Positive electrode active material and preparation method thereof, positive electrode plate and battery
Patent Information
- Application Number
- CN202411218264.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-30
AI Technical Summary
但是,磷酸铁锂材料会发生铁溶出,降低电池的循环性能
[0068] (1) In the process of preparing the cathode active material, by selecting a suitable P/Fe iron phosphate precursor, reduce the content of P element in the slurry, reduce the generation of pyrophosphate during high-temperature sintering, and reduce the impact of pyrophosphate on Li consumption, reducing Li in the cathode active material 4 P 2 O 7 content, reducing iron dissolution, thereby improving battery capacity and cycle performance.
Smart Images

Figure CN118970011A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and in particular, to positive electrode active materials and preparation methods thereof, positive electrode plates and batteries. Background Art
[0002] Lithium-ion batteries have attracted much attention due to their high theoretical capacity (170mAh / g), good stability, high safety, and environmental friendliness. They have been widely used in energy storage, power tools, electric vehicles, military equipment, aerospace, and other fields. With the application of energy storage, long-life lithium-ion batteries have become a research hotspot in the battery field in recent years. New energy storage systems have high requirements for the service life of lithium-ion batteries. Usually, household energy storage systems require the service life of lithium-ion batteries to be more than 3,000 times, commercial energy storage systems require the service life of lithium-ion batteries to be more than 6,000 times, and large-scale energy storage systems require the service life of lithium-ion batteries to be more than 10,000 times. Among different types of lithium-ion batteries, olivine-structured lithium iron phosphate materials are a research hotspot due to their good safety, low cost, and long cycle performance. However, lithium iron phosphate materials will cause iron dissolution, which reduces the cycle performance of the battery. Summary of the invention
[0003] The present invention aims to solve one of the technical problems in the related art at least to a certain extent.
[0004] In a first aspect, the present application provides a positive electrode active material, wherein the positive electrode active material comprises Li y Fe a M b PO4, wherein 0.95≤a≤0.99, 0.001≤b≤0.1, 1≤y≤1.08, M includes at least one of Ti, Na, K, Mg, V, W, Nb, La, Cr, Mo, Ca, Zn, Y, Zr, Sm, Co, Ni, B, Cu, and Gd, and the positive electrode active material includes Li4P2O7, and the mass proportion of the Li4P2O7 based on the total mass of the positive electrode active material is less than or equal to 0.3%. Thus, the content of Li4P2O7 in the positive electrode active material is reduced, the iron dissolution is reduced, and the cycle performance of the battery is improved.
[0005] According to some embodiments of the present application, the positive electrode active material is compacted using a pressure i, and the specific surface area of the positive electrode active material before compaction is SSA0, and the specific surface area of the positive electrode active material after compaction is SSA i , and satisfies: 0<(SSA i -SSA0) / SSA0≤(7.07ln(i)-5.9) / 100, where 6T≤i≤12T. Thus, after the positive electrode active material is compacted with different pressures, the specific surface area increase rate ((SSAi -SSA0) / SSA0) is small, indicating that the number of large particles in the positive electrode active material is small, which can reduce the risk of cracking of the positive electrode active material during battery cycling, reduce iron dissolution, and improve the capacity and cycle performance of the battery.
[0006] According to some embodiments of the present application, the positive electrode active material satisfies at least one of the following conditions: under the condition of i=6T, (SSA 6T -SSA0) / SSA0≤6.5%; Under the condition of i=9T, (SSA 9T -SSA0) / SSA0≤9%; Under the condition of i=12T, (SSA 12T -SSA0) / SSA0≤11%. Thus, the specific surface area increase rate of the positive electrode active material under different pressures is reduced, the risk of cracking of the positive electrode active material during battery cycling is reduced, iron dissolution is reduced, and the capacity and cycle performance of the battery are improved.
[0007] According to some embodiments of the present application, K 95 =(Dv 95 -Dv5) / Dv 50 , and satisfy 0.1≤K 95 ≤7, optional 1≤K 95 ≤5, wherein Dv5 is the particle size corresponding to the particle size distribution percentage of the positive electrode active material reaching 5%, Dv 50 Dv is the particle size corresponding to the positive electrode active material particle size volume distribution percentage reaching 50%, 95 The particle size corresponding to the positive electrode active material particle size volume distribution percentage reaches 95%. Thus, the uniformity of the positive electrode active material particles is improved, the risk of cracking of the positive electrode active material during battery cycling is reduced, iron dissolution is reduced, and the battery cycle performance is improved.
[0008] According to some embodiments of the present application, the iron dissolution in the positive electrode active material is less than or equal to 300 ppm, and optionally, the iron dissolution in the positive electrode active material is less than or equal to 150 ppm. Thus, the structural stability of the positive electrode active material is improved during the battery cycle, and the capacity and cycle performance of the battery are improved.
[0009] According to some embodiments of the present application, the positive electrode active material satisfies at least one of the following conditions: under a pressure of 3T, the compaction density of the positive electrode active material is 2.3 g / cm 3 -2.6g / cm 3 The resistance of the positive electrode active material is 1Ω·cm-20Ω·cm. Thus, the energy density and rate performance of the battery are improved.
[0010] According to some embodiments of the present application, at least part of the surface of the positive electrode active material has a carbon coating layer, thereby improving the electronic conductivity of the positive electrode sheet.
[0011] The second aspect of the present application provides a method for preparing the positive electrode active material provided in the first aspect of the present application, the method comprising: mixing a Li source, a P source, an Fe source, an M source, and a solvent to obtain a slurry, wherein the molar ratio of the P element in the P source to the Fe element in the Fe source is less than or equal to 1.053, grinding and drying the slurry to obtain precursor particles; sintering the precursor particles for the first time and the second time in sequence, wherein the temperature of the first sintering is T1, the temperature of the second sintering is T2, T1<T2, and crushing to obtain the positive electrode active material. Thus, by controlling the molar ratio of the P element and the Fe element, the probability of generating pyrophosphate is reduced during the sintering process, the content of Li4P2O7 in the positive electrode active material is reduced, and the iron dissolution is reduced, thereby improving the cycle performance and capacity of the battery.
[0012] According to some embodiments of the present application, the molar ratio of the P element in the P source to the Fe element in the Fe source is 1.015-1.045. Thus, the content of Li4P2O7 in the positive electrode active material is reduced, thereby reducing iron dissolution and improving the cycle performance and capacity of the battery.
[0013] According to some embodiments of the present application, the first sintering satisfies at least one of the following conditions: 300≤T1≤500℃; the holding time of the first sintering is t1, and satisfies 1h≤t1≤7h, optionally, 3h≤t1≤5h; the heating rate of heating the precursor particles to T1 is 2℃ / min-3℃ / min. Thus, by making the temperature, heating rate and holding time of the first sintering within this range, the crystallization process is better controlled to form a positive electrode active material with uniform particle distribution.
[0014] According to some embodiments of the present application, the second sintering satisfies at least one of the following conditions: 700≤T2≤900℃; the holding time of the second sintering is t2, and satisfies 5h≤t2≤15h, optionally, 7h≤t2≤10h; the heating rate from T1 to T2 is 0.5℃ / min-3℃ / min. Thus, by making the temperature, heating rate and holding time of the second sintering within the above range, the crystallization effect is improved, the number of large particles in the positive electrode active material is reduced, and the uniformity of the particles is improved.
[0015] According to some embodiments of the present application, the method further comprises: mixing the Li source, the P source, the Fe source, the M source, the carbon source, and the solvent, thereby improving the electronic conductivity of the positive electrode active material.
[0016] According to some embodiments of the present application, the method satisfies at least one of the following conditions: the Li source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium oxalate, and lithium nitrate; the carbon source includes at least one of glucose, sucrose, starch, cellulose, citric acid, oxalic acid, polyethylene glycol, polyvinyl alcohol, and polyethylene; the P source and the Fe source include iron phosphate; and the M source includes an oxide of M.
[0017] The third aspect of the present application provides a positive electrode plate, which includes the positive electrode active material provided in the first aspect of the present application or the positive electrode active material prepared by the method provided in the second aspect of the present application.
[0018] The fourth aspect of the present application provides a battery, comprising the positive electrode sheet provided in the third aspect of the present application. Thus, the battery has excellent cycle performance and high capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0020] Figure 1 A schematic flow chart of a method for preparing a positive electrode active material according to an embodiment of the present application is shown.
[0021] Figure 2 The XRD pattern of lithium iron phosphate prepared in Example 2 of the present application is shown.
[0022] Figure 3 The SEM image of the lithium iron phosphate prepared in Example 2 of the present application is shown. DETAILED DESCRIPTION
[0023] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0024] The quality of positive electrode active materials directly affects various performance indicators of lithium batteries as they are the key to further improving battery performance. During the long-term circulation and storage of olivine structure positive electrode materials, iron dissolution will occur, and the dissolved iron ions will migrate to the surface of the negative electrode and deposit, accelerating the decomposition reaction of the electrolyte. Iron dissolution has an adverse effect on the performance of both the positive and negative electrodes and the electrolyte, exacerbating the capacity decay of the olivine structure positive electrode active materials and reducing the cycle performance of the battery.
[0025] The present application proposes a positive electrode active material, wherein the positive electrode active material comprises Li y Fe a M b PO4, wherein 0.95≤a≤0.99, 0.001≤b≤0.1, 1≤y≤1.08, M includes at least one of Ti, Na, K, Mg, V, W, Nb, La, Cr, Mo, Ca, Zn, Y, Zr, Sm, Co, Ni, B, Cu, and Gd, and the positive electrode active material includes Li4P2O7, and the mass proportion of the Li4P2O7 based on the total mass of the positive electrode active material is less than or equal to 0.3%. Thus, the content of Li4P2O7 in the positive electrode active material is reduced, the iron dissolution is reduced, and the capacity and cycle performance of the battery are improved.
[0026] According to some embodiments of the present application, the mass proportion of Li4P2O7 is less than or equal to 0.3%, for example, it can be 0.05%, 0.1%, 0.15%, 0.2%, 0.25% or 0.3%, or it can be a range composed of any of the above values. Thus, the content of Li4P2O7 in the positive electrode active material is reduced, the consumption of Li by pyrophosphate is reduced, the structural stability of the lithium iron phosphate material is improved, and the iron dissolution is reduced.
[0027] According to some embodiments of the present application, the positive electrode active material is compacted using a pressure i, and the specific surface area of the positive electrode active material before compaction is SSA0, and the specific surface area of the positive electrode active material after compaction is SSA i , and satisfies: 0<(SSA i -SSA0) / SSA0≤(7.07ln(i)-5.9) / 100, where 6T≤i≤12T. i -SSA0) / SSA0 is within the above range, after the positive electrode active material is compacted with different pressures i, the increase rate of specific surface area of the positive electrode active material is small, indicating that the number of cracked particles in the positive electrode active material is small and the particle uniformity is good. During the battery cycle, the structural stability of the positive electrode active material can be improved, the risk of cracking of the positive electrode active material can be reduced, and iron dissolution can be reduced, thereby reducing the attenuation of the capacity of the positive electrode active material, reducing the influence of iron dissolution on the positive and negative electrodes and the electrolyte, and improving the cycle performance and capacity of the battery.
[0028] In this application, the specific surface area of the positive electrode active material can be tested by BET, using the nitrogen adsorption method and a Micromeritics Tristar II 3030 machine to measure the total surface area of all particles in each gram of the positive electrode active material. The unit is: m 2Specifically, the specific surface area SSA0 of the positive electrode active material before compaction is first tested, and then the positive electrode active material is compacted with pressure i, ground and sieved, and the specific surface area SSA of the positive electrode active material under the sieve is tested. i .
[0029] As an example, i may be 6T, 8T, 10T or 12T, etc., or may be a range consisting of any of the above values.
[0030] According to some embodiments of the present application, under the condition of i=6T, (SSA 6T -SSA0) / SSA0≤6.5%, for example, it can be 1.5%, 2.5%, 3.5%, 4.5%, 5.5% or 6.5%, or it can be a range composed of any of the above values. Therefore, after compaction with a pressure of 6T, the increase rate of the specific surface area of the positive electrode active material is small, indicating that the positive electrode active material particles are evenly distributed, and the risk of cracking of the particles can be reduced during the battery cycle, and the iron dissolution is reduced, thereby improving the capacity and cycle performance of the battery.
[0031] According to some embodiments of the present application, under the condition of i=9T, (SSA 9T -SSA0) / SSA0≤9%, for example, it can be 2%, 4%, 6%, 8% or 9%, or can be a range composed of any of the above values. Therefore, after compaction with a pressure of 9T, the increase rate of the specific surface area of the positive electrode active material is small, indicating that the positive electrode active material particles are evenly distributed, and the risk of particle cracking can be reduced during the battery cycle, reducing iron dissolution, thereby improving the capacity and cycle performance of the battery.
[0032] According to some embodiments of the present application, under the condition of i=12T, (SSA 12T -SSA0) / SSA0≤11%, for example, (SSA 12T -SSA0) / SSA0 can be 3%, 5%, 7%, 9% or 11%, etc., or can be a range composed of any of the above values. Therefore, after compaction with a pressure of 12T, the specific surface area increase rate of the positive electrode active material is small, indicating that the positive electrode active material particles are evenly distributed, and the risk of particle cracking can be reduced during the battery cycle, reducing iron dissolution, thereby improving the battery capacity and cycle performance.
[0033] It can be seen from this that the positive electrode active material proposed in this application has a specific surface area increase rate (SSA i -SSA0) / SSA0) are both small, indicating that the positive electrode active material particles are evenly distributed, which can reduce the risk of particle cracking during battery cycling and reduce iron dissolution, thereby improving the battery capacity and cycle performance.
[0034] According to some embodiments of the present application, the K of the positive electrode active material 95 =(Dv 95 -Dv5) / Dv 50 , and satisfy 0.1≤K 95 ≤7, wherein Dv5 is the particle size corresponding to the particle size distribution percentage of the positive electrode active material reaching 5%, Dv 50 Dv is the particle size corresponding to the positive electrode active material particle size volume distribution percentage reaching 50%, 95 is the particle size corresponding to the positive electrode active material particle size volume distribution percentage reaching 95%. 95 It can be 0.1, 1, 3, 4, 5, 6 or 7, or can be a range of any of the above values. As a result, the uniformity of the positive electrode active material particles is good, the difference in particle size between particles is small, and the risk of cracking of the positive electrode active material during battery cycling can be reduced, reducing iron dissolution, thereby improving the capacity and cycle performance of the battery. According to some specific embodiments of the present application, 4.5≤K 95 ≤6.
[0035] As an example, the Dv of the positive electrode active material 50 The thickness may be 0.55 μm to 0.75 μm, for example, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm or 0.75 μm, or may be within a range consisting of any of the above values.
[0036] As an example, the Dv5 of the positive electrode active material may be 0.25 μm-0.35 μm, for example, 0.25 μm, 0.27 μm, 0.29 μm, 0.31 μm, 0.33 μm or 0.35 μm, or a range consisting of any of the above values.
[0037] As an example, the Dv of the positive electrode active material 95 The thickness may be 3 μm to 7 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm or 7 μm, or may be within a range consisting of any of the above values.
[0038] Thus, by making Dv 50 , Dv5, Dv 95 In the above range, the K of the positive electrode active material is regulated 95 , thereby improving the particle uniformity of the lithium iron phosphate material. During the battery cycle, the risk of cracking of the lithium iron phosphate material can be reduced, and iron dissolution can be reduced, thereby improving the capacity and cycle performance of the battery.
[0039] According to some embodiments of the present application, the iron dissolution of the positive electrode active material is less than or equal to 300ppm. As a result, the iron dissolution of the positive electrode active material is less, which can reduce the attenuation of the capacity of the positive electrode active material; during the battery cycle, the risk of iron dissolution and deposition at the negative electrode can be reduced, and the decomposition of the electrolyte can be reduced, thereby improving the cycle performance and capacity of the battery. According to some specific embodiments of the present application, the iron dissolution of the positive electrode active material is less than or equal to 150ppm.
[0040] According to some embodiments of the present application, under a pressure of 3T, the compaction density of the positive electrode active material can be 2.3 g / cm 3 -2.6g / cm 3 , for example, can be 2.3 g / cm 3 , 2.35g / cm 3 , 2.4g / cm 3 , 2.45g / cm 3 , 2.5g / cm 3 , 2.55g / cm 3 or 2.6g / cm 3 The energy density of the battery is thereby increased.
[0041] According to some embodiments of the present application, the resistance of the positive electrode active material is 1Ω·cm-20Ω·cm, for example, 1Ω·cm, 5Ω·cm, 10Ω·cm, 15Ω·cm or 20Ω·cm, or a range of any of the above values. Thus, the lithium ion migration efficiency is improved and the rate performance of the battery is improved.
[0042] According to some embodiments of the present application, at least part of the surface of the positive electrode active material has a carbon coating layer, thereby improving the electronic conductivity of the positive electrode sheet.
[0043] The second aspect of the present application provides a method for preparing the positive electrode active material provided in the first aspect of the present application, the method comprising: mixing a Li source, a P source, an Fe source, an M source, and a solvent to obtain a slurry, wherein the molar ratio of the P element in the P source to the Fe element in the Fe source is less than or equal to 1.053, grinding and drying the slurry to obtain precursor particles; sequentially performing a first sintering and a second sintering on the precursor particles, the temperature of the first sintering is T1, the temperature of the second sintering is T2, T1<T2, and crushing to obtain the positive electrode active material.
[0044] The method for preparing positive electrode active materials proposed in the present application can reduce the generation of pyrophosphate during sintering by controlling the molar ratio of P element and Fe element, reduce the consumption of Li by pyrophosphate, reduce iron dissolution, and thus reduce the capacity loss of positive electrode active materials, reduce the influence of iron dissolution on positive and negative electrodes and electrolyte, and improve the cycle performance and capacity of the battery.
[0045] The method for preparing the positive electrode active material proposed in this application is described in detail below. Figure 1 , the method comprising:
[0046] S10: Mixing a Li source, a P source, a Fe source, a M source, and a solvent to obtain a slurry, and grinding and drying the slurry to obtain precursor particles.
[0047] According to some embodiments of the present application, the Li source, the P source, the Fe source, the M source, the carbon source, and the solvent are mixed. Thus, in the process of preparing lithium iron phosphate, the temperature of the first sintering is the temperature at which the carbon source is cracked, and the carbon source can be fully carbonized after the first sintering, thereby forming a uniform carbon coating layer on the surface of the lithium iron phosphate, further improving the uniformity of the carbon coating layer and improving the electronic conductivity of the positive electrode sheet.
[0048] According to some embodiments of the present application, the carbon source includes at least one of glucose, sucrose, starch, cellulose, citric acid, oxalic acid, polyethylene glycol, polyvinyl alcohol, and polyethylene.
[0049] According to some embodiments of the present application, anhydrous ferric phosphate, the Li source, the M source, the carbon source, and a solvent are mixed.
[0050] According to some embodiments of the present application, the Dv of the anhydrous ferric phosphate is 50 The thickness may be 1 μm to 5 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm, or may be within a range consisting of any of the above values.
[0051] As an example, the Li source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium oxalate, and lithium nitrate.
[0052] As an example, the P source and the Fe source include iron phosphate.
[0053] As an example, the M source includes an M oxide.
[0054] According to some embodiments of the present application, the molar ratio of the P element in the P source to the Fe element in the Fe source can be 1.010, 1.015, 1.020, 1.025, 1.030, 1.035, 1.040, 1.045 or 1.053, etc., or can be a range composed of any of the above numerical values. Thus, by making the molar ratio of the P element and the Fe element in the above range, the content of the P element in the material is reduced, the generation of pyrophosphate is reduced during high-temperature sintering, the consumption of pyrophosphate for Li is reduced, and the dissolution of iron is reduced, thereby improving the capacity and cycle performance of the battery. At the same time, by making the molar ratio of the P element and the Fe element in the above range, the crystallization performance of the particles can also be improved during high-temperature sintering, and the compaction density of the positive electrode active material can be improved. According to some specific embodiments of the present application, the molar ratio of the P element in the P source to the Fe element in the Fe source is 1.015-1.045.
[0055] According to some embodiments of the present application, the grinding method may include: coarse grinding the slurry, the zirconium ball size is 0.7mm-0.8mm, the coarse grinding time is 0.5h-1h, and the Dv of the particles in the slurry after coarse grinding is 50 The slurry is finely ground, the zirconium ball size is 0.3mm-0.4mm, the fine grinding time is 1h-5h, and the Dv of the slurry after fine grinding 50 It can be 0.2 μm-0.6 μm. Thus, the particle size of the particles in the slurry is reduced and the crystallization performance is improved.
[0056] According to some embodiments of the present application, the drying method may include spray drying the finely ground slurry, with an atomization frequency of 20 Hz-70 Hz, a heated air inlet temperature of 100°C-300°C, and an outlet temperature of 50°C-150°C.
[0057] S20: performing a first sintering and a second sintering on the precursor particles in sequence
[0058] According to some embodiments of the present application, the precursor particles are subjected to a first sintering and a second sintering in sequence, the temperature of the first sintering is T1, the temperature of the second sintering is T2, T1<T2, and are crushed to obtain the positive electrode active material.
[0059] According to some embodiments of the present application, 300≤T1≤500°C, for example, it can be 300°C, 340°C, 380°C, 420°C, 460°C or 500°C, etc., or can be a range consisting of any of the above numerical values.
[0060] The method for preparing positive electrode active materials proposed in the present application can better control the growth process of particles, improve the crystallinity of positive electrode active materials, and make the reaction more complete by adding a first sintering step, and the temperature of the first sintering is 300°C-500°C. After the prepared positive electrode active materials are compacted with different pressures, the increase rate of specific surface area of the positive electrode active materials is small, indicating that the particles of the positive electrode active materials are evenly distributed. During the battery cycle, the risk of particle cracking can be reduced, iron dissolution can be reduced, and the side reactions of the electrolyte can be reduced, thereby improving the cycle performance and capacity of the battery.
[0061] According to some embodiments of the present application, the precursor particles are sequentially sintered for the first time and for the second time in an atmosphere of a protective gas, wherein the protective gas includes at least one of nitrogen and an inert gas.
[0062] According to some embodiments of the present application, the holding time of the first sintering is t1, and satisfies 1h≤t1≤7h, for example, it can be 1h, 2h, 3h, 4h, 5h, 6h or 7h, or it can be a range composed of any of the above values. Thus, by making the holding time of the first sintering within this range, the crystallization process is better controlled to form a positive electrode active material with uniform particle distribution. According to some specific embodiments of the present application, 3h≤t1≤5h.
[0063] According to some embodiments of the present application, the heating rate of the precursor particles to T1 is 2°C / min-3°C / min, for example, 2°C / min, 2.2°C / min, 2.4°C / min, 2.6°C / min, 2.8°C / min or 3°C / min, or a range of any of the above values. Thus, by making the heating rate of the first sintering within this range, the crystallization process is better controlled to form a positive electrode active material with uniform particle distribution.
[0064] According to some embodiments of the present application, 700 ≤ T2 ≤ 900°C, for example, it can be 700°C, 800°C or 900°C, or it can be a range of any of the above values. Thus, the reaction is more complete, the crystallization is better, and the compaction density of the positive electrode active material is increased.
[0065] According to some embodiments of the present application, the heating rate from T1 to T2 is 0.5°C / min-3°C / min, for example, 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min or 3°C / min, or a range of any of the above values. Thus, the reaction is more fully carried out, the crystallization is better, and the compaction density of the positive electrode active material is increased.
[0066] According to some embodiments of the present application, the holding time of the second sintering is t2, and satisfies 5h≤t2≤15h, for example, it can be 5h, 7h, 9h, 11h, 13h or 15h, or can be a range of any of the above values. According to some specific embodiments of the present application, 7h≤t2≤10h.
[0067] In summary, the positive electrode active material and the preparation method thereof proposed in this application have the following advantages:
[0068] (1) In the process of preparing the positive electrode active material, by selecting a suitable P / Fe iron phosphate precursor, the content of P element in the slurry is reduced, the generation of pyrophosphate is reduced during high-temperature sintering, the consumption of Li by pyrophosphate is reduced, the content of Li4P2O7 in the positive electrode active material is reduced, and the iron dissolution is reduced, thereby improving the capacity and cycle performance of the battery.
[0069] (2) After compaction with different pressures i, the increase rate of the specific surface area of the positive electrode active material is small, indicating that the positive electrode active material particles are evenly distributed. During the battery cycle, the probability of cracking of the positive electrode active material particles can be reduced, the iron dissolution can be reduced, and the capacity and cycle performance of the battery can be improved.
[0070] (3) In the process of preparing positive electrode active materials, adding the first sintering process can better control the crystallization process, improve the uniformity of the positive electrode active material particles, reduce the probability of cracking of the positive electrode active material particles during battery cycling, reduce iron dissolution, and improve the capacity and cycle performance of the battery.
[0071] The third aspect of the present application provides a positive electrode plate, comprising the positive electrode active material provided in the first aspect of the present application or the positive electrode active material prepared by the method provided in the second aspect of the present application.
[0072] The fourth aspect of the present application provides a battery, comprising the positive electrode sheet provided in the third aspect of the present application. Therefore, the battery provided in the present application has a higher capacity and excellent cycle performance.
[0073] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.
[0074] Example 1
[0075] 1. Preparation of positive electrode active materials
[0076] Fe 0.99The iron phosphate precursor of PO4 (Fe source and P source), lithium carbonate (Li source), and titanium dioxide are mixed with pure water in a molar ratio of Li:Fe:Ti:P=1.03:0.99:0.008:1. Glucose accounts for 8.5% of the mass of the iron phosphate, polyethylene glycol accounts for 3% of the mass of the iron phosphate, and the solid content of the slurry is 48% to obtain the first slurry.
[0077] The slurry is coarsely ground, the zirconium ball size is 0.7mm-0.8mm, the coarse grinding time is 0.5h, and then ultra-finely ground, the zirconium ball size is 0.3mm-0.4mm, the fine grinding time is 2h, and the slurry particle size Dv 50 0.42μm;
[0078] The slurry was spray dried to obtain precursor particles, the atomization frequency was 20 Hz, the heating air inlet temperature was 120°C, and the air outlet temperature was 70°C;
[0079] The precursor particles were sintered in a nitrogen atmosphere. The sintering schedule was as follows: heating to 400°C at 2°C / min, keeping the temperature for 3h, heating to 800°C at 2°C / min, keeping the temperature for 8h, to obtain Li 1.03 Fe 0.99 Ti 0.008 PO4 positive electrode active material.
[0080] 2. Preparation of positive electrode sheet
[0081] The positive electrode active material Li 1.03 Fe 0.99 Ti 0.008 PO4, conductive agent carbon nanotubes, binder polyvinylidene fluoride (PVDF) are mixed with N-methylpyrrolidone (NMP) in a mass ratio of 92:5:3 to obtain a positive electrode slurry. The positive electrode slurry is evenly coated on the current collector aluminum foil, and then dried in a vacuum drying oven at 60°C for 20 hours. Then, it is stamped into a positive electrode sheet with a diameter of 11 mm and a thickness of 54 μm at a pressure of 100 MPa. The positive electrode sheet is placed in a vacuum drying oven at 120°C and dried for 12 hours.
[0082] 3. Negative electrode
[0083] The negative electrode is a metal lithium sheet with a diameter of 15.6 mm and a thickness of 0.45 mm.
[0084] 4. Isolation film
[0085] A polyethylene porous membrane with a thickness of 25 μm and coated with an alumina ceramic layer on its surface was used as the isolation membrane.
[0086] 5. Electrolyte
[0087] LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1, and the molar concentration of LiPF6 was 1 mol / L.
[0088] 6. Preparation of batteries
[0089] The positive electrode sheet, the separator, the negative electrode sheet and the electrolyte were assembled into a 2025 button cell in an Ar gas glove box with a water content and an oxygen content less than 5 ppm.
[0090] The preparation methods of lithium iron phosphate in Examples 2 to 15 and Comparative Example 1 are the same as those in Example 1, and the differences are detailed in Table 1.
[0091] Table 1
[0092]
[0093]
[0094] Performance Testing
[0095] 1. Specific surface area of positive electrode active material
[0096] The total surface area of all particles in each gram of positive electrode active material was measured using a Micromeritics Tristar II 3030 machine using the nitrogen adsorption method. The unit is: m 2 / g.
[0097] 2.Mass proportion of Li4P2O7
[0098] 1) dissolving the positive electrode active material in water, and filtering the obtained suspension to obtain a filtrate; 2) adjusting the pH of the filtrate to 11-13 with a standard alkali solution, and performing positive titration with a standard acid solution as an acid titrant to obtain a positive titration solution; the volume of the acid titrant consumed at the first hopping point and the second hopping point is respectively recorded as V 正1 mL and V 正2 mL; 3) cooling the positive titration solution to room temperature after heating, and back-titrifying with the alkali standard solution as the alkali titrant to obtain a back titration solution; respectively recording the volume of the alkali titrant consumed at the first jump point 'and the second jump point 'as V 反1 mL and V 反2 mL; 4) based on the amount of the acid titrant and the base titrant, determine the existence form and content of the residual pyrophosphate.
[0099] 3. Testing of Dv5, Dv50 and Dv95
[0100] The test was conducted by Malvern 3000 particle size analyzer, with a particle refractive index of 1.74, an absorptivity of 1, an ultrasonic intensity of 100%, and an ultrasonic test of 45S, in μm.
[0101] 4. Iron dissolution
[0102] 1) Place a 50ml beaker on a ten-thousandth electronic balance, reset it to zero, accurately weigh 5.0000±0.005g (target is close to 5.0000g) of lithium iron phosphate sample, then use a measuring cylinder to measure 50.0ml of pure water, pour it into the beaker, seal it with plastic wrap, shake it a few times by hand, and then leave it at room temperature for 70h;
[0103] 2) After the standing period, take a clean centrifuge tube and place 3 layers of medium-speed filter paper on it, pour the sample into the filter, and rinse the inner wall of the beaker with a wash bottle; 3) Assemble the filtration device with 3 layers of 0.22μm filter membrane, connect it to the vacuum pump, turn on the vacuum pump, pour the filtrate into the filtration cup for filtration, and thoroughly wash the centrifuge tube and the inner wall of the beaker with a wash bottle. After the filtration is complete, dilute all the filtrate into a 100ml volumetric flask, and then perform an inductively coupled plasma test (ICP test).
[0104] 5. Compacted density
[0105] UTM7305 compaction density meter, test value under test force 3T, unit: g / cm 3 。
[0106] 6. Resistance of positive electrode active material
[0107] D600 resistance meter, test pressure 1.57KN, test value under pressure holding 10S.
[0108] 7. Capacity retention rate
[0109] The prepared battery was subjected to a 200-cycle charge and discharge test under the conditions of 3.75V-2.0V, 45°C, and 1C charge and discharge to evaluate the battery's cycle performance.
[0110] 8. Discharge capacity
[0111] The prepared battery was tested at 3.75V~2.0V, 25°C, and 0.1C / 0.1C+1C / 1C charge and discharge to evaluate the discharge capacity of the battery.
[0112] 9. Scanning electron microscope test
[0113] The model of the scanning electron microscope used is S-4800 (manufacturer is Hitachi, Japan), and the testing conditions of the scanning electron microscope are: acceleration voltage is 1 kV, and magnification is 10K.
[0114] 10.XRD test
[0115] The model of the XRD diffractometer used is XRD-6000 X-ray powder diffractometer (Shimadzu, Japan), and the test conditions of XRD are: Cu target, Kα ray (wavelength λ=0.154nm), tube voltage of 40kV, tube current of 200mA, and scanning speed of 10°(2θ) / min.
[0116] The test results of the positive electrode active materials and the batteries in Examples 1 to 15 and Comparative Example 1 are shown in Tables 2 and 3.
[0117]
[0118]
[0119] It can be seen from the comparison between Examples 1 to 15 and Comparative Example 1 that the battery assembled from the positive electrode active material proposed in the present application has a higher discharge capacity and cycle capacity retention rate, indicating that by making the Li4P2O7 content in the positive electrode active material less than 0.3%, iron dissolution can be reduced and the capacity decay of the lithium iron phosphate material can be reduced. At the same time, due to the low iron dissolution, the impact on the electrolyte and the positive and negative electrodes can be reduced, thereby improving the cycle performance of the battery.
[0120] It can be seen from the comparison between Examples 1 to 4 and Comparative Example 1 that when preparing lithium iron phosphate, the P / Fe molar ratio is different and the content of Li4P2O7 in the lithium iron phosphate is different. By controlling the P / Fe molar ratio, a lithium iron phosphate material with high compaction density and low Li4P2O7 content can be obtained. The degree of iron dissolution is different. The less the content of Li4P2O7, the less iron is dissolved, and the better the discharge capacity and cycle performance of the battery.
[0121] It can be seen from Examples 5 to 8 that the temperature of the first sintering is different, and the specific surface area increase rate (SSA i -SSA0) / SSA0) is different. The smaller the specific surface area increase rate of lithium iron phosphate, the less iron dissolution, and the better the discharge capacity and cycle performance of the battery. This shows that the smaller the specific surface area increase rate of lithium iron phosphate, the better the uniformity of the particles, and the probability of cracking of lithium iron phosphate particles can be reduced during the battery cycle.
[0122] It can be seen from Example 2, Example 3, Example 6-Example 8 that when the lithium iron phosphate material simultaneously meets the following requirements: low Li4P2O7 content, small specific surface area increase rate, low iron dissolution, and the battery has a higher discharge capacity and cycle capacity retention rate.
[0123] It can be seen from Examples 9 to 12 that by controlling the heating rate and holding time during the first sintering, the generation of pyrophosphate can be reduced, the content of Li4P2O7 and iron dissolution can be reduced, and the discharge capacity and cycle performance of the battery can be improved.
[0124] It can be seen from Example 14 and Example 15 that by using different temperatures for the second sintering, batteries with high powder compaction density, high battery discharge capacity and good cycle performance can be obtained.
[0125] By the attached Figure 2 It can be seen that the material prepared in Example 2 is lithium iron phosphate material.
[0126] By the attached Figure 3 It can be seen that the lithium iron phosphate particles prepared in Example 2 are evenly distributed.
[0127] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A positive electrode active material, It is characterized in that Including Li y Fe a M b PO 4 , wherein 0.95≤a≤0.99, 0.001≤b≤0.1, 1≤y≤1.08, M includes at least one of Ti, Na, K, Mg, V, W, Nb, La, Cr, Mo, Ca, Zn, Y, Zr, Sm, Co, Ni, B, Cu, and Gd, and the positive electrode active material includes Li 4 P 2 O 7 , based on the total mass of the positive electrode active material, the Li 4 P 2 O 7 The mass proportion is less than or equal to 0.3%.
2. The positive electrode active material according to claim 1, It is characterized in that The positive electrode active material is compacted using a pressure i, and the specific surface area of the positive electrode active material before compaction is SSA 0 , the specific surface area of the positive electrode active material after compaction is SSA i , and satisfies: 0<(SSA i -SSA 0 ) / SSA 0 ≤(7.07ln(i)-5.9) / 100, where 6T≤i≤12T.
3. The positive electrode active material according to claim 2, It is characterized in that Satisfy at least one of the following conditions: Under the condition of i=6T, (SSA 6T -SSA 0 ) / SSA 0 ≤6.5%; Under the condition of i=9T, (SSA 9T -SSA 0 ) / SSA 0 ≤9%; Under the condition of i=12T, (SSA 12T -SSA 0 ) / SSA 0 ≤11%.
4. The positive electrode active material according to claim 3, It is characterized in that K 95 =(Dv 95 -Dv 5 ) / Dv 50 , and satisfy 0.1≤K 95 ≤7, optional 4.5≤K 95 ≤6, where Dv 5 Dv is the particle size corresponding to the positive electrode active material particle size volume distribution percentage reaching 5%, 50 Dv is the particle size corresponding to the positive electrode active material particle size volume distribution percentage reaching 50%, 95 It is the particle size corresponding to when the volume distribution percentage of the positive electrode active material particle size reaches 95%.
5. The positive electrode active material according to any one of claims 1 to 4, It is characterized in that The iron dissolution of the positive electrode active material is less than or equal to 300 ppm. Optionally, the iron dissolution of the positive electrode active material is less than or equal to 150 ppm.
6. The positive electrode active material according to claim 5, It is characterized in that Satisfy at least one of the following conditions: Under the pressure of 3T, the compaction density of the positive electrode active material is 2.3g / cm 3 -2.6g / cm 3 ; The positive electrode active material has a resistance of 1 Ω·cm-20 Ω·cm.
7. The positive electrode active material according to claim 5, It is characterized in that At least a portion of the surface of the positive electrode active material has a carbon coating layer.
8. A method for preparing the positive electrode active material according to any one of claims 1 to 7, It is characterized in that include: Mixing a Li source, a P source, an Fe source, an M source, and a solvent to obtain a slurry, wherein the molar ratio of the P element in the P source to the Fe element in the Fe source is less than or equal to 1.053, and grinding and drying the slurry to obtain precursor particles; The precursor particles are subjected to a first sintering and a second sintering in sequence, wherein the temperature of the first sintering is T 1 The temperature of the second sintering is T 2 , T 1 <T 2 , and crushed to obtain the positive electrode active material.
9. The method according to claim 8, It is characterized in that The molar ratio of the P element in the P source to the Fe element in the Fe source is 1.015-1.
045.
10. The method according to claim 8, It is characterized in that The first sintering satisfies at least one of the following conditions: 300≤T 1 ≤500℃; The holding time of the first sintering is t 1 , and satisfy 1h≤t 1 ≤7h, optionally, 3h≤t 1 ≤5h; The precursor particles are heated to the T 1 The heating rate is 2℃ / min-3℃ / min.
11. The method according to claim 8, It is characterized in that The second sintering satisfies at least one of the following conditions: 700≤T 2 ≤900℃; The holding time of the second sintering is t 2 , and satisfy 5h≤t 2 ≤15h, optionally, 7h≤t 2 ≤10h; By the T 1 Heating to the T 2 The heating rate is 0.5℃ / min-3℃ / min.
12. The method according to claim 8, It is characterized in that Also includes: The Li source, the P source, the Fe source, the M source, the carbon source, and the solvent are mixed.
13. The method according to claim 12, It is characterized in that Satisfy at least one of the following conditions: The Li source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium oxalate, and lithium nitrate; The carbon source comprises at least one of glucose, sucrose, starch, cellulose, citric acid, oxalic acid, polyethylene glycol, polyvinyl alcohol, and polyethylene; The P source and the Fe source include iron phosphate; The M source includes M oxide.
14. A positive electrode sheet, It is characterized in that The invention comprises the positive electrode active material according to any one of claims 1 to 7 or the positive electrode active material prepared by the method according to any one of claims 8 to 13.
15. A battery, It is characterized in that Including the positive electrode sheet as described in claim 14.
Citation Information
Patent Citations
Secondary battery and preparation method thereof
CN115513515A
Carbon-coated lithium iron phosphate positive active material, preparation method thereof, positive pole piece containing carbon-coated lithium iron phosphate positive active material and lithium ion battery
CN116601798A
Lithium iron phosphate positive electrode material and preparation method and application thereof
CN117080436A
Preparation method of lithium iron phosphate, positive active material, positive pole piece, battery and electric device
CN117088352A
Method for testing content of residual lithium in positive electrode material with olivine structure
CN118362681A
Cited By
Method for rapidly evaluating performance of silicon-carbon negative electrode material of lithium ion battery
CN119618907A
Positive electrode material and preparation method thereof, lithium ion battery and electric device
CN120237203A