2-methoxyethoxy)aluminate continuously diffuse into the interior of SiO, thereby reacting with SiO to form a large amount of sodium silicate. At high temperature, the sodium silicate formed at medium temperature is converted into sodium aluminosilicate. In addition, the organic functional groups in sodium dihydrobis(2-methoxyethoxy)aluminate are carbonized during the calcination process, which helps to repair the carbon coating layer destroyed during the pre-sodiumization process, thereby improving the conductivity of the negative electrode material.
[0033] In addition, it is preferred to control the particle size distribution of SiO2 in step S1 to be Dmin≥2μm, D10≥5μm, 8≤D50≤10μm, and Dmax≤16μm, which helps to improve the integrity of the carbon coating layer and further ensure the uniformity of the carbon-coated SiO2 particle size, thereby helping to reduce the negative impact of the pre-sodium process. If Dmin is too small or Dmax is too large, it is easy to cause excessive pre-sodium of small particles and insufficient pre-sodium of large particles, which ultimately affects the first effect and cycle performance of the negative electrode material. It is preferred to control the D50 particle size to 8-10μm, which helps to balance the reduction reaction and disproportionation reaction during the pre-sodium process, and thus helps to control the grain size of monocrystalline silicon, and further helps to improve the cycle stability of the negative electrode material.
[0034] It is preferred to control the particle size distribution of carbon-coated SiO2 to be Dmin≥3μm, D10≥5.5μm, 8.5≤D50≤10.5μm, and Dmax≤20μm, which is beneficial to controlling the uniformity of pre-sodium in the subsequent pre-sodium process.
[0035] In one embodiment of the present application, in the above step S2, the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to the organic solvent is 2-4:6-8; and / or the temperature of the pre-sodium reaction is 40-60°C; and / or the insulation time of the pre-sodium reaction is 4-8h; and / or the second inert atmosphere is selected from any one or more of helium, neon and argon; and / or the organic solvent is a benzene organic solvent, preferably the benzene organic solvent is benzene and / or toluene; and / or the solid-liquid separation is a process of evaporating the solvent, and the evaporation temperature is 100-150°C.
[0036] It is preferred to control the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to the organic solvent within the above range, which helps to improve the dispersibility of sodium dihydrobis(2-methoxyethoxy)aluminate in the organic solvent. It is preferred to control the temperature and holding time of the pre-sodium reaction within the above range, which helps to control the reaction rate of sodium dihydrobis(2-methoxyethoxy)aluminate and SiO, thereby helping to control the grain size of single crystal silicon. It is preferred to control the type of the second inert atmosphere within the above range, which helps to enrich the selectivity of the inert gas. It is preferred to control the type of the organic solvent within the above range, which helps to improve the solubility and dispersibility of sodium dihydrobis(2-methoxyethoxy)aluminate in the solvent. The solvent after the pre-sodium reaction is removed by evaporation. The evaporation temperature is controlled within the above range according to the boiling point of the solvent, which helps to improve the efficiency of solvent removal.
[0037] In one embodiment of the present application, in the above-mentioned step S1, the temperature of the sintering treatment is 600℃~800℃; and / or the holding time of the sintering treatment is 1h~6h; preferably, the sintering treatment is carried out in the first kiln, and the rotation speed of the first kiln is 0.25r / min~2r / min; and / or, the carbon source is an organic hydrocarbon gas, and preferably the organic hydrocarbon gas is selected from any one or more of alkanes, alkenes, and alkynes; further, it is preferred that the organic hydrocarbon gas is selected from any one or more of methane, ethylene and acetylene; and / or, the volume ratio of the first inert atmosphere and the carbon source is 1~4:1; and / or, the total flow rate of the first inert atmosphere and the carbon source is 80L / h~200L / h; and / or, the first inert atmosphere is selected from any one or more of nitrogen, helium, neon and argon.
[0038] If the sintering temperature is too low, it will be disadvantageous to reduce the defects of the carbon coating layer; if the sintering temperature is too high, it will be disadvantageous to reduce the effect of temperature on SiO. It is preferred to control the sintering temperature and the holding time within the above range, which helps to balance the integrity of the carbon coating layer and the effect of temperature on SiO. It is preferred to control the sintering process in a kiln and control the rotation speed of the kiln within the above range, which helps to improve the efficiency of the sintering process. It is preferred to control the type of carbon source within the above range, which helps to reduce the defects of the carbon coating layer. It is preferred to control the volume ratio of the first inert atmosphere and the carbon source and the total flow rate of the first inert atmosphere and the carbon source within the above range, which helps to control the thickness of the carbon coating layer, thereby helping to improve the conductivity of the negative electrode material. It is preferred to control the type of the first inert atmosphere within the above range, which helps to enrich the selectivity of the first inert atmosphere.
[0039] In one embodiment of the present application, in the above step S3, the calcination treatment includes a first calcination treatment, a second calcination treatment and a third calcination treatment performed in sequence; and / or the temperature of the first calcination treatment is 200°C to 400°C, and / or the holding time of the first calcination treatment is 8h to 24h, and / or the heating rate of the first calcination treatment is 1°C / min to 3°C / min; and / or the temperature of the second calcination treatment is 450°C to 700°C, and / or the holding time of the second calcination treatment is 8h to 24h, And / or the heating rate of the second calcination treatment is 1°C / min to 3°C / min; and / or the temperature of the third calcination treatment is 750°C to 900°C, and / or the holding time of the third calcination treatment is 2h to 8h, and / or the heating rate of the third calcination treatment is 1°C / min to 3°C / min; preferably, the calcination treatment is carried out in the second kiln, and the rotation speed of the second kiln is 2.5r / min to 5r / min; and / or the third inert atmosphere is selected from any one or more of helium, neon and argon.
[0040] The purpose of the first calcination treatment is to melt the unreacted sodium dihydrobis(2-methoxyethoxy)aluminate in the pre-sodium reaction and reduce part of SiO to Si. It is preferred to control the temperature, time and heating rate of the first calcination treatment within the above range, which helps to promote the melting of sodium dihydrobis(2-methoxyethoxy)aluminate and control the size of single crystal silicon grains. Under the second calcination treatment, the sodium ions in sodium dihydrobis(2-methoxyethoxy)aluminate continue to diffuse into the interior of SiO and react with SiO to form sodium silicate. It is preferred to control the temperature, time and heating rate of the second calcination treatment within the above range, which helps to promote the formation of sodium silicate. Under the third calcination treatment, the sodium silicate formed by the second calcination treatment is converted into sodium aluminosilicate. It is preferred to control the temperature, time and heating rate of the third calcination treatment within the above range, which helps to promote the formation of sodium aluminosilicate. It is preferred to control the calcination treatment in a kiln, which helps to improve the reaction efficiency of the calcination treatment. It is preferred to control the third inert atmosphere in the above range, which helps to reduce the side effects of the calcination atmosphere on the calcination treatment and enrich the selectivity of the third inert atmosphere.
[0041] In one embodiment of the present application, the preparation method further includes: step S4, wherein a reaction system comprising a mixture of the raw materials of the calcined product in step S3, polyvinyl alcohol, 3,4-ethylenedioxythiophene, a grafting agent, a solvent, acetylacetone and hydrogen peroxide is subjected to polymerization reaction and high temperature treatment in sequence to obtain a negative electrode material; preferably, the molecular weight of the polyvinyl alcohol is 25000 to 120000, and / or the mass ratio of the polyvinyl alcohol to 3,4-ethylenedioxythiophene is 8 to 100:1; and / or the mass ratio of the grafting agent to 3,4-ethylenedioxythiophene is 0.2 to 1:1; and / or the calcined product in step S3 is subjected to polymerization reaction and high temperature treatment in sequence to obtain a negative electrode material. The mass ratio of the calcined product to polyvinyl alcohol is 95:99 to 1:5; and / or the mass ratio of hydrogen peroxide to 3,4-ethylenedioxythiophene is 1:2 to 4; and / or the pH value of the reaction system is 3 to 5, and / or the mass ratio of acetylacetone to 3,4-ethylenedioxythiophene is 1 to 2:1; and / or the polymerization temperature is 10 to 40°C, and / or the polymerization time is 2h to 8h; and / or the high temperature treatment temperature is 60 to 80°C, and / or the high temperature treatment time is 8 to 24h; and / or the grafting agent is 3-boric acid thiophene; and / or the solvent is dimethyl sulfoxide.
[0042] In step S4, the grafting agent and polyvinyl alcohol are connected by hydrogen bonds. Under the co-catalysis of hydrogen peroxide and acetylacetone, 3,4-ethylenedioxythiophene is polymerized on the surface of the carbon coating layer, and the grafting agent and 3,4-ethylenedioxythiophene are copolymerized, thereby forming a graft copolymer coating layer on the surface of the carbon coating layer, in which poly 3,4-ethylenedioxythiophene is grafted as a side chain segment onto the main chain of the polyvinyl alcohol molecule. The graft copolymer coating layer formed by grafting poly 3,4-ethylenedioxythiophene as a side chain segment onto the main chain of the polyvinyl alcohol molecule is treated at high temperature, which helps to improve the strength and integrity of the graft copolymer coating layer. It is preferred to control the molecular weight of polyvinyl alcohol within the above range, which helps to obtain a polymer material with a certain chain length and flexibility. It is preferred to control the molar ratio of polyvinyl alcohol and 3,4-ethylenedioxythiophene within the above range, which helps to control the mass ratio of the main chain of the polyvinyl alcohol molecule to the side chain segment of poly-3,4-ethylenedioxythiophene, thereby helping to make the graft copolymer coating layer have both the rigidity of poly-3,4-ethylenedioxythiophene and the flexibility of polyvinyl alcohol, thereby effectively buffering the volume expansion of the negative electrode material during charging and discharging. It is preferred to control the molar ratio of the grafting agent and 3,4-ethylenedioxythiophene within the above range, which helps to promote the formation of the graft copolymer coating layer. It is preferred to control the mass ratio of the product after calcination treatment in step S3 and 3,4-ethylenedioxythiophene within the above range, which helps to control the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer, thereby helping to reduce the volume expansion of the negative electrode material during charging and discharging and improve the conductivity of the negative electrode material. It is preferred to control the molar ratio of hydrogen peroxide to 3,4-ethylenedioxythiophene, the pH value of the reaction system, and the molar ratio of acetylacetone to 3,4-ethylenedioxythiophene within the above ranges, which helps to improve the reaction efficiency of the polymerization reaction. It is preferred to control the temperature and time of the high temperature treatment within the above ranges, which helps to further improve the strength and integrity of the graft copolymer coating layer. It is preferred to control the types of grafting agents and solvents within the above ranges, which helps to enrich the selectivity of grafting agents and solvents.
[0043] In addition, polyvinyl alcohol is preferably added to dimethyl sulfoxide, and the polyvinyl alcohol is completely dissolved by heating in a water bath at a temperature of 60°C to 80°C. Then, 3,4-ethylenedioxythiophene and 3-boric acid thiophene are added, stirred to completely dissolve, and then cooled to room temperature. Then, the product calcined in step S3 is added, stirred to disperse evenly, and then hydrogen peroxide is added, stirred and mixed evenly, and then acetylacetone solution is added to carry out polymerization reaction.
[0044] In another typical embodiment of the present application, a negative electrode sheet is provided, wherein the negative electrode sheet contains the aforementioned negative electrode material.
[0045] The negative electrode sheet including the above negative electrode materials has the characteristics of high initial efficiency, good cycle performance and good rate performance.
[0046] In another typical embodiment of the present application, a lithium-ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the negative electrode sheet is the negative electrode sheet mentioned above.
[0047] The lithium-ion battery including the above negative electrode sheet has high initial efficiency, good cycle performance, excellent rate performance, and at the same time, the lithium-ion battery has a high safety factor.
[0048] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0049] Example 1
[0050] 3 kg of SiO2 was placed in a rotary kiln and sintered in a mixed gas of nitrogen and acetylene. The sintered product was crushed to obtain carbon-coated SiO2. min 3.2μm, D10 is 5.6μm, D50 is 8.3μm, D max The D50 of carbon-coated SiO is 14.7μm, the D50 of carbon-coated SiO is 8.8μm, the rotation speed of the first kiln is 0.25r / min, the sintering temperature is 750℃, the holding time of sintering is 2h, nitrogen and acetylene are introduced in a volume ratio of 2:1, and the total gas flow rate of nitrogen and acetylene is 180L / h.
[0051] 200 g of sodium dihydrobis(2-methoxyethoxy)aluminate and 800 g of toluene were added to a reactor under argon gas protection, stirred to dissolve evenly, and then 120 g of carbon-coated SiO was added, and after mechanical stirring and dispersion, pre-sodium reaction and solid-liquid separation were performed to obtain pre-sodium carbon-coated SiO. The temperature of the pre-sodium reaction was 60°C, the insulation time of the pre-sodium reaction was 8 hours, and the temperature of the solid-liquid separation was 150°C.
[0052] The pre-sodium carbon-coated SiO2 is placed in a kiln under argon gas protection for calcination, and the calcination treatment includes a first calcination treatment, a second calcination treatment and a third calcination treatment in sequence to obtain a calcined product. The rotation speed of the second kiln is 2.5r / min, the heating rate of the calcination treatment is 1°C / min, the temperature of the first calcination treatment is 400°C, the holding time of the first calcination treatment is 8h, the temperature of the second calcination treatment is 700°C, the holding time of the second calcination treatment is 8h, the temperature of the third calcination treatment is 750°C, and the holding time of the third calcination treatment is 2h.
[0053] Take 25g of polyvinyl alcohol with a molecular weight of 25,000 and add it to 475g of dimethyl sulfoxide. Heat it in a water bath to 60°C to completely dissolve it. Then add 0.25g of 3,4-ethylenedioxythiophene and 0.25g of 3-boric acid thiophene. Stir it to completely dissolve it and cool it to room temperature. Then add 475g of the calcined product and stir it to disperse it evenly. Then add 0.125g of hydrogen peroxide and control the pH of the solution to 5. After stirring and mixing evenly, add 0.5g of acetylacetone to carry out polymerization reaction. The temperature of the polymerization reaction is 30°C, and the reaction time is controlled to 2h to obtain the product after the polymerization reaction. Then place the product after the polymerization reaction in a 60°C oven for high temperature treatment for 8h, then wash it three times with deionized water and alcohol, and then dry it to obtain the negative electrode material. Among them, the thickness of the carbon coating layer is 20nm, the thickness of the graft copolymer coating layer is 50nm, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 44:46:5:5, and the mass ratio of the polyvinyl alcohol molecular main chain and the poly (3,4-ethylenedioxythiophene) side chain segments in the graft copolymer coating layer is 99:1.
[0054] Example 2
[0055] 3kg of SiO2 was placed in a rotary kiln and sintered in a mixed gas of nitrogen and acetylene. The sintered product was crushed to obtain carbon-coated SiO2. Among them, the Dmin of SiO2 was 4.1μm, D10 was 6.2μm, D50 was 10μm, Dmax was 15.8μm, and D50 of carbon-coated SiO2 was 10.5μm. The rotation speed of the first kiln was 2r / min, the sintering temperature was 800℃, the holding time of the sintering was 6h, the volume ratio of nitrogen and acetylene was 4:1, and the total gas flow rate of nitrogen and acetylene was 200L / h.
[0056] 200 g of sodium dihydrobis(2-methoxyethoxy)aluminate and 300 g of toluene were added to a reactor under argon gas protection, stirred to dissolve evenly, and then 256 g of carbon-coated SiO was added, and after mechanical stirring and dispersion, pre-sodium reaction and solid-liquid separation were performed to obtain pre-sodium carbon-coated SiO. The temperature of the pre-sodium reaction was 40°C, the insulation time of the pre-sodium reaction was 4h, and the temperature of the solid-liquid separation was 100°C.
[0057] The pre-sodium carbon-coated SiO2 is placed in a kiln under the protection of helium gas for calcination, and the calcination treatment includes a first calcination treatment, a second calcination treatment and a third calcination treatment in sequence to obtain a calcined product. The rotation speed of the second kiln is 5r / min, the heating rate of the calcination treatment is 3°C / min, the temperature of the first calcination treatment is 200°C, the holding time of the first calcination treatment is 24h, the temperature of the second calcination treatment is 450°C, the holding time of the second calcination treatment is 24h, the temperature of the third calcination treatment is 900°C, and the holding time of the third calcination treatment is 2h.
[0058] Take 25g of polyvinyl alcohol with a molecular weight of 50,000 and add it to 475g of dimethyl sulfoxide. Heat it in a water bath to 60°C to completely dissolve it. Then add 3.125g of 3,4-ethylenedioxythiophene and 0.625g of 3-boric acid thiophene. Stir it to completely dissolve it and cool it to room temperature. Then add 2475g of the calcined product and stir it to disperse it evenly. Then add 0.78g of hydrogen peroxide and control the pH of the solution to 3. After stirring and mixing evenly, add 3.125g of acetylacetone to carry out polymerization reaction. The temperature of the polymerization reaction is 10°C, and the reaction time is controlled to 8h to obtain the product after the polymerization reaction. Then place the product after the polymerization reaction in a 60°C oven for high temperature treatment for 6h, then wash it three times with deionized water and alcohol, and then dry it to obtain the negative electrode material. Among them, the thickness of the carbon coating layer is 100nm, the thickness of the graft copolymer coating layer is 5nm, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 33:57:3:2, and the mass ratio of the polyvinyl alcohol molecular main chain and the poly (3,4-ethylenedioxythiophene) side chain segment in the graft copolymer coating layer is 9:1.
[0059] Example 3
[0060] 3kg of SiO2 was placed in a rotary kiln and sintered in a mixed gas of nitrogen and acetylene. The sintered product was crushed to obtain carbon-coated SiO2. Among them, the Dmin of SiO2 was 3.5μm, the D10 was 5.8μm, the D50 was 9μm, the Dmax was 15.1μm, the D50 of the carbon-coated SiO2 was 9.5μm, the rotation speed of the first kiln was 0.5r / min, the sintering temperature was 600℃, the holding time of the sintering was 4h, the volume ratio of nitrogen and acetylene was 1:1, and the total gas flow rate of nitrogen and acetylene was 80L / h.
[0061] 200 g of sodium dihydrobis(2-methoxyethoxy)aluminate and 500 g of toluene were added to a reactor under argon gas protection, stirred to dissolve evenly, and then 200 g of carbon-coated SiO was added, and after mechanical stirring and dispersion, pre-sodium reaction and solid-liquid separation were performed to obtain pre-sodium carbon-coated SiO. The temperature of the pre-sodium reaction was 50°C, the insulation time of the pre-sodium reaction was 6 hours, and the temperature of the solid-liquid separation was 120°C.
[0062] The pre-sodium carbon-coated SiO2 is placed in a kiln under the protection of helium gas for calcination, and the calcination treatment includes a first calcination treatment, a second calcination treatment and a third calcination treatment in sequence to obtain a calcined product. The rotation speed of the second kiln is 4r / min, the heating rate of the calcination treatment is 2°C / min, the temperature of the first calcination treatment is 300°C, the holding time of the first calcination treatment is 16h, the temperature of the second calcination treatment is 550°C, the holding time of the second calcination treatment is 12h, the temperature of the third calcination treatment is 800°C, and the holding time of the third calcination treatment is 4h.
[0063] Take 25g of polyvinyl alcohol with a molecular weight of 100,000 and add it to 475g of dimethyl sulfoxide. Heat it in a water bath to 60°C to completely dissolve it. Then add 0.5g of 3,4-ethylenedioxythiophene and 0.25g of 3-boric acid thiophene. Stir it to completely dissolve it and cool it to room temperature. Then add 1225g of the calcined product and stir it to disperse it evenly. Then add 0.25g of hydrogen peroxide and control the pH of the solution to 3. After stirring and mixing evenly, add 0.5g of acetylacetone to carry out polymerization reaction. The temperature of the polymerization reaction is 40°C, and the reaction time is controlled to 4h to obtain the product after the polymerization reaction. Then place the product after the polymerization reaction in an 80°C oven for high temperature treatment for 12h, then wash it three times with deionized water and alcohol, and then dry it to obtain the negative electrode material. Among them, the thickness of the carbon coating layer is 40nm, the thickness of the graft copolymer coating layer is 20nm, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 38:55:5:2, and the mass ratio of the polyvinyl alcohol molecular main chain and the poly (3,4-ethylenedioxythiophene) side chain segment in the graft copolymer coating layer is 50:1.
[0064] Example 4
[0065] 3kg of SiO2 was placed in a rotary kiln and sintered in a mixed gas of nitrogen and acetylene. The sintered product was crushed to obtain carbon-coated SiO2. Among them, the Dmin of SiO2 was 3.2μm, D10 was 5.6μm, D50 was 8.3μm, Dmax was 14.7μm, the D50 of carbon-coated SiO2 was 8.6μm, the rotation speed of the first kiln was 1.5r / min, the sintering temperature was 700℃, the holding time of the sintering was 4h, the volume ratio of nitrogen and acetylene was 3:1, and the total gas flow rate of nitrogen and acetylene was 160L / h.
[0066] 200 g of sodium dihydrobis(2-methoxyethoxy)aluminate and 800 g of toluene were added to a reactor under argon gas protection, stirred to dissolve evenly, and then 133.3 g of carbon-coated SiO was added, and after mechanical stirring and dispersion, pre-sodium reaction and solid-liquid separation were performed to obtain pre-sodium carbon-coated SiO. The temperature of the pre-sodium reaction was 50°C, the insulation time of the pre-sodium reaction was 8 hours, and the temperature of the solid-liquid separation was 140°C.
[0067] The pre-sodium carbon-coated SiO is placed in a kiln under the protection of helium gas for calcination, and the calcination treatment includes a first calcination treatment, a second calcination treatment and a third calcination treatment in sequence to obtain a calcined product. Among them, the rotation speed of the second kiln is 3r / min, the heating rate of the calcination treatment is 1°C / min, the temperature of the first calcination treatment is 400°C, the insulation time of the first calcination treatment is 8h, the temperature of the second calcination treatment is 650°C, the insulation time of the second calcination treatment is 12h, the temperature of the third calcination treatment is 750°C, and the insulation time of the third calcination treatment is 2h.
[0068] Take 25g of polyvinyl alcohol with a molecular weight of 120,000 and add it to 475g of dimethyl sulfoxide. Heat it in a water bath to 60°C to completely dissolve it. Then add 1.25g of 3,4-ethylenedioxythiophene and 0.625g of 3-boric acid thiophene. Stir it to completely dissolve it and cool it to room temperature. Then add 816.7g of the calcined product and stir it to disperse it evenly. Then add 0.3g of hydrogen peroxide and control the pH of the solution to 4. After stirring and mixing evenly, add 2.5g of acetylacetone to carry out polymerization reaction. The temperature of the polymerization reaction is 20°C, and the reaction time is controlled to 6h to obtain the product after the polymerization reaction. Then place the product after the polymerization reaction in an 80°C oven for high temperature treatment for 12h, then wash it three times with deionized water and alcohol, and then dry it to obtain the negative electrode material. Among them, the thickness of the carbon coating layer is 60nm, the thickness of the graft copolymer coating layer is 40nm, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 41:49:4:4, and the mass ratio of the polyvinyl alcohol molecular main chain and the poly (3,4-ethylenedioxythiophene) side chain segment in the graft copolymer coating layer is 20:1.
[0069] Example 5
[0070] The difference from Example 1 is that 3,4-ethylenedioxythiophene is not added, and the negative electrode material is finally obtained.
[0071] Example 6
[0072] The difference from Example 1 is that no polyvinyl alcohol is added, and the negative electrode material is finally obtained.
[0073] Example 7
[0074] The difference from Example 1 is that the volume ratio of nitrogen to acetylene is 4:1, and the negative electrode material is finally obtained. The thickness of the carbon coating layer is 10 nm.
[0075] Example 8
[0076] The difference from Example 1 is that the volume ratio of nitrogen to acetylene is 1:1, and the negative electrode material is finally obtained. The thickness of the carbon coating layer is 100 nm.
[0077] Example 9
[0078] The difference from Example 1 is that the volume ratio of nitrogen to acetylene is 1:1.2, and the negative electrode material is finally obtained. The thickness of the carbon coating layer is 110 nm.
[0079] Example 10
[0080] The difference from Example 1 is that the mass ratio of the calcined product to polyvinyl alcohol is 99:1, and the negative electrode material is finally obtained. The thickness of the graft copolymer coating layer is 5 nm.
[0081] Embodiment 11
[0082] The difference from Example 1 is that the mass ratio of the calcined product to polyvinyl alcohol is 96:4, and the negative electrode material is finally obtained. The thickness of the graft copolymer coating layer is 40 nm.
[0083] Example 12
[0084] The difference from Example 1 is that the mass ratio of the calcined product to polyvinyl alcohol is 90:10, and the negative electrode material is finally obtained. The thickness of the graft copolymer coating layer is 80 nm.
[0085] Embodiment 13
[0086] The difference from Example 1 is that the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to carbon-coated SiO is 25:32, and the negative electrode material is finally obtained. Among them, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 33:57:5:5.
[0087] Embodiment 14
[0088] The difference from Example 1 is that the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to carbon-coated SiO is 25:21, and the negative electrode material is finally obtained. Among them, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 39:51:5:5.
[0089] Embodiment 15
[0090] The difference from Example 1 is that the mass ratio of sodium dihydrobis(2-methoxyethoxy)aluminate to carbon-coated SiO is 2:1, and the negative electrode material is finally obtained. Among them, the mass ratio of single crystal silicon, sodium aluminosilicate core, carbon coating layer and graft copolymer coating layer is 48:42:5:5.
[0091] Example 16
[0092] The difference from Example 1 is that the mass ratio of polyvinyl alcohol to 3,4-ethylenedioxythiophene is 8:1; the mass ratio of 3-boric acid thiophene to 3,4-ethylenedioxythiophene is 0.2:1; the mass ratio of hydrogen peroxide to 3,4-ethylenedioxythiophene is 1:4; the mass ratio of acetylacetone to 3,4-ethylenedioxythiophene is 1:1, and the negative electrode material is finally obtained. Among them, the mass ratio of the polyvinyl alcohol main chain to the poly 3,4-ethylenedioxythiophene side chain segment is 9:1.
[0093] Embodiment 17
[0094] The difference from Example 1 is that the mass ratio of polyvinyl alcohol to 3,4-ethylenedioxythiophene is 90:6; the mass ratio of 3-boric acid thiophene to 3,4-ethylenedioxythiophene is 0.6:1; the mass ratio of hydrogen peroxide to 3,4-ethylenedioxythiophene is 1:3; the mass ratio of acetylacetone to 3,4-ethylenedioxythiophene is 1:1, and the negative electrode material is finally obtained. Among them, the mass ratio of the polyvinyl alcohol main chain and the poly 3,4-ethylenedioxythiophene side chain segment is 95:5.
[0095] Embodiment 18
[0096] The difference from Example 1 is that the mass ratio of polyvinyl alcohol to 3,4-ethylenedioxythiophene is 7:1; the mass ratio of 3-boric acid thiophene to 3,4-ethylenedioxythiophene is 1.5:1; the mass ratio of hydrogen peroxide to 3,4-ethylenedioxythiophene is 1:1; the mass ratio of acetylacetone to 3,4-ethylenedioxythiophene is 1:1, and the negative electrode material is finally obtained. Among them, the mass ratio of the main chain of the polyvinyl alcohol molecule to the side chain segment of poly 3,4-ethylenedioxythiophene is 8:1.
[0097] Embodiment 19
[0098] The difference from Example 1 is that the temperature of the pre-sodium reaction is 40° C., the insulation time of the pre-sodium reaction is 4 h, and finally the negative electrode material is obtained.
[0099] Embodiment 20
[0100] The difference from Example 1 is that the sintering temperature is 600° C., the sintering holding time is 1 h, and finally the negative electrode material is obtained.
[0101] Embodiment 21
[0102] The difference from Example 1 is that the sintering temperature is 800° C., the sintering holding time is 6 h, and finally the negative electrode material is obtained.
[0103] Embodiment 22
[0104] The difference from Example 1 is that the temperature of the first calcination treatment is 200°C, and the insulation time of the first calcination treatment is 24 hours, the temperature of the second calcination treatment is 450°C, and the insulation time of the second calcination treatment is 24 hours, the temperature of the third calcination treatment is 900°C, and the insulation time of the third calcination treatment is 8 hours, and finally the negative electrode material is obtained.
[0105] Comparative Example 1
[0106] The difference from Example 1 is that the negative electrode material is a pre-lithium silicon oxide material.
[0107] Comparative Example 2
[0108] The difference from Example 1 is that n-butyl lithium is used to replace sodium dihydrogen bis(2-methoxyethoxy)aluminate to finally obtain the negative electrode material.
[0109] Comparative Example 3
[0110] The difference from Example 1 is that sodium dihydrobis(2-methoxyethoxy)aluminate is not added to finally obtain the negative electrode material.
[0111] Surface residual alkali test
[0112] Weigh the sample according to Table 1 below, accurate to 0.0001g, place the weighed sample in a 100mL beaker, add 50mL deionized water, put the magnetic beads in the beaker and seal it with plastic wrap, then place the beaker on a magnetic stirrer and stir for about 10 to 15 minutes, remove it, let it stand for 5 minutes, and filter it with a glass funnel. The filtered clear liquid is the test solution.
[0113] Table 1
[0114]
[0115] Accurately transfer the solution to be tested into a 100mL beaker, add a stirring rotor, control the sample volume to about 50mL, place the beaker on the magnetic stirrer of the automatic potentiometric titrator, add phenolphthalein for 2d, select the HCl standard solution from the table and titrate it until it changes from red to colorless. The instrument will record the volume Ep of the HCl standard solution consumed at the stoichiometric point. 1 (V 1 ) and pH; then add methyl orange for 2d, continue titrating until it changes from yellow to orange, the instrument will record the volume of HCl standard solution consumed at the stoichiometric point Ep 2 (V 2 ) and pH.
[0116] Analysis results calculation: (1) When 2V 1 ﹥V 2 When containing LiOH, Li 2 CO 3 , the calculation formula is as follows:
[0117]
[0118]
[0119] (2) When 2V 1 <V 2 When Li 2 CO 3 、LiHCO 3 , the calculation formula is as follows:
[0120]
[0121]
[0122] (3) When 2V 1 =V 2 When only Li 2 CO 3 , the calculation formula is as follows:
[0123]
[0124] In the above formula: c represents the concentration of HCl standard solution (mol / L); V 1 (Ep 1 ) represents the volume of HCl standard solution consumed at the first equivalence point (mL); V 2 (Ep 2 ) represents the volume of HCl standard solution consumed at the second equivalence point (including the first equivalence point) (mL); V' represents the volume of the sample solution (mL); V represents the volume of the sample solution (mL); 23.95 is the molar mass of LiOH (g / mol); 73.89 is the molar mass of Li 2 CO 3 The molar mass is g / mol; 67.96 for LiHCO 3 The molar mass is g / mol; m represents the mass of the sample (g).
[0125] pH Test
[0126] Before testing, plug in the pH meter and preheat for 30 minutes. Weigh 5g of the sample to be tested into a clean 100mL beaker, and continue to add 45mL of deionized water to the beaker. When adding deionized water, stir with a glass rod to fully wet the sample. Place the beaker containing the sample mixture in an ultrasonic cleaner for 5 minutes, stir with a glass rod while ultrasonic treatment, then take it out and place it on the upper layer to clarify. Use a pH meter to measure the pH value of the clarified liquid on the sample mixture, and record the data. Parallel measurements are made three times to obtain the average value.
[0127] Button battery assembly
[0128] The negative electrode materials were mixed and coated in a mass ratio of 8:1:1 to obtain a negative electrode sheet. The negative electrode sheet, the positive electrode sheet and the electrolyte were assembled to obtain a CR2016 button battery, wherein the electrolyte used was 1 mol / L LiPF 6 EC+EMC+DMC (volume ratio of 1:1:1) solution.
[0129] Button Cell Battery Test
[0130] The lithium-ion battery charge and discharge test uses the Neware battery test system BTS-5V, 10mA, and the 50-week cycle capacity retention rate test is carried out at a constant temperature of 25°C and a 0.1C rate, with a voltage range of 0.005 to 1.5V.
[0131] The test results of the grain size, pH value and surface residual alkali of the negative electrode materials of the above embodiments and comparative examples, the slurry results of the negative electrode materials of the above embodiments and comparative examples, and the electrical test results of the button batteries assembled from the negative electrode materials of the above embodiments and comparative examples are shown in Table 2.
[0132] Table 2
[0133]
[0134]
[0135] Figure 1 This is the SEM image of the negative electrode material in Example 1 of the present application. It can be found from the SEM image that the particle size of the negative electrode material in Example 1 is relatively uniform. The reference ruler can estimate that the average particle size of the particles is about 9μm, and the surface of the material is relatively flat.
[0136] Figure 2 This is the SEM image of the negative electrode material in Comparative Example 1 of the present application. Figure 2 It can be seen that there are many point-like particles on the surface of the material. This is because the lithium source reacts insufficiently or unevenly in the pre-lithiation process and the surface is not washed sufficiently in the subsequent treatment. There are a large amount of lithium carbonate and lithium hydroxide on the surface of the material, resulting in high residual alkali and pH value on the surface of the material. The residual alkali will react with the thickener and binder during the slurry mixing process, reducing the bonding performance, which not only affects the process stability of the material in the battery cell, but also reduces the cycle stability of the material.
[0137] Figure 3This is a first charge and discharge curve diagram of the negative electrode material in Example 1 and Comparative Example 1 of the present application at a current density of 0.1C. At a current density of 0.1C, the first discharge specific capacity of the material prepared in Example 1 is 1558.5mAh / g, the charging specific capacity is 1435.4mAh / g, the first coulombic efficiency is 92.1%, the discharge specific capacity at the 50th cycle is 1368.9mAh / g, and the capacity retention rate is 95.4%; the first discharge specific capacity of the material prepared in Comparative Example 1 is 1538.3mAh / g, the charging specific capacity is 1372.2mAh / g, the first coulombic efficiency is 89.2%, the discharge specific capacity at the 50th cycle is 1213mAh / g, and the capacity retention rate is 88.4%. The charge specific capacity, first efficiency, cycle stability and slurry stability of Comparative Example 1 are worse than those of the negative electrode material prepared in Example 1. At the same time, the discharge curve voltage (quasi-platform area) of Comparative Example 1 is lower than that of Example 1. This is because the degree of crystallization of silicon in the material of Comparative Example 1 is higher than that of Example 1, which ultimately affects the expansion and cycle of the material.
[0138] Figure 4 This is a first charge and discharge curve diagram of the negative electrode material in Example 1 and Comparative Example 2 of the present application at a current density of 0.1C. At a current density of 0.1C, the first discharge specific capacity of the material prepared in Example 1 is 1558.5mAh / g, the charging specific capacity is 1435.4mAh / g, the first coulombic efficiency is 92.1%, the discharge specific capacity at the 50th cycle is 1368.9mAh / g, and the capacity retention rate is 95.4%; the first discharge specific capacity of the material prepared in Comparative Example 2 is 1572.5mAh / g, the charging specific capacity is 1421.5mAh / g, the first coulombic efficiency is 90.4%, the discharge specific capacity at the 50th cycle is 1289.5mAh / g, and the capacity retention rate is 90.7%. The charging specific capacity, first efficiency, cycle stability and slurry stability of Comparative Example 2 are worse than those of the negative electrode material prepared in Example 1. At the same time, the discharge curve voltage (quasi-platform area) of Comparative Example 2 is lower than that of Example 1, and the delithiation voltage on the charging curve is higher than that of Example 2. This is because the reaction activity of the pre-lithiation agent n-butyl lithium used in the material of Comparative Example 1 is higher than that of sodium dihydrobis(2-methoxyethoxy)aluminate, resulting in the degree of crystallization of silicon in the material of Comparative Example 1 being higher than that of Example 1, which ultimately affects the expansion and circulation of the material.
[0139] Figure 5The performance diagram of the full battery of Example 1, Comparative Example 1, Comparative Example 2, and Example 5 mixed with graphite to 450mAh / g at a current density of 1C / 1C. The materials prepared in Example 1, Comparative Example 1, Comparative Example 2, and Example 5 were mixed with graphite to 450mAh / g as the negative electrode, and NCM811 was used as the positive electrode. The 10Ah soft-pack battery was assembled by slurry mixing, coating, rolling, slitting, die-cutting, lamination, welding of pole ears, top and side sealing, baking, and injection. After the capacity was divided, a normal temperature cycle test was carried out at a current density of 1C / 1C. At present, the full battery of Example 1 has been cycled for 400 weeks, and the capacity retention rate is 97.4%. The full battery of Comparative Example 1 has been cycled for 400 weeks, and the capacity retention rate is 89.6%. The full battery of Comparative Example 2 has been cycled for 400 weeks, and the capacity retention rate is 93%. The full battery of Example 5 has been cycled for 400 weeks, and the capacity retention rate is 95.9%. Comparing Example 1 with Comparative Example 1, it can be found that the 400-week cycle performance of the material in the full battery is improved by about 8%. This is because the pre-sodium solution adopted in Example 1 has good uniformity, and sodium dihydrogen bis(2-methoxyethoxy)aluminate can more effectively control the heat generated by the reaction than the commonly used lithium source pre-lithium, so the synthesized material has smaller grains and better structural stability; at the same time, the surface is coated with a "hard and flexible" conductive polymer, the residual alkali is low, the slurry stability and processing performance are good, so the cycle performance is good. Comparing Example 1 with Comparative Example 2, it can be found that the 400-week cycle performance of the material in the full battery is improved by about 4%. This is because the sodium dihydrogen bis(2-methoxyethoxy)aluminate adopted in Example 1 can more effectively control the heat generated by the reaction than the commonly used n-butyl lithium, so the synthesized material has smaller grains and better structural stability; at the same time, sodium aluminosilicate that is stable to water is formed inside the material during the high-temperature treatment process, so the material is stable during the homogenization process, and the binder and sodium carboxymethyl cellulose will not be denatured, so the cycle performance and processing performance are improved. Comparing Example 1 with Example 5, it can be found that the 400-cycle performance of the material in the full battery is improved by about 1.5%. This is because Example 5 does not add 3,4-ethylenedioxythiophene, and the surface polymer rigidity is poor, so the ability to inhibit the volume expansion of the material is reduced, resulting in a decrease in cycle performance. At the same time, the conductivity of the material surface is reduced, the polarization of the material becomes larger, and the cycle stability of the material is further reduced.
[0140] At a current density of 0.1C, the material prepared in Comparative Example 1 has a first charge specific capacity of 1372.2mAh / g, a first coulombic efficiency of 89.2%, a grain size of 5.4nm, a residual alkali of 350ppm, and a pH of 11.2. After 50 cycles, the specific capacity is 1213mAh / g, and the capacity retention rate is 88.4%. By comparing Example 1 with Comparative Example 1, it can be found that the material prepared by the present invention is superior to commercial materials in specific capacity, first efficiency, and cycle capacity retention rate, and the residual alkali and pH are lower. The slurry is basically not gasified after being left for 7 days, and the grains are smaller. This is because the present invention pre-sodiumizes the SiO material through the liquid phase and controls the three-stage sintering temperature, and the reaction is more uniform. Compared with the traditional medium / high temperature treatment, the reaction intensity can be effectively controlled, and the grain size of the single crystal silicon can be reduced, thereby reducing the expansion of the material and improving the cycle performance of the material. Secondly, sodium aluminosilicate is generated inside the material during the pre-sodium process, which can effectively buffer the expansion, and is stable to water, improves the storage performance of the material, and avoids water erosion during the homogenization process, reduces the risk of gas production, and improves the processing performance. Finally, the grafted copolymer coating layer formed by in situ polymerization on the surface of the material, which is composed of poly (3,4-ethylenedioxythiophene) as a side chain segment grafted onto the main chain of the polyvinyl alcohol molecule, can effectively improve the electronic conductivity and interface properties of the material. At the same time, the conductive polymer has both the rigidity of the poly (3,4-ethylenedioxythiophene) side chain segment and the flexibility of the polyvinyl alcohol main chain, which can effectively buffer the volume expansion of the material during charging and discharging, maintain the interface stability between the material and the electrode, and thus improve the cycle performance.
[0141] By comparing Example 1 with Comparative Example 2, it can be found that the material of the present invention has advantages in first effect, circulation, residual alkali, grain and improved gas production. This is because although Comparative Example 2 uses n-butyl lithium for pre-lithiation to improve the first effect, it does not use sodium dihydrogen bis(2-methoxyethoxy)aluminate, so sodium aluminosilicate cannot be formed, resulting in the inability to avoid water vapor or water erosion during storage and homogenization, and then gas production. At the same time, the activity of n-butyl lithium is also higher than that of sodium dihydrogen bis(2-methoxyethoxy)aluminate, so the grain is also low during the pre-lithiation process. The combination of various factors leads to the cycle performance being inferior to that of Example 1.
[0142] By comparing Example 1 with Comparative Example 3, it can be found that Example 1 has a higher initial efficiency and a better cycle. This is because Example 1 uses sodium dihydrobis(2-methoxyethoxy)aluminate to pre-sodiumize the material, resulting in a high initial efficiency. During the pre-sodiumization, sodium aluminosilicate is generated for buffer expansion, resulting in a better cycle.
[0143] By comparing Example 1 with Example 5 and Example 6, it can be found that Example 1 has a higher first efficiency and a better cycle. This is because the material prepared in Example 1 can take into account the rigidity of the poly (3,4-ethylenedioxythiophene) side chain segments and the flexibility of the polyvinyl alcohol molecular main chain, which not only has a stronger ability to resist the volume expansion of the material, but also can maintain the structural stability and interface stability of the material while the material expands, so the material has better cycle performance.
[0144] Based on the above, the performance of the material prepared in Example 1 is better through the above steps and the raw materials and proportions used.
[0145] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0146] The single crystal silicon in the negative electrode material is embedded in the sodium aluminosilicate core. On the one hand, the presence of the sodium aluminosilicate core helps to reduce the volume expansion of the single crystal silicon during the charge and discharge process; on the other hand, the single crystal silicon is a single silicon substance and is easy to react with water. Since the sodium aluminosilicate core can exist stably in water, the sodium aluminosilicate core can prevent the direct contact between the single crystal silicon and water, thereby helping to reduce the erosion of water on the single crystal silicon during the slurry process, and further solves the problem that the silicon-based negative electrode material is easy to react with water during the slurry process. In addition, the carbon coating layer in the negative electrode material is coated on the surface of the sodium aluminosilicate core, which helps to improve the conductivity and structural stability of the negative electrode material. Combining the above favorable factors, the negative electrode material of the present application has the characteristics of high initial efficiency, good cycle performance and good rate performance.
[0147] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A negative electrode material, It is characterized in that The negative electrode material comprises single crystal silicon, a sodium aluminosilicate core and a coating layer, wherein the single crystal silicon is embedded in the sodium aluminosilicate core, and the coating layer comprises a carbon coating layer, and the carbon coating layer is coated on the surface of the sodium aluminosilicate core.
2. The negative electrode material according to claim 1, It is characterized in that The thickness of the carbon coating layer is 10 to 100 nm; And / or, the coating layer also includes a graft copolymer coating layer formed by grafting poly 3,4-ethylenedioxythiophene as a branched chain segment onto the main chain of a polyvinyl alcohol molecule, and the graft copolymer coating layer is arranged on the outer surface of the carbon coating layer, and / or, the thickness of the graft copolymer coating layer is 5nm to 50nm; and / or, the mass ratio of the single crystal silicon, the sodium aluminosilicate core, the carbon coating layer and the graft copolymer coating layer is 33 to 44:46 to 57:3 to 5:2 to 5; and / or, the grain size of the single crystal silicon is 0.5nm to 5nm; And / or, the mass ratio of the polyvinyl alcohol main chain to the poly (3,4-ethylenedioxythiophene) side chain segments in the graft copolymer coating layer is 9 to 99:
1.
3. The negative electrode material according to claim 1 or 2, It is characterized in that The pH value of the negative electrode material is 7.5 to 10; and / or the residual alkali content on the surface of the negative electrode material is 20 to 150 ppm; and / or the powder resistivity of the negative electrode material is 0.5 Ω·cm to 1 Ω·cm.
4. A method for preparing the negative electrode material according to any one of claims 1 to 3, It is characterized in that The preparation method comprises: Step S1, sintering a raw material including SiO and a carbon source in a first inert atmosphere to obtain carbon-coated SiO; Step S2, mixing the raw materials including the carbon-coated SiO2, sodium dihydrogen bis(2-methoxyethoxy)aluminate, and an organic solvent in a second inert atmosphere, and then sequentially performing a pre-sodium reaction and solid-liquid separation to obtain pre-sodium carbon-coated SiO2; Step S3, calcining the pre-sodium carbon-coated SiO in a third inert atmosphere to obtain the negative electrode material; Wherein, the mass ratio of the sodium dihydrogen bis(2-methoxyethoxy)aluminate to the carbon-coated SiO is 5:3 to 25:32; During the calcination process, the temperature of the calcination process is gradually increased.
5. The preparation method according to claim 4, It is characterized in that In the step S2, the mass ratio of the sodium dihydrobis(2-methoxyethoxy)aluminate to the organic solvent is 2-4:6-8; and / or, the temperature of the pre-sodium reaction is 40-60° C.; and / or the insulation time of the pre-sodium reaction is 4-8 h; And / or, the second inert atmosphere is selected from any one or more of helium, neon and argon; And / or, the organic solvent is a benzene organic solvent, preferably the benzene organic solvent is benzene and / or toluene; And / or, the solid-liquid separation is a process of removing the solvent by evaporation, and the evaporation temperature is 100-150°C.
6. The preparation method according to claim 4 or 5, It is characterized in that In the step S1, the temperature of the sintering treatment is 600°C to 800°C; and / or the holding time of the sintering treatment is 1h to 6h; preferably, the sintering treatment is performed in a first kiln, and the rotation speed of the first kiln is 0.25r / min to 2r / min; And / or, the carbon source is an organic hydrocarbon gas, preferably the organic hydrocarbon gas is selected from any one or more of alkanes, alkenes, and alkynes; further, preferably the organic hydrocarbon gas is selected from any one or more of methane, ethylene, and acetylene; and / or, the volume ratio of the first inert atmosphere to the carbon source is 1 to 4:1; and / or, the total flow rate of the first inert atmosphere and the carbon source is 80 L / h to 200 L / h; And / or, the first inert atmosphere is selected from any one or more of nitrogen, helium, neon and argon.
7. The preparation method according to any one of claims 4 to 6, It is characterized in that In the step S3, the calcination treatment includes a first calcination treatment, a second calcination treatment and a third calcination treatment performed sequentially; and / or, the temperature of the first calcination treatment is 200° C. to 400° C.; and / or, the holding time of the first calcination treatment is 8 h to 24 h; and / or, the heating rate of the first calcination treatment is 1° C. / min to 3° C. / min; and / or, the temperature of the second calcination treatment is 450°C to 700°C; and / or, the holding time of the second calcination treatment is 8h to 24h; and / or, the heating rate of the second calcination treatment is 1°C / min to 3°C / min; and / or, the temperature of the third calcination treatment is 750° C. to 900° C.; and / or, the holding time of the third calcination treatment is 2 h to 8 h; and / or, the heating rate of the third calcination treatment is 1° C. / min to 3° C. / min; Preferably, the calcination treatment is carried out in a second kiln, and the rotation speed of the second kiln is 2.5 r / min to 5 r / min; And / or, the third inert atmosphere is selected from any one or more of helium, neon and argon.
8. The preparation method according to any one of claims 4 to 7, It is characterized in that The preparation method further comprises: Step S4, sequentially subjecting a reaction system comprising the product after the calcination treatment in step S3, polyvinyl alcohol, 3,4-ethylenedioxythiophene, a grafting agent, a solvent, acetylacetone and hydrogen peroxide to a polymerization reaction and a high-temperature treatment to obtain the negative electrode material; Preferably, the molecular weight of the polyvinyl alcohol is 25000-120000, and / or the mass ratio of the polyvinyl alcohol to the 3,4-ethylenedioxythiophene is 8-100:1; and / or the mass ratio of the grafting agent to the 3,4-ethylenedioxythiophene is 0.2-1:1; and / or the mass ratio of the product after calcination in step S3 to the polyvinyl alcohol is 95:99-1:5; and / or the mass ratio of the hydrogen peroxide to the 3,4-ethylenedioxythiophene is 1:2-4; and / or, the pH value of the reaction system is 3 to 5, and / or the mass ratio of the acetylacetone to the 3,4-ethylenedioxythiophene is 1 to 2:1; and / or, the polymerization reaction temperature is 10° C. to 40° C., and / or the polymerization reaction time is 2 h to 8 h; And / or, the temperature of the high temperature treatment is 60-80°C, and / or the time of the high temperature treatment is 8-24h; And / or, the grafting agent is 3-boric acid thiophene; And / or, the solvent is dimethyl sulfoxide.
9. A negative electrode sheet, It is characterized in that The negative electrode sheet contains the negative electrode material according to any one of claims 1 to 3.
10. A lithium ion battery comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, It is characterized in that The negative electrode sheet is the negative electrode sheet according to claim 9.
Citation Information
Patent Citations
Porous silicon-based alloy composite
CN106058167A
Nanometer porous silicon-based compound electrode material and preparation method thereof
CN108110240A
Lithium ion battery negative electrode material and preparation method thereof
CN112234174A
Electrode additive, preparation method thereof and positive plate
CN114649529A
Carbon-coated silicon-carbon composite material as well as preparation method and application thereof
CN116885126A
Cited By
Composite negative electrode material, preparation method thereof, negative electrode plate applying composite negative electrode material and lithium battery
CN119742333A