Positive electrode active material and preparation method and application thereof
By coating the surface of the positive electrode active material of lithium-ion batteries with a carbon-lithium alloy composite layer, the problems of insufficient cycle stability and rate performance of the material are solved, and the performance and safety of the battery under different temperature conditions are improved.
Patent Information
- Application Number
- CN202411253264.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-15
AI Technical Summary
Existing positive electrode active materials for lithium-ion batteries have shortcomings in terms of cycle stability and rate performance, especially under low and high temperature conditions, and there are problems with electrolyte side reactions.
A carbon-lithium alloy composite coating layer is used to coat the cathode substrate material. By controlling the thickness, composition and ratio of the coating layer, the structural stability and electronic and ion conduction properties of the material are improved. The preparation method includes mixing, evaporation and calcination.
It improves the rate performance and cycle performance of lithium-ion batteries, enhances battery performance at low and high temperatures, reduces electrolyte interface reactions, and strengthens battery safety and stability.
Smart Images

Figure CN118970013A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a positive electrode active material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are widely used in various portable electronic devices and electric vehicles due to their high energy density, long cycle life and environmental friendliness. Among them, the positive electrode active material is one of the key factors affecting the performance of lithium-ion batteries. At present, the commonly used positive electrode active materials for lithium-ion batteries are mainly lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, etc.
[0003] However, these materials still have some problems in practical applications, such as poor stability and easy side reactions with electrolytes. Currently, surface coating is often used to solve the above problems. However, the positive electrode active materials prepared by surface coating have poor cycle stability and poor rate performance when applied to lithium-ion batteries. Summary of the invention
[0004] The main purpose of the present invention is to provide a positive electrode active material, which is applied to a lithium ion battery to improve the rate performance and cycle performance of the lithium ion battery.
[0005] The present invention also provides a method for preparing a positive electrode active material, which can prepare the positive electrode active material and has simple process and low cost.
[0006] The present invention also provides a positive electrode sheet. Since the positive electrode sheet comprises the positive electrode active material, the positive electrode sheet is used in a lithium ion battery and can improve the rate performance and cycle performance of the lithium ion battery.
[0007] The present invention also provides a lithium ion battery. Since the lithium ion battery comprises the positive electrode sheet, the lithium ion battery has excellent rate performance and cycle performance.
[0008] In a first aspect, the present invention provides a positive electrode active material, comprising a positive electrode base material and a carbon-lithium alloy composite coating layer coated on at least a portion of the surface of the positive electrode base material.
[0009] The positive electrode active material as described above has a contact angle of 5-20°.
[0010] The positive electrode active material as described above, wherein the ion diffusion coefficient of the positive electrode active material is 4×10 -13 -9×10 -13 cm 2 ·s -1 , impedance is 20-1000Ω.
[0011] The positive electrode active material as described above, wherein the composite coating layer accounts for 1.5-2% of the mass fraction of the positive electrode active material; and / or,
[0012] The mass fraction of the lithium alloy in the composite coating layer is 4-15%.
[0013] For the positive electrode active material as described above, the thickness of the composite coating layer is 10-20 nm.
[0014] The positive electrode active material as described above, wherein the positive electrode matrix material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
[0015] As the positive electrode active material described above, the lithium-based alloy includes at least one of lithium aluminum alloy, lithium magnesium alloy, lithium lead alloy, lithium beryllium alloy, lithium sodium alloy, lithium silicon alloy, lithium cobalt alloy, lithium nickel alloy and lithium manganese alloy.
[0016] In a second aspect, the present invention provides a method for preparing the positive electrode active material as described above, comprising the following steps:
[0017] 1) mixing a raw material system including a positive electrode matrix material, a lithium alloy, a carbon source, and an emulsifier, adding the mixture into deionized water, and evaporating the solvent to obtain a positive electrode active material precursor;
[0018] 2) calcining the cathode active material precursor at 600-750° C. in a protective atmosphere to obtain the cathode active material.
[0019] In the preparation method as described above, the mass of the added emulsifier is 0.5-4% of the mass of the raw material system.
[0020] In a third aspect, the present invention provides a positive electrode sheet, comprising the positive electrode active material as described above or the positive electrode active material prepared by the preparation method as described above.
[0021] In a fourth aspect, the present invention provides a lithium-ion battery comprising the positive electrode sheet as described above.
[0022] The positive electrode active material provided by the present invention can improve the structural stability of the positive electrode active material because the composite coating layer includes a lithium-based alloy, and make it have excellent electronic and ion conductivity, thereby improving the rate performance and cycle performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 This is a SEM image of the positive electrode active material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In a first aspect, the present invention provides a positive electrode active material, comprising a positive electrode base material and a carbon-lithium alloy composite coating layer coated on at least a portion of the surface of the positive electrode base material.
[0027] The positive electrode active material in the present invention includes a carbon-lithium alloy composite coating layer, which is applied to a lithium-ion battery to improve the rate performance and cycle performance of the lithium-ion battery. It is speculated that this may be because the lithium alloy has excellent electronic and ion conductivity, and the positive electrode active material is applied to the lithium-ion battery to improve the rate performance of the lithium-ion battery; and the lithium alloy has a high mechanical strength, so that the carbon-lithium alloy composite coating layer has good stability and durability, and after long-term use, it is not easy to collapse and fail, so the cycle and safety performance of the lithium-ion battery can be improved.
[0028] At low temperatures, the electrolyte activity is poor and the ion mobility is reduced, resulting in an increase in the internal resistance of the battery. However, lithium alloys have high electronic conductivity. The carbon-lithium alloy composite coating can improve the interface stability between the positive electrode active material and the electrolyte (isolate the electrolyte, form a CEI film, reduce interface reactions, and inhibit gas production), reduce interface impedance, and thus improve the cycle performance of lithium-ion batteries at low temperatures.
[0029] In addition, lithium alloys have excellent thermal conductivity. The coating of the carbon-lithium alloy composite coating layer can improve the thermal conductivity of the positive electrode active material, reduce the occurrence of local overheating, improve the cycle performance of lithium-ion batteries at high temperatures, and inhibit gas production to a certain extent, reduce the risk of thermal runaway of the battery, and improve the safety of the battery.
[0030] The positive electrode active material provided by the present invention can improve the structural stability of the positive electrode active material because the composite coating layer includes a lithium alloy, and make it have excellent electronic and ion conductivity, thereby improving the rate performance and cycle performance of the lithium ion battery. The coating of the composite coating layer can also improve the structural integrity of the positive electrode active material, improve the processing performance of the positive electrode active material, and avoid failure after long-term use, which affects the performance of the lithium ion battery.
[0031] The present invention does not limit the specific type of the positive electrode matrix material. Further, the positive electrode matrix material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
[0032] The present invention does not limit the specific type of lithium alloy. Furthermore, the lithium alloy includes at least one of lithium aluminum alloy, lithium magnesium alloy, lithium lead alloy, lithium beryllium alloy, lithium sodium alloy, lithium silicon alloy, lithium cobalt alloy, lithium nickel alloy and lithium manganese alloy.
[0033] In some embodiments of the present invention, the contact angle of the positive electrode active material is 5-20°.
[0034] The present invention introduces an O / W type emulsifier to make the contact angle of the positive electrode active material within an appropriate range. Since the surface tension and the contact angle are positively correlated, the surface tension of the positive electrode active material is relatively appropriate. This can avoid the positive electrode active material with high surface tension from causing structural damage to the battery during the charge and discharge process due to internal stress concentration, such as the formation of cracks. This damage will further accelerate the degradation of the material, such as Mn 2+ Therefore, the positive electrode active material with a contact angle within the above range in the present invention can effectively alleviate the stress caused by volume expansion and contraction of the positive electrode active material during the charge and discharge process, and effectively avoid the Mn 2+ The dissolution phenomenon occurs, thereby improving the structural stability of the positive electrode active material, thereby improving the rate performance and cycle performance of the lithium-ion battery and extending the battery life.
[0035] In some embodiments of the present invention, the ion diffusion coefficient of the positive electrode active material is 4×10 -13 -9×10 -13 cm 2 ·s -1 , impedance is 20-1000Ω.
[0036] The ion diffusion coefficient and impedance of the positive electrode active material in the present invention are within a suitable range, and ions can be quickly embedded and extracted. When applied to lithium-ion batteries, the rate performance and cycle performance of lithium-ion batteries can be improved.
[0037] Specifically, the ion diffusion coefficient and impedance of the positive electrode active material can be adjusted by adjusting the mass fraction of the composite coating layer in the positive electrode active material and the mass fraction of the lithium alloy in the composite coating layer. In one embodiment, the mass fraction of the composite coating layer in the positive electrode active material is 1.5-2%; and / or the mass fraction of the lithium alloy in the composite coating layer is 4-15%, which can be applied to lithium-ion batteries to further improve the rate performance and cycle performance of lithium-ion batteries.
[0038] In some embodiments of the present invention, the thickness of the composite coating layer is 10-20 nm.
[0039] It can be understood that the thickness of the composite coating layer will greatly affect the electronic conductivity of the positive electrode active material, thereby affecting the rate performance and cycle performance of the battery. The composite coating layer in the present invention has a suitable coating thickness, which can take into account the conduction of both electrons and ions.
[0040] In one embodiment, the thickness of the composite coating layer is controlled to be 10-20 nm, which is within a suitable range. The suitable composite coating layer thickness can inhibit the growth of particles and reduce the diffusion distance of lithium ions. In addition, the suitable composite coating layer thickness has excellent conductivity, is conducive to the transmission of electrons, and improves the electronic conductivity of the positive electrode active material, thereby improving the rate performance and cycle performance of the battery.
[0041] The present invention does not limit the testing method of the composite coating layer thickness. For example, the thickness can be obtained by measuring the coating layer of the positive electrode active material in a scanning electron microscope.
[0042] The thickness of the composite coating layer in the present invention is 10-20 nm. Within a suitable range, the coating layer thickness can effectively increase electron transfer without affecting ion transmission. When used in lithium-ion batteries, the rate performance and cycle performance of lithium-ion batteries can be improved.
[0043] In a second aspect, the present invention provides a method for preparing the positive electrode active material as described above, comprising the following steps:
[0044] 1) mixing a raw material system including a positive electrode matrix material, a lithium alloy, a carbon source, and an emulsifier, adding the mixture into deionized water, and evaporating the solvent to obtain a positive electrode active material precursor;
[0045] 2) calcining the cathode active material precursor at 600-750° C. in a protective atmosphere to obtain the cathode active material.
[0046] The invention obtains a positive electrode active material precursor by uniformly mixing a raw material system, and then sintering the positive electrode active material precursor to obtain the positive electrode active material.
[0047] Specifically, in step 1), the positive electrode matrix material, lithium alloy, carbon source, and emulsifier are mixed in a certain molar ratio and added to deionized water, and the solvent water is evaporated and removed by natural evaporation to obtain a positive electrode active material precursor. The present invention can adjust the mass proportion of the composite coating layer and the lithium alloy in the positive electrode active material by controlling the molar ratio of the positive electrode matrix material, lithium alloy, carbon source, and emulsifier. Among them, the positive electrode matrix material may include at least one of lithium cobalt oxide, lithium manganate, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide; the lithium alloy may include at least one of lithium aluminum alloy, lithium magnesium alloy, lithium lead alloy, lithium beryllium alloy, lithium sodium alloy, lithium silicon alloy, lithium cobalt alloy, lithium nickel alloy, and lithium manganese alloy; the carbon source may include at least one of glucose, sucrose, citric acid, carbon nanotubes, and reduced graphene oxide; the emulsifier may include at least one of PEG, PVA, PVP, Span, SDS, and PAA.
[0048] In step 2), the positive electrode active material precursor is heated to 600-750° C. at a rate of 5° C. / min under a protective atmosphere and calcined for 6-8 hours to obtain a positive electrode active material. The protective gas may be Ar, N2, He, or H2.
[0049] The preparation method provided by the present invention can prepare the positive electrode active material of the first aspect, and the positive electrode active material is applied to a lithium ion battery to improve the rate performance and cycle performance of the lithium ion battery.
[0050] In some embodiments of the present invention, the added mass of the emulsifier is 0.5-4% of the mass of the raw material system.
[0051] In the present invention, the amount of the emulsifier added is controlled to be 0.5-4% of the mass of the raw material system. Within a suitable range, a positive electrode active material with a suitable surface tension can be obtained, which effectively alleviates the stress generated by the volume expansion and contraction of the positive electrode active material during the charge and discharge process, thereby improving the structural stability of the positive electrode active material, thereby improving the rate performance and cycle performance of the lithium ion battery, and extending the service life of the battery.
[0052] In a third aspect, the present invention provides a positive electrode sheet, comprising the positive electrode active material as described above or the positive electrode active material prepared by the preparation method as described above.
[0053] The positive electrode sheet of the present invention can be prepared by conventional technical means in the art. Specifically, the above-mentioned positive electrode material, conductive agent, and binder can be uniformly dispersed in a solvent to obtain a positive electrode active layer slurry, and then the positive electrode active layer slurry is coated on at least one functional surface of the positive electrode collector. After drying, the positive electrode sheet of the present invention can be obtained.
[0054] The present invention does not particularly limit the specific types of the conductive agent and the adhesive. The conductive agent, the adhesive and other components can be selected from conventional materials in the field. For example, the conductive agent can be selected from one or more of conductive carbon black, carbon nanotubes, conductive graphite, and graphene, and the adhesive can be selected from one or more of polyvinylidene fluoride (PVDF), acrylic modified PVDF, polyacrylate polymers, polyimide, styrene-butadiene rubber, and styrene-propylene rubber.
[0055] The present invention does not specifically limit the coating method, and any coating method such as gravure coating, extrusion coating, spraying, screen printing, etc. can be used to coat the positive electrode active layer slurry.
[0056] Since the positive electrode sheet provided by the present invention includes the above-mentioned positive electrode active material, the positive electrode sheet is used in a lithium ion battery, which can improve the rate performance and cycle performance of the lithium ion battery.
[0057] In a fourth aspect, the present invention provides a lithium-ion battery comprising the positive electrode sheet as described above.
[0058] The lithium ion battery of the present invention includes a separator, a negative electrode and an electrolyte in addition to a positive electrode sheet. The composition of the negative electrode sheet can refer to conventional negative electrode sheets in the art, and the separator can also be a separator conventionally used in the art, such as a PP film, a PE film, etc.
[0059] The lithium-ion battery of the present invention can be prepared by conventional methods in the art. Specifically, the positive electrode sheet, the separator and the negative electrode sheet can be stacked in sequence, and then a battery cell can be obtained through a stacking or winding process, and then the above-mentioned lithium-ion battery can be obtained through baking, liquid injection, formation, packaging and other processes.
[0060] Since the lithium ion battery provided by the present invention includes the above-mentioned positive electrode sheet, the lithium ion battery has excellent rate performance and cycle performance.
[0061] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0062] Example 1
[0063] The method for preparing the positive electrode active material of this embodiment comprises the following steps:
[0064] 1) mixing lithium manganese iron phosphate material, lithium magnesium alloy, PEG and sucrose in a molar ratio of 1:0.008:0.0012:0.04 to obtain a raw material system, wherein the mass of the emulsifier accounts for 1.54% of the mass of the raw material system, and then adding the raw material system to an aqueous solution, and forming a positive electrode active material precursor by autothermal evaporation and crushing;
[0065] 2) The positive electrode active material precursor is heated to 680°C at a rate of 5°C / min in a N2 atmosphere and calcined for 8 hours to obtain a carbon-lithium alloy composite coating layer coated lithium manganese iron phosphate positive electrode active material. Among them, the mass fraction of the composite coating layer in the positive electrode active material is 1.80%, recorded as ratio 1, and the mass fraction of the lithium alloy in the composite coating layer is 6.19%, recorded as ratio 2.
[0066] Example 2
[0067] The method for preparing the positive electrode active material of this embodiment comprises the following steps:
[0068] 1) mixing lithium nickel cobalt manganese oxide material, lithium magnesium alloy, PEG and sucrose in a molar ratio of 1:0.008:0.0008:0.025 to obtain a raw material system, wherein the mass of the emulsifier accounts for 1.64% of the mass of the raw material system, and then adding the raw material system to an aqueous solution, and forming a positive electrode active material precursor by autothermal evaporation and crushing;
[0069] 2) The positive electrode active material precursor is heated to 680°C at a rate of 5°C / min in a N2 atmosphere and calcined for 8 hours to obtain a lithium nickel cobalt manganese oxide positive electrode active material coated with a carbon-lithium alloy composite coating layer. The mass fraction of the composite coating layer in the positive electrode active material is 1.86%, recorded as ratio 1, and the mass fraction of the lithium alloy in the composite coating layer is 9.58%, recorded as ratio 2.
[0070] Example 3
[0071] The method for preparing the positive electrode active material of this embodiment comprises the following steps:
[0072] 1) mixing lithium iron phosphate material, lithium magnesium alloy, PEG and glucose in a molar ratio of 1:0.008:0.0012:0.08 to obtain a raw material system, wherein the mass of the emulsifier accounts for 1.53% of the mass of the raw material system, and then adding the raw material system to an aqueous solution, and forming a positive electrode active material precursor by autothermal evaporation and crushing;
[0073] 2) The positive electrode active material precursor is heated to 680°C at a rate of 5°C / min in a N2 atmosphere and calcined for 8 hours to obtain a lithium iron phosphate positive electrode active material coated with a carbon-lithium alloy composite coating layer. The mass fraction of the composite coating layer in the positive electrode active material is 1.96%, recorded as ratio 1, and the mass fraction of the lithium alloy in the composite coating layer is 5.65%, recorded as ratio 2.
[0074] Example 4
[0075] The preparation method of the positive electrode active material of Example 4 is basically the same as that of Example 1, except that the lithium alloy is changed to lithium aluminum alloy.
[0076] Example 5
[0077] The preparation method of the positive electrode active material of Example 5 is basically the same as that of Example 1, except that the lithium alloy is changed to a lithium-sodium alloy.
[0078] Example 6
[0079] The preparation method of the positive electrode active material of Example 6 is basically the same as that of Example 1, except that the calcination temperature is changed to 600°C.
[0080] Example 7
[0081] The preparation method of the positive electrode active material of Example 7 is basically the same as that of Example 1, except that the calcination temperature is changed to 750°C.
[0082] Example 8
[0083] The preparation method of the positive electrode active material of Example 8 is basically the same as that of Example 1, except that the molar ratio of the lithium nickel cobalt manganese oxide material, the lithium magnesium alloy, PEG and sucrose is changed to 1:0.004:0.0004:0.03, wherein the mass of the emulsifier accounts for 0.82% of the mass of the raw material system.
[0084] Example 9
[0085] The preparation method of the positive electrode active material of Example 9 is basically the same as that of Example 1, except that the molar ratio of the lithium nickel cobalt manganese oxide material, the lithium magnesium alloy, PEG and sucrose is changed to 1:0.004:0.0016:0.02, wherein the mass of the emulsifier accounts for 3.29% of the mass of the raw material system.
[0086] Example 10
[0087] The preparation method of the positive electrode active material of Example 10 is basically the same as that of Example 1, except that the lithium manganese iron phosphate material, lithium magnesium alloy, PEG and sucrose are mixed in a molar ratio of 1:0.008:0.0012:0.1.
[0088] Embodiment 11
[0089] The preparation method of the positive electrode active material of Example 11 is basically the same as that of Example 1, except that the molar ratio of the lithium nickel cobalt manganese oxide material, the lithium magnesium alloy, PEG and sucrose is changed to 1:0.008:0.0002:0.04, wherein the mass of the emulsifier accounts for 0.26% of the mass of the raw material system.
[0090] Comparative Example 1
[0091] The preparation methods of the positive electrode active materials of Comparative Example 1 and Example 1 are basically the same, except that no lithium alloy is added in step 1), and finally a carbon-coated lithium manganese iron phosphate positive electrode active material is prepared.
[0092] Comparative Example 2
[0093] The preparation methods of the positive electrode active materials of Comparative Example 2 and Example 1 are basically the same, except that no lithium alloy and carbon source are added in step 1), and finally an uncoated lithium manganese iron phosphate positive electrode active material is prepared.
[0094] Comparative Example 3
[0095] This comparative example provides a composite coated lithium ion battery positive electrode active material, including a positive electrode base material and a composite coating layer coated on the outer surface of the positive electrode base material, wherein the composite coating layer contains an electronic conductor material and a positive electrode lithium supplement material.
[0096] 20g of Li5FeO4 with a median particle size of 100nm was added to 500g of anhydrous ethanol and stirred to obtain a dispersion. 0.8 Co 0.1 Mn 0.1 O2 (median particle size of 4.5 μm) was added to the above dispersion, and a precursor of a coated Li5FeO4 material layer was obtained by evaporating the solvent;
[0097] 100 g of Li5FeO4 coated material layer precursor was added to 100 g of anhydrous ethanol dispersion with a mass concentration of 2.8% polyethylene glycol, and the dispersion was evenly dispersed to obtain a composite material dispersion; the composite material dispersion was spray-dried to obtain a composite coating layer precursor; the composite coating layer precursor was calcined at 400°C in a nitrogen atmosphere for 5 h to obtain a positive electrode lithium supplement material Li5FeO4 and an electronic conductor amorphous carbon composite coated LiNi 0.8 Co 0.1 Mn 0.1 O2 composite positive electrode material. The mass fraction of the composite coating layer in the composite positive electrode active material is about 2.55%, and the mass fraction of the electronic conductor coating layer in the composite positive electrode active material is about 0.56%.
[0098] Test example:
[0099] 1. Contact angle: Use a microsyringe to drop deionized water onto the surface of the LMFP sample, and use the contact angle meter to automatically calculate the contact angles between the droplet and the surface of the LMFP sample to obtain the average contact angle of the sample;
[0100] 2. Ion diffusion coefficient: The ion diffusion coefficient is calculated by formula (1):
[0101]
[0102] D Li+ represents the lithium ion diffusion coefficient, cm 2 ·s -1 ;
[0103] R represents the gas constant, which is 8.314 J·(mol K) -1 ;
[0104] T represents absolute temperature, T = 273.15 + actual temperature (°C), K;
[0105] A is the surface area of the electrode, cm 2 ;
[0106] n represents the number of electrons gained or lost per mole of molecules involved in the redox reaction;
[0107] F represents the Faraday constant, which is 69485.3 C·mol -1 ;
[0108] C Li+ Represents Li + Concentration, take 0.059 mol·L -1 ;
[0109] σ represents the Warburg factor. The slope of the straight line in the low-frequency region is obtained by fitting the impedance spectrum analysis, which is σ.
[0110] 3. Impedance: The Princeton electrochemical workstation was used to test the material's AC impedance spectroscopy (EIS). The test conditions were: the AC excitation signal amplitude was 10mV and the frequency range was 10 -2 -10 5 Hz, and the voltage range is between 2.0-4.5V.
[0111] 4. Coating thickness: The amplitude ratio and phase shift parameters of the material are measured by ellipsometer, and the composite coating thickness of the LMFP material is calculated by combining the ellipsometer related software and appropriate optical models.
[0112] 5. Carbon-lithium alloy composite coating: The carbon-lithium alloy coating layer on the surface of the positive electrode active material was detected by transmission electron microscopy; the mass fraction was composed of carbon and lithium alloy. The carbon was confirmed by carbon-sulfur analyzer and its mass fraction was calculated; the lithium alloy was confirmed by EDS and its mass fraction was calculated.
[0113] 6. Specific capacity: At 25°C and normal pressure (0.1 MPa), the positive electrode active material, conductive carbon black, and binder polyvinylidene fluoride (PVDF) of each embodiment and comparative example were respectively stirred and mixed in an N-methylpyrrolidone solvent at a mass percentage ratio of 95:3:2 to obtain a positive electrode slurry. The positive electrode slurry was coated on an aluminum foil, and after drying and cold pressing, a positive electrode sheet containing a positive electrode active layer with a thickness of 100 μm was obtained; then the positive electrode sheet was punched into a small disc with a diameter of 12 mm with a film mold, and after drying and weighing, a button battery was assembled in a glove box under an Ar protective atmosphere using a 2025 button battery shell, a Li metal disc as the negative electrode, and a conventional high-voltage lithium cobalt oxide electrolyte. The batteries were charged at a constant current of 0.1C / 1C / 5C to 4.5V, then charged at a constant voltage of 4.5V to a current of 0.05C. The charging capacity at this time was recorded as the first-cycle charging capacity. After that, the batteries were allowed to stand for 5 minutes and then discharged at a constant current of 0.1C / 1C / 5C to a voltage of 2.5V. The discharge capacity was recorded as the first-cycle discharge capacity of the battery.
[0114] 7. Rate performance: According to the method in the withholding capacity test, the positive electrode active material is coated into a positive electrode sheet, the negative electrode is graphite, and the diaphragm polyethylene and the electrolyte (the electrolyte is LiPF6 and the solvent is EC / DMC) form a full battery, which is charged at a constant current of 0.1C rate to a voltage of 4.5V, and then charged at a constant voltage at a voltage of 4.5V to a current equal to 0.05C, then allowed to stand for 5 minutes, and then discharged at a constant current of 0.1C rate to a voltage of 2.5V. The capacity at this time is recorded as the discharge capacity at 0.1C rate; stand for 10 minutes, charge at a constant current of 1C rate to a voltage of 4.5V, and then charge at a constant voltage of 4.5V to a current equal to 0.05C, then allowed to stand for 5 minutes, and then discharged at a constant current of 1C rate to a voltage of 2.5V. The capacity at this time is recorded as the discharge capacity at 1C rate, and the ratio of the discharge capacity at 1C rate to the discharge capacity at 0.1C rate is the 1C rate performance.
[0115] 8. Cycle performance: According to the method in the charge capacity test, the positive electrode active material is coated into a positive electrode sheet, the negative electrode is graphite, and the separator polyethylene and the electrolyte (the electrolyte is LiPF6, the solvent is EC / DMC) form a full battery. At 25℃ / 45℃ / -20℃, the battery is charged to 4.5V at a constant current of 1C, then charged to 4.5V at a constant voltage of 0.5C, and then discharged to 2.5V at a discharge rate of 1C. Repeat this charge and discharge cycle 500 times, and measure the discharge capacity Q1 at the first cycle and the discharge capacity Q at the 500th cycle. 500 The capacity retention rate after 500 cycles is Q = Q 500 / Q1*100%.
[0116] Table 1
[0117]
[0118] It can be seen from Table 1 that, compared with the comparative example, the positive electrode active material provided by the present invention can improve the structural stability of the positive electrode active material and have excellent electronic and ion conductivity, because the composite coating layer includes a lithium alloy, thereby improving the rate performance and cycle performance of the lithium ion battery.
[0119] From the comparison between Example 1 and Comparative Examples 1-3, it can be seen that the positive electrode active material prepared by the present invention can improve the rate performance and cycle performance of the lithium ion battery because the composite coating layer includes a lithium alloy.
[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A positive electrode active material, characterized in that: It comprises a positive electrode base material and a carbon-lithium alloy composite coating layer coated on at least a part of the surface of the positive electrode base material.
2. The positive electrode active material according to claim 1, characterized in that The contact angle of the positive electrode active material is 5-20°.
3. The positive electrode active material according to claim 1 or 2, characterized in that: The ion diffusion coefficient of the positive electrode active material is 4×10 -13 -9×10 -13 cm 2 ·s -1 , impedance is 20-1000Ω.
4. The positive electrode active material according to any one of claims 1 to 3, characterized in that: The mass fraction of the composite coating layer in the positive electrode active material is 1.5-2%; and / or, The mass fraction of the lithium alloy in the composite coating layer is 4-15%.
5. The positive electrode active material according to any one of claims 1 to 4, characterized in that: The thickness of the composite coating layer is 10-20 nm.
6. The positive electrode active material according to any one of claims 1 to 5, characterized in that: The positive electrode matrix material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
7. The positive electrode active material according to any one of claims 1 to 6, characterized in that: The lithium alloy includes at least one of lithium aluminum alloy, lithium magnesium alloy, lithium lead alloy, lithium beryllium alloy, lithium sodium alloy, lithium silicon alloy, lithium cobalt alloy, lithium nickel alloy and lithium manganese alloy.
8. A method for preparing a positive electrode active material according to any one of claims 1 to 7, characterized in that: The following steps are involved: 1) mixing a raw material system including a positive electrode matrix material, a lithium alloy, a carbon source, and an emulsifier, adding the mixture into deionized water, and evaporating the solvent to obtain a positive electrode active material precursor; 2) calcining the cathode active material precursor at 600-750° C. in a protective atmosphere to obtain the cathode active material.
9. The preparation method according to claim 8, characterized in that: The added mass of the emulsifier is 0.5-4% of the mass of the raw material system.
10. A positive electrode sheet, characterized in that: The invention comprises the positive electrode active material according to any one of claims 1 to 7 or the positive electrode active material prepared by the preparation method according to claim 8 or 9.
11. A lithium ion battery, characterized in that: Including the positive electrode sheet as claimed in claim 10.
Citation Information
Patent Citations
Lithium ion battery
CN103700849A
Composite anode material of lithium ion battery and preparation method thereof
CN108695505A
Carbon-coated porous Cr-Cu alloy / lithium iron phosphate positive electrode and preparation method thereof
CN114551880A
Positive electrode material, preparation method thereof and lithium ion battery
CN118248845A