MOF positive electrode additive, preparation method thereof and positive electrode lead paste containing MOF positive electrode additive
By using MOF positive electrode additives in lead-acid batteries, the problem of insufficient specific energy and service life of lead-acid batteries is solved, and higher corrosion resistance and specific energy are achieved, which extends the battery life and reduces internal resistance.
Patent Information
- Application Number
- CN202411006547.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
The specific energy and service life of existing lead-acid batteries are difficult to meet high requirements, especially in electric bicycle applications.
MOF positive electrode additives, including acid nickel salt, acid zinc salt and 2-methylimidazole, are used to form MOF positive electrode additives through a specific preparation method and add them to the positive electrode lead paste to reduce internal resistance and avoid the growth of lead dendrites.
It improves the corrosion resistance and specific energy of lead-acid batteries, extends the service life, and reduces the internal resistance of the battery and improves the utilization rate of active substances.
Smart Images

Figure CN118970044A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of storage batteries, and in particular to a MOF positive electrode additive and a preparation method thereof, and a positive electrode lead paste containing the MOF positive electrode additive. Background Art
[0002] Lead-acid batteries are acid batteries that use lead as electrodes, manganese dioxide or nickel sulfate as positive active materials, and dilute sulfuric acid as electrolyte. At present, lead-acid batteries are widely used in electric bicycles due to their high safety, low cost, and recyclable raw materials.
[0003] With the introduction of the new national standard for electric bicycles, the requirements for the specific energy and service life of lead-acid batteries for electric bicycles are getting higher and higher. In the existing technology, the specific energy and service life of lead-acid batteries are difficult to meet the high requirements for use. Based on this, the development of positive electrode additives that can improve the specific energy and service life has become an urgent problem that needs to be solved to a certain extent. Summary of the invention
[0004] The purpose of the present invention is to provide a MOF positive electrode additive and a preparation method thereof, and a positive electrode lead paste containing the same, to solve the following technical problems: How to improve the service life of lead-acid batteries? How to improve the specific energy of lead-acid batteries? The purpose of the present invention can be achieved by the following technical solutions: In a first aspect, the present invention discloses a MOF cathode additive, comprising the following raw materials in parts by weight: 3-33 parts of acidic nickel salt, 10-108 parts of acidic zinc salt, 10-103 parts of 2-methylimidazole, and 500 parts of deionized water.
[0005] Preferably, the acidic nickel salt is 10-20 parts, the acidic zinc salt is 30-80 parts, the 2-methylimidazole is 30-75 parts, and the deionized water is 500 parts; more preferably, the acidic nickel salt is 15 parts, the acidic zinc salt is 50 parts, the 2-methylimidazole is 50 parts, and the deionized water is 500 parts.
[0006] In a further embodiment of the present invention, the acidic nickel salt is nickel sulfate hexahydrate, and the acidic zinc salt is zinc sulfate heptahydrate.
[0007] In a further embodiment of the present invention, the molar concentration of the nickel sulfate hexahydrate is 0.05-0.5 mol / L, and the molar concentration of the zinc sulfate heptahydrate is 0.15-1.5 mol / L.
[0008] In a second aspect, the present invention discloses a method for preparing the MOF cathode additive as described above, characterized in that it comprises the following preparation steps: S1: adding an acidic nickel salt into half of the deionized water to fully dissolve to form a nickel salt solution, and adding an acidic zinc salt into the nickel salt solution to fully dissolve to form a mixed solution; S2: adding 2-methylimidazole to the remaining deionized water to fully dissolve it to form a 2-methylimidazole solution, and then mixing the mixed solution with the 2-methylimidazole solution to obtain a reaction solution; S3: The reaction solution is transferred to a reactor, and the reactor is placed in a heating furnace at 100-240° C. to react for 4-16 hours. After the reaction is completed, the reactor is taken out and cooled to room temperature to obtain a MOF positive electrode additive.
[0009] In a further embodiment of the present invention: in steps S1-S2, the nickel salt solution, the mixed solution, the 2-methylimidazole solution and the reaction solution are all fully mixed and dissolved by an ultrasonic cleaner.
[0010] In a further embodiment of the present invention: in step S3, the heating furnace is a muffle furnace.
[0011] In a third aspect, the present invention further discloses a positive electrode lead paste containing the MOF positive electrode additive as described above, comprising the following raw materials in parts by weight: 100 parts of lead powder, 6-8 parts of red lead, 0.1-0.2 parts of graphite, 0.1-0.2 parts of stannous sulfate, 0.05-1 parts of antimony trioxide, 0.2-0.8 parts of short fibers, 1-10 parts of water, and 1 part of MOF positive electrode additive.
[0012] Preferably, lead powder is 100 parts, red lead is 7 parts, graphite is 0.15 parts, stannous sulfate is 0.15 parts, antimony trioxide is 0.5 parts, short fibers are 0.5 parts, water is 5 parts, and MOF positive electrode additive is 1 part.
[0013] In a further embodiment of the present invention: the preparation method is: Step 1: Evenly mix graphite, stannous sulfate, antimony trioxide, short fibers and water to form a mixture A; Step 2: Add mixture A to red lead and stir to mix evenly to obtain mixture B, add mixture B to lead powder and stir to mix, during the stirring and mixing process, add MOF additive by high pressure spraying and stir to mix evenly to finally obtain positive electrode lead paste.
[0014] In a further embodiment of the present invention: the apparent density of the positive electrode lead paste is 3.6-5.2 g / cm 3 .
[0015] Beneficial effects of the present invention: The MOF additive of the present invention has low internal resistance, high oxygen evolution overpotential and filamentous morphology. In the process of synthesizing lead paste, the additive can be added to make the active substances mixed evenly, thereby reducing the internal resistance of the lead paste and avoiding the growth of lead dendrites. During the charge and discharge process of the battery, once lead dendrites grow on the electrode plate, it may cause the diaphragm to be damaged, and then the positive and negative electrodes contact, resulting in a short circuit and reducing the service life of the battery. Therefore, avoiding the growth of lead dendrites is beneficial to improving the corrosion resistance of the positive electrode plate and extending the service life of the battery; at the same time, it can also reduce the internal resistance of the battery, improve the active utilization rate of the lead paste, and thus improve the specific energy of the lead-acid battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a comparison chart of the corrosion resistance test results of the positive electrode lead paste containing MOF positive electrode additives prepared in Examples 1-5 of the present invention; Figure 2 This is a comparison chart of impedance test results of positive electrode lead pastes containing MOF positive electrode additives prepared in Examples 1-5 of the present invention; Figure 3 It is an equivalent circuit diagram obtained by fitting the results of impedance testing of the positive electrode lead paste containing MOF positive electrode additives prepared in Examples 1-5 of the present invention. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0019] Example 1
[0020] Preparation of MOF cathode additives: Add 250 mL of deionized water to the No. 1 ultrasonic cleaner, then add 3 g of nickel sulfate hexahydrate (0.5 mol / L), mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved nickel sulfate solution; then add 10 g of zinc sulfate heptahydrate (1.5 mol / L) to the nickel sulfate solution, mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved mixed solution; add 250 mL of deionized water to the No. 2 ultrasonic cleaner, then add 10 g of 2-methylimidazole, mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved 2-methylimidazole solution, transfer the mixed solution in the No. 1 ultrasonic cleaner to the No. 2 ultrasonic cleaner and mix with the 2-methylimidazole solution, mix at a frequency of 50 kHz for 10 min to obtain a uniformly mixed reaction solution, transfer the reaction solution to a reactor, place the reactor in a muffle furnace and react at 100 ° C for 16 hours, take out the reactor after the reaction, and cool to room temperature to obtain a MOF positive electrode additive.
[0021] Preparation of positive electrode lead paste containing MOF positive electrode additive: Add 0.1g of graphite, 0.1g of stannous sulfate, 0.05g of antimony trioxide, 0.2g of short fibers, and 1g of water to the mixer, mix at a speed of 150rpm for 2min to obtain a uniformly mixed mixture A, then add 6g of red lead to the mixer, mix at a speed of 150rpm for 10min to obtain a uniformly mixed mixture B, then add 200g of lead powder to the mixer, mix at a speed of 200rpm for 10min, and while mixing, spray 1g of the above-prepared MOF positive electrode additive into the mixer by high-pressure spraying. After the end, a positive electrode lead paste containing MOF positive electrode additive is obtained, and its apparent density is 3.6g / cm3.
[0022] Example 2
[0023] Add 250 mL of deionized water to the No. 1 ultrasonic cleaner, then add 10 g of nickel sulfate hexahydrate (0.4 mol / L), mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved nickel sulfate solution; then add 30 g of zinc sulfate heptahydrate (1.2 mol / L) to the nickel sulfate solution, mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved mixed solution; add 250 mL of deionized water to the No. 2 ultrasonic cleaner, then add 30 g of 2-methylimidazole, mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved 2-methylimidazole solution, transfer the mixed solution in the No. 1 ultrasonic cleaner to the No. 2 ultrasonic cleaner and mix with the 2-methylimidazole solution, mix at a frequency of 50 kHz for 10 min to obtain a uniformly mixed reaction solution, transfer the reaction solution to a reactor, place the reactor in a muffle furnace and react at 150° C. for 13 h, take out the reactor after the reaction, and cool to room temperature to obtain a MOF positive electrode additive.
[0024] Preparation of positive electrode lead paste containing MOF positive electrode additive: Add 0.1g of graphite, 0.1g of stannous sulfate, 0.05g of antimony trioxide, 0.2g of short fibers, and 1g of water to the mixer, mix at a speed of 150rpm for 2min to obtain a uniformly mixed mixture A, then add 6g of red lead to the mixer, mix at a speed of 150rpm for 10min to obtain a uniformly mixed mixture B, then add 200g of lead powder to the mixer, mix at a speed of 200rpm for 10min, and while mixing, spray 1g of the above-prepared MOF positive electrode additive into the mixer by high-pressure spraying. After the end, a positive electrode lead paste containing MOF positive electrode additive is obtained, and its apparent density is 3.8g / cm3.
[0025] Example 3
[0026] Add 250 mL of deionized water to the No. 1 ultrasonic cleaner, and then add 15 g of nickel sulfate hexahydrate (0.25 mol / L), mix at a frequency of 50 kHz for 5 minutes to obtain a uniformly dissolved nickel sulfate solution; then add 50 g of zinc sulfate heptahydrate (0.8 mol / L) to the nickel sulfate solution, mix at a frequency of 50 kHz for 5 minutes to obtain a uniformly dissolved mixed solution; add 250 mL of deionized water to the No. 2 ultrasonic cleaner, and then add 50 g of 2-methylimidazole, mix at a frequency of 50 kHz for 5 minutes to obtain a uniformly dissolved 2-methylimidazole solution, transfer the mixed solution in the No. 1 ultrasonic cleaner to the No. 2 ultrasonic cleaner and mix with the 2-methylimidazole solution, mix at a frequency of 50 Hz for 10 minutes to obtain a uniformly mixed reaction solution, transfer the reaction solution to a reactor, place the reactor in a muffle furnace and react at 180°C for 10 hours, take out the reactor after the reaction, and cool to room temperature to obtain a MOF positive electrode additive.
[0027] Preparation of positive electrode lead paste containing MOF positive electrode additive: 0.15 g of graphite, 0.15 g of stannous sulfate, 0.5 g of antimony trioxide, 0.5 g of short fibers, and 5 g of water were added to the mixer, and mixed at a speed of 150 rpm for 2 min to obtain a uniformly mixed mixture A. Subsequently, 7 g of red lead was added to the mixer, and mixed at a speed of 150 rpm for 10 min to obtain a uniformly mixed mixture B. 200 g of lead powder was added to the mixer, and mixed at a speed of 200 rpm for 10 min. While mixing, 1 g of the MOF positive electrode additive prepared above was sprayed into the mixer by high-pressure spraying. After the end, a positive electrode lead paste containing a MOF positive electrode additive was obtained, and its apparent density was 4.5 g / cm3.
[0028] Example 4
[0029] Add 250 mL of deionized water to the No. 1 ultrasonic cleaner, then add 20 g of nickel sulfate hexahydrate (0.1 mol / L), mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved nickel sulfate solution; then add 80 g of zinc sulfate heptahydrate (0.5 mol / L) to the nickel sulfate solution, mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved mixed solution; add 250 mL of deionized water to the No. 2 ultrasonic cleaner, then add 75 g of 2-methylimidazole, mix at a frequency of 50 kHz for 5 min to obtain a uniformly dissolved 2-methylimidazole solution, transfer the mixed solution in the No. 1 ultrasonic cleaner to the No. 2 ultrasonic cleaner and mix with the 2-methylimidazole solution, mix at a frequency of 50 kHz for 10 min to obtain a uniformly mixed reaction solution, transfer the reaction solution to a reactor, place the reactor in a muffle furnace and react at 200° C. for 8 h, take out the reactor after the reaction, and cool to room temperature to obtain a MOF positive electrode additive.
[0030] Preparation of positive electrode lead paste containing MOF positive electrode additive: 0.2 g of graphite, 0.2 g of stannous sulfate, 1 g of antimony trioxide, 0.8 g of short fibers, and 10 g of water were added to the mixer, and mixed at a speed of 150 rpm for 2 min to obtain a uniformly mixed mixture A. Subsequently, 8 g of red lead was added to the mixer, and mixed at a speed of 150 rpm for 10 min to obtain a uniformly mixed mixture B. 200 g of lead powder was added to the mixer, and mixed at a speed of 200 rpm for 10 min. While mixing, 1 g of the MOF positive electrode additive prepared above was sprayed into the mixer by high-pressure spraying. After the end, a positive electrode lead paste containing a MOF positive electrode additive was obtained, and its apparent density was 4.9 g / cm3.
[0031] Example 5
[0032] Add 250 mL of deionized water to the No. 1 ultrasonic cleaner, and then add 33 g of nickel sulfate hexahydrate (0.05 mol / L), mix at a frequency of 50 kHz for 5 minutes to obtain a uniformly dissolved nickel sulfate solution; then add 108 g of zinc sulfate heptahydrate (0.15 mol / L) to the nickel sulfate solution, mix at a frequency of 50 kHz for 5 minutes to obtain a uniformly dissolved mixed solution; add 250 mL of deionized water to the No. 2 ultrasonic cleaner, and then add 103 g of 2-methylimidazole, mix at a frequency of 50 kHz for 5 minutes to obtain a uniformly dissolved 2-methylimidazole solution, transfer the mixed solution in the No. 1 ultrasonic cleaner to the No. 2 ultrasonic cleaner and mix with the 2-methylimidazole solution, mix at a frequency of 50 kHz for 10 minutes to obtain a uniformly mixed reaction solution, transfer the reaction solution to a reactor, place the reactor in a muffle furnace and react at 240° C. for 4 hours, take out the reactor after the reaction, and cool to room temperature to obtain a MOF positive electrode additive.
[0033] Preparation of positive electrode lead paste containing MOF positive electrode additive: 0.2 g of graphite, 0.2 g of stannous sulfate, 1 g of antimony trioxide, 0.8 g of short fibers, and 10 g of water were added to the mixer, and mixed at a speed of 150 rpm for 2 min to obtain a uniformly mixed mixture A. Subsequently, 8 g of red lead was added to the mixer, and mixed at a speed of 150 rpm for 10 min to obtain a uniformly mixed mixture B. 200 g of lead powder was added to the mixer, and mixed at a speed of 200 rpm for 10 min. While mixing, 1 g of the MOF positive electrode additive prepared above was sprayed into the mixer by high-pressure spraying. After the end, a positive electrode lead paste containing a MOF positive electrode additive was obtained, and its apparent density was 5.2 g / cm3.
[0034] Comparative Example 1 Preparation of positive electrode lead paste: Compared with the positive electrode paste containing MOF positive electrode additive prepared in Example 3, the only difference is that the MOF positive electrode additive is not added; finally, the positive electrode paste is prepared.
[0035] The positive electrode lead pastes containing MOF positive electrode additives prepared in Examples 1-5 and the positive electrode lead paste prepared in Comparative Example 1 were subjected to performance tests, and the test method was as follows: The positive electrode lead paste containing MOF positive electrode additive prepared in Examples 1-5 was coated, cured, assembled, and formed to finally obtain a lead-acid battery. The Tafel method was then used to test the corrosion resistance of the prepared lead-acid battery plates. The test results are shown in FIG. Figure 1 In addition, the impedance of the prepared lead-acid battery was tested, and the test results are shown in Figure 2 As shown, the impedance test results are fitted and obtained as follows Figure 3 The equivalent circuit diagram is shown.
[0036] right Figure 1 By analyzing the data in, it can be known that the cooked electrode plates of the lead-acid batteries prepared with the positive electrode lead paste containing MOF positive electrode additives prepared in Examples 1-5 have lower corrosion resistance current and more positive corrosion resistance potential than the cooked electrode plates of the lead-acid batteries prepared with the positive electrode lead paste prepared in Comparative Example 1. The smaller the corrosion resistance current, the slower the corrosion rate of the electrode plate, the more positive the corrosion resistance potential, the smaller the possibility of corrosion of the electrode plate, and the longer the service life. It can be known that the cooked electrode plates of the lead-acid batteries prepared with the positive electrode lead paste containing MOF positive electrode additives prepared in Examples 1-5 have better corrosion resistance and longer service life.
[0037] right Figure 2-3 The data in are analyzed, and the fitting results of the impedance test are listed in Table 1. Table 1 is as follows:
[0038] By analyzing the data in Table 1, it can be known that the lead-acid battery prepared with the positive electrode lead paste containing MOF positive electrode additives prepared in Examples 1-5 has smaller internal resistance and charge transfer resistance than the lead-acid battery prepared with the positive electrode lead paste prepared in Comparative Example 1. The smaller the resistance, the better the performance of the battery. It can be seen that the lead-acid battery prepared with the positive electrode lead paste containing MOF positive electrode additives prepared in Examples 1-5 has better performance.
[0039] In summary, the MOF cathode additive of the present invention has a longer service life and a higher specific energy.
[0040] In the description of the present invention, it should be understood that the terms "upper", "lower", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction and a specific direction structure and operation, and therefore, cannot be understood as a limitation on the present invention. In addition, "first" and "second" are only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0041] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", etc. should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0042] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A MOF cathode additive, characterized in that: The invention comprises the following raw materials in parts by weight: 3-33 parts of acidic nickel salt, 10-108 parts of acidic zinc salt, 10-103 parts of 2-methylimidazole, and 500 parts of deionized water.
2. The MOF cathode additive according to claim 1, characterized in that: The acidic nickel salt is nickel sulfate hexahydrate, and the acidic zinc salt is zinc sulfate heptahydrate.
3. The MOF cathode additive according to claim 2, characterized in that: The molar concentration of the nickel sulfate hexahydrate is 0.05-0.5 mol / L, and the molar concentration of the zinc sulfate heptahydrate is 0.15-1.5 mol / L.
4. A method for preparing the MOF cathode additive according to any one of claims 1 to 3, characterized in that: The method comprises the following preparation steps: S1: adding an acidic nickel salt into half of the deionized water to fully dissolve to form a nickel salt solution, and adding an acidic zinc salt into the nickel salt solution to fully dissolve to form a mixed solution; S2: adding 2-methylimidazole to the remaining deionized water to fully dissolve it to form a 2-methylimidazole solution, and then mixing the mixed solution with the 2-methylimidazole solution to obtain a reaction solution; S3: The reaction solution is transferred to a reactor, and the reactor is placed in a heating furnace at 100-240° C. to react for 4-16 hours. After the reaction is completed, the reactor is taken out and cooled to room temperature to obtain a MOF positive electrode additive.
5. The method for preparing the MOF cathode additive according to claim 4, characterized in that: In steps S1-S2, the nickel salt solution, the mixed solution, the 2-methylimidazole solution and the reaction solution are all fully mixed and dissolved by an ultrasonic cleaner.
6. The method for preparing the MOF cathode additive according to claim 4, characterized in that: In step S3, the heating furnace is a muffle furnace.
7. A positive electrode lead paste containing the MOF positive electrode additive according to any one of claims 1 to 3, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of lead powder, 6-8 parts of red lead, 0.1-0.2 parts of graphite, 0.1-0.2 parts of stannous sulfate, 0.05-1 parts of antimony trioxide, 0.2-0.8 parts of short fibers, 1-10 parts of water, and 1 part of MOF positive electrode additive.
8. The positive electrode lead paste containing MOF positive electrode additive according to claim 7, characterized in that: Its preparation method is: Step 1: Evenly mix graphite, stannous sulfate, antimony trioxide, short fibers and water to form a mixture A; Step 2: Add mixture A to red lead and stir to mix evenly to obtain mixture B, add mixture B to lead powder and stir to mix, during the stirring and mixing process, add MOF additive by high pressure spraying and stir to mix evenly to finally obtain positive electrode lead paste.
9. The positive electrode lead paste containing MOF positive electrode additive according to claim 7, characterized in that: The apparent density of the positive electrode lead paste is 3.6-5.2 g / cm 3 .