Foil for inhibiting head lithium precipitation or sodium precipitation as well as preparation method and application of foil

By forming pits and blind holes on the foil and coating lithium titanate and graphene, the problem of lithium or sodium degradation on the battery head is solved, improving the adhesion and safety of the battery, reducing heating and Lithium/sodium excision risk.

CN118970065APending Publication Date: 2024-11-15ANQING CHAOREN ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410980675.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The battery head position causes severe heat due to the convergence of current, and the negative electrode edge is prone to lithium or sodium dissipation, resulting in poor adhesion, peeling, battery short circuit failure, and even causing safety risks such as fire.

Method used

Using a foil with pits and blind holes, the surface of the pit is coated with a coating of lithium titanate and graphene, and a small pore structure is formed by stamping and chemical etching, which increases the adhesion and reduces heat generation.

Benefits of technology

Significantly reduce the heat at the head of the battery cell, improve the adhesion of the negative electrode active substance, effectively inhibit lithium/sodium evolution, and improve the circulation performance and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970065A_ABST
    Figure CN118970065A_ABST
Patent Text Reader

Abstract

The invention relates to the field of batteries, and provides a foil for inhibiting lithium precipitation or sodium precipitation of a head as well as a preparation method and application of the foil aiming at the problem of lithium precipitation or sodium precipitation of the head of a battery. Pits are formed in the surface of the foil, blind holes are formed in the surfaces of the pits, a first coating layer is arranged on the surfaces of the pits, the first coating layer contains lithium titanate, the size of the pits is 1.1-2 times of the particle size D50 of the lithium titanate, and the size of the blind holes is 1-20% of the size of the pits. The preparation method of the foil material comprises the following steps: stamping the foil material to form pits in the surface of the foil material; corroding the position of the pit with a chemical reagent, and forming a blind hole in the surface of the pit; and coating slurry on the surfaces of the pits. When the foil is applied to a negative plate or a battery, the heating of the head of a battery cell can be greatly reduced, the binding power of active substances at the head of the negative electrode is improved, and lithium / sodium precipitation at the head of the battery cell is effectively inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of batteries, and in particular to a foil material for inhibiting lithium or sodium deposition at the head, and a preparation method and application thereof. Background Art

[0002] Whether it is a lithium-ion battery or a sodium-ion battery, since the current collector or the tabs are at the head or two ends of the battery, the current is collected at the head of the battery, causing severe heating at the head of the battery. In addition, due to the edge effect of the electrode, the surface density of the electrode gradually decreases as it approaches the current collector. Especially for the negative electrode, the surface density at the edge decreases, which means that lithium or sodium is easily precipitated at this location. Especially when the heat is severe, the electrochemical reaction activity is higher, the adhesion of the active material at the head of the negative electrode becomes worse, and it is easy to peel off. The head of the negative electrode is more likely to precipitate lithium or sodium, pierce the diaphragm, and cause the battery to short-circuit and fail. In severe cases, it may cause safety risks such as fire and explosion.

[0003] At present, the method of coating the negative electrode edge with high gram capacity active materials is mainly used to treat the sodium precipitation at the head of the battery. For example, patent CN117476867A discloses a negative electrode sheet and its preparation method and secondary battery for improving edge lithium or sodium precipitation. By using a first carbon material with a smaller discharge gram capacity in the middle area of ​​the current collector surface and a second carbon material with a larger discharge gram capacity in the two edge areas of the current collector surface, the surface capacity of the edge area and the interface state of the edge electrode sheet are improved, thereby improving the lithium / sodium storage capacity of the edge area. Although this method can alleviate the edge lithium / sodium precipitation to a certain extent, the problems of edge heating and easy peeling of the head active material still exist. Therefore, an ideal solution is needed. Summary of the invention

[0004] In order to overcome the problem of lithium or sodium deposition at the head of a battery, the present invention provides a foil material for inhibiting lithium or sodium deposition at the head, and a preparation method and application thereof, which greatly reduces the heat generation at the head of a battery cell, improves the bonding force of the active material at the head of the negative electrode, and effectively inhibits lithium / sodium deposition at the head of the battery cell.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A foil material for inhibiting lithium or sodium deposition on a head, wherein a pit is arranged on the surface of the foil material, a blind hole is arranged on the surface of the pit, a coating layer 1 is arranged on the surface of the pit, the coating layer 1 contains lithium titanate, the size of the pit is 1.1-2 times the particle size D50 of the lithium titanate, and the size of the blind hole is 1-20% of the size of the pit.

[0006] Preferably, the depth of a single pit is 5-37% of the thickness of the foil material. When the foil material thickness is 8-20 μm, the pit depth is 1-3 μm.

[0007] Preferably, pits are provided on both the front and back sides of the foil; and further preferably, the pits on the front and back sides of the foil are symmetrically arranged.

[0008] Preferably, the pit is a cylinder or a spherical segment (a spherical segment refers to a portion obtained by cutting a sphere with a plane).

[0009] Preferably, a plurality of pits are arranged adjacent to each other in rows, a plurality of rows are arranged in a rectangular array, and a distance between adjacent pits is 10-100 μm.

[0010] Preferably, the pit is located at the head of the foil, 5-20mm away from the edge of the foil head, and the width of the area where the pit is located is 2-10mm. That is, a 5-20mm wide tab blank area is left at the edge of the foil, and a 2-10mm wide processing area is provided adjacent to the tab blank area; the pits and blind holes are located in the processing area, the total area of ​​the pits on a single side accounts for 50-80% of the processing area, and the total area of ​​the blind holes accounts for 20-50% of the total area of ​​the processing area; the processing area is provided with a coating layer 1.

[0011] Preferably, the coating layer 1 contains lithium titanate and graphene; the particle size D50 of the lithium titanate is 1-10 μm; the graphene is a single-layer graphene with a tube diameter of 1-5 nm and a tube length of 1-10 μm; the mass ratio of lithium titanate to graphene is (98-99.9):(0.1-2), and the thickness of the coating layer 1 is 1-5 μm.

[0012] Preferably, the slurry of coating layer one is composed of a mixture of lithium titanate and graphene, a conductive agent, and a binder in a mass ratio of (85-95):(3-7):(2-8).

[0013] Preferably, the foil material is one of aluminum foil, copper foil and copper tape.

[0014] The present invention also provides a method for preparing the foil for inhibiting lithium or sodium deposition on the head, comprising the following steps: punching the foil to form a pit on the surface of the foil; corroding the location of the pit with a chemical reagent to form a blind hole on the surface of the pit; and coating the surface of the pit with slurry.

[0015] Preferably, the chemical reagent is a mixed solution of silver sulfate and silver nitrate, the mass fraction of the mixed solution is 3-10%, and the molar ratio of silver sulfate to silver nitrate is (1-2):1; the corrosion conditions are: the chemical reagent is heated to 70-100°C and treated for 3-10 minutes.

[0016] The present invention also provides application of the foil material for inhibiting lithium or sodium deposition at the head, which is used for negative electrode sheets.

[0017] Preferably, a 5-20 mm wide tab blank area is left at the edge of the foil, and a 2-10 mm wide processing area is provided adjacent to the tab blank area; the pits and blind holes are located in the processing area; a coating layer 1 is provided in the processing area; and the positions on the foil except the tab blank area are coated with negative electrode active material slurry to obtain a negative electrode sheet.

[0018] Preferably, the negative electrode active material slurry includes a negative electrode active material, a binder, a conductive agent, and a solvent.

[0019] Preferably, the negative electrode active material is one or more of natural graphite, artificial graphite, soft carbon, and hard carbon; the binder is one or more of sodium carboxymethyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, polyacrylic acid, polytetrafluoroethylene, and polyethylene oxide; the conductive agent is one or more of activated carbon, conductive carbon black, carbon nanotubes, graphene, and vapor-grown carbon fibers.

[0020] Preferably, the mass ratio of the negative electrode active material, the conductive agent and the binder is (85-95):(3-10):(2-5).

[0021] The present invention also provides the application of the foil material or negative electrode sheet for inhibiting lithium or sodium deposition at the head, which is used in batteries.

[0022] Preferably, the negative electrode sheet, the positive electrode sheet and the separator are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery.

[0023] Preferably, the separator is one of PP, PE, non-woven fabric or a composite thereof.

[0024] Therefore, the beneficial effects of the present invention are as follows: (1) the small circular holes formed by the stamping process of the foil can increase the contact area between the slurry and the foil, greatly slowing down the peeling of the coating material and the foil, and the aperture size of the circular hole can form a better matching coating with the particle size of the material, so that the contact is better and the bonding force is greatly increased; (2) A mixed solution of silver sulfate and silver sulfate can effectively etch the foil to form micropores, which not only increases the adhesion between the foil and the material, but also the deposited silver can provide better thermal conductivity and reduce heat generation; (3) Spinel-type lithium titanate has three-dimensional channels and excellent rate performance, which can achieve charging and discharging at high rate currents. In addition, the lithium / sodium insertion potential of lithium titanate is relatively high and lithium / sodium precipitation will not occur. Graphene has excellent electrical and thermal conductivity, which can not only improve the conductivity of lithium titanate, but also reduce heat accumulation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the foil before coating.

[0026] Figure 2This is a cross-sectional view of the foil after coating.

[0027] In the figure, 1, blank area of ​​the tab, 2, processing area, 21, pit, 22, blind hole, 3, coating layer one, 4, coating layer two. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below through specific embodiments.

[0029] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the embodiments, unless otherwise specified, are all conventional methods in the art. Unless otherwise specified, parts are all weight parts, temperatures are expressed in ° C or at ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. There are many variations and combinations of reaction conditions (such as component concentrations, desired solvents, solvent mixtures, temperatures, pressures, and other reaction ranges) and conditions that can be used to optimize the purity and yield of the product obtained by the method, and only reasonable routine experiments will be required to optimize such method conditions.

[0030] Example 1. A method for preparing foil Take a piece of aluminum foil / copper foil / copper strip with a thickness of 8-20μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 5-20mm; the width of the processing area is 2-10mm; the width of the coating area is 100-800mm.

[0031] The treatment method for the treatment area is: (1) Stamping pits Punch pits are punched out on the surface of the treatment area by a punching machine. A single pit is a cylinder or a spherical segment (a spherical segment refers to the part obtained by cutting a sphere with a plane), the size of which is 1.1-2 times the D50 of the lithium titanate or graphene particle size, and the depth of a single pit is 1-3 μm, accounting for 5-37% of the thickness of the foil.

[0032] Several pits are arranged in adjacent rows, several rows are arranged in a rectangular array, the spacing between adjacent pits is 10-100 μm; the total area of ​​the pits on a single surface accounts for 50-80% of the area of ​​the processing area.

[0033] The front and back sides of the foil are both punched with pits, and the pits on the front and back sides are preferably symmetrically arranged, and the punching machine is a double-sided continuous round hole punching machine.

[0034] (2) Etching blind holes with chemical reagents A mixed solution of silver sulfate and silver nitrate with a mass fraction of 3-10% is prepared, wherein the molar ratio of silver sulfate to silver nitrate is (1-2):1, and heated to 70-100° C.; the treated area of ​​the foil punched in step (1) is treated with the heated mixed solution for 3-10 minutes to form small blind holes on the surface of the treated area, wherein the size of a single blind hole accounts for 1-20% of the size of a single pit; and the total area of ​​the blind holes accounts for 20-50% of the total area of ​​the treated area.

[0035] (3) Coating The slurry for coating layer 1 is prepared, and the slurry is composed of a mixture of lithium titanate and graphene, a conductive agent, and a binder in a mass ratio of (85-95):(3-7):(2-8). The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 1-10 μm; the graphene is a single layer, the tube diameter is 1-5 nm, and the tube length is 1-10 μm. The mass ratio of lithium titanate to graphene is 98:2 to 99.9:0.1.

[0036] The slurry prepared above is coated on the treated area to form a coating layer 1, with a coating thickness of 1-5 μm on one side and double-sided coating.

[0037] 2. Use foil to make negative electrode sheets The negative electrode active material is mixed evenly with a binder, a conductive agent, and a solvent, dispersed at high speed to form a negative electrode active material slurry, which is evenly coated on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0038] The mass ratio of the negative electrode active material, the conductive agent and the binder is (85-95):(3-10):(2-5). The negative electrode active material is one or more of natural graphite, artificial graphite, soft carbon and hard carbon; the binder is one or more of sodium carboxymethyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, polyacrylic acid, polytetrafluoroethylene and polyethylene oxide; the conductive agent is one or more of activated carbon, conductive carbon black, carbon nanotubes, graphene and vapor-grown carbon fiber.

[0039] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in the second step are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is one of PP, PE, non-woven fabric or a composite.

[0040] Example 1 1. A method for preparing foil like Figure 1As shown, a piece of aluminum foil with a thickness of 15 μm is taken as the foil material. From one side to the corresponding side, the foil material is the tab blank area 1, the processing area 2 and the coating area. The width of the tab blank area 1 is 10 mm; the width of the processing area 2 is 6 mm; and the width of the coating area is 400 mm.

[0041] The treatment method for treatment area 2 is: (1) Punching pit 21 A punching machine is used to punch out pits 21 on the surface of the treatment area 2. A single pit is a spherical segment, and the horizontal size of the spherical segment is 1.5 times the particle size D50 of lithium titanate. The depth of a single pit 21 is 2 μm, accounting for 13% of the thickness of the foil.

[0042] A plurality of pits 21 are arranged adjacent to each other in rows, and two rows are arranged in a rectangular array. The spacing between adjacent pits 21 is 60 μm. The total area of ​​the pits on a single surface accounts for 60% of the area of ​​the processing zone.

[0043] The front and back sides of the foil are both punched with pits 21, and the pits 21 on the front and back sides are symmetrically arranged, and the punching machine is a double-sided continuous round hole punching machine.

[0044] (2) Use chemical reagents to etch out blind holes 22 A mixed solution of silver sulfate and silver nitrate with a mass fraction of 10% is prepared, wherein the molar ratio of silver sulfate to silver nitrate is 1:1, and heated to 100° C. The treated area 2 of the foil punched in step (1) is treated with the heated mixed solution for 10 minutes to form small blind holes 22 on the surface of the treated area 2, wherein the size of a single blind hole 22 accounts for 20% of the size of a single pit 21; and the total area of ​​the blind holes 22 accounts for 40% of the total area of ​​the treated area 2.

[0045] (3) Coating The slurry for coating layer 13 is prepared, and the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 6 μm; the graphene is a single layer, the tube diameter is 3 nm, and the tube length is 5 μm. The mass ratio of lithium titanate to graphene is 98:2.

[0046] like Figure 2 As shown, the slurry prepared above is coated on the treatment area 2 to form a coating layer 3, the coating thickness on one side is 2 μm, and the double-sided coating is performed.

[0047] 2. Use foil to make negative electrode sheets The negative electrode active material is mixed evenly with a binder, a conductive agent, and a solvent, dispersed at high speed to form a negative electrode active material slurry, which is evenly coated on the foil obtained in step 1 (the blank area 1 of the tab is not coated) to form a coating layer 2 4 with a smooth surface to obtain a negative electrode sheet.

[0048] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0049] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0050] Example 2 1. A method for preparing foil A piece of copper foil with a thickness of 8 μm is taken as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 5 mm; the width of the processing area is 2 mm; and the width of the coating area is 100 mm.

[0051] The treatment method for the treatment area is: (1) Stamping pits A punching machine is used to punch out pits on the surface of the treatment area. A single pit is a cylinder, the diameter of the cylinder is 1.5 times the diameter D50 of the lithium titanate particle, and the depth of a single pit is 2.96 μm, accounting for 37% of the thickness of the foil.

[0052] Several pits are arranged in adjacent rows, and two rows are arranged in a rectangular array. The spacing between adjacent pits is 10 μm; the total area of ​​the pits on a single surface accounts for 50% of the area of ​​the processing area.

[0053] The front and back sides of the foil are both punched with pits, and the pits on the front and back sides are symmetrically arranged.

[0054] (2) Etching blind holes with chemical reagents A mixed solution of silver sulfate and silver nitrate with a mass fraction of 3% is prepared, wherein the molar ratio of silver sulfate to silver nitrate is 1:1, and heated to 70° C. The treated area of ​​the foil punched in step (1) is treated with the heated mixed solution for 3 minutes to form small blind holes on the surface of the treated area, wherein the size of a single blind hole accounts for 1% of the size of a single pit; and the total area of ​​the blind holes accounts for 20% of the total area of ​​the treated area.

[0055] (3) Coating The slurry for coating layer 1 is prepared, and the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 85:7:8. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12The structure is spinel type, the particle size D50 of lithium titanate is 1 μm; the graphene is a single layer, the tube diameter is 1 nm, and the tube length is 1 μm. The mass ratio of lithium titanate to graphene is 99.9:0.1.

[0056] The slurry prepared above is coated on the treated area to form a coating layer 1, with a coating thickness of 1 μm on one side and double-sided coating.

[0057] 2. Use the foil to make negative electrode sheets: Evenly mix the negative electrode active material with the binder, conductive agent and solvent, disperse them at high speed to make negative electrode active material slurry, and evenly coat the slurry on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0058] The mass ratio of the negative electrode active material, the conductive agent and the binder is 85:10:5. The negative electrode active material is soft carbon, the binder is polyethylene oxide, and the conductive agent is carbon nanotubes.

[0059] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0060] Example 3 1. A method for preparing foil Take a piece of copper foil with a thickness of 20μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 20mm; the width of the processing area is 10mm; and the width of the coating area is 800mm.

[0061] The treatment method for the treatment area is: (1) Stamping pits A punching machine is used to punch out pits on the surface of the treatment area. A single pit is a cylinder, the diameter of the cylinder is twice the diameter D50 of the lithium titanate particle, and the depth of a single pit is 1 μm, accounting for 5% of the thickness of the foil.

[0062] Several pits are arranged in adjacent rows, and three rows are arranged in a rectangular array. The spacing between adjacent pits is 100 μm; the total area of ​​the pits on a single surface accounts for 80% of the area of ​​the processing area.

[0063] The front and back sides of the foil are both punched with pits, and the pits on the front and back sides are symmetrically arranged.

[0064] (2) Etching blind holes with chemical reagents A mixed solution of silver sulfate and silver nitrate with a mass fraction of 10% is prepared, wherein the molar ratio of silver sulfate to silver nitrate is 2:1, and the solution is heated to 100° C. The treated area of ​​the foil punched in step (1) is treated with the heated mixed solution for 10 minutes to form small blind holes on the surface of the treated area, wherein the size of a single blind hole accounts for 20% of the size of a single pit; and the total area of ​​the blind holes accounts for 50% of the total area of ​​the treated area.

[0065] (3) Coating The slurry for coating layer 1 is prepared, and the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 95:3:2. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 10 μm; the graphene is a single layer, the tube diameter is 5 nm, and the tube length is 10 μm. The mass ratio of lithium titanate to graphene is 99:1.

[0066] The slurry prepared above is coated on the treated area to form a coating layer 1, with a coating thickness of 5 μm on one side and double-sided coating.

[0067] 2. Use the foil to make negative electrode sheets: Evenly mix the negative electrode active material with the binder, conductive agent and solvent, disperse them at high speed to make negative electrode active material slurry, and evenly coat the slurry on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0068] The mass ratio of the negative electrode active material, the conductive agent and the binder is 95:3:2. The negative electrode active material is soft carbon and hard carbon (mass ratio is 1:1), the binder is sodium carboxymethyl cellulose, and the conductive agent is conductive carbon black and carbon nanotubes (mass ratio is 1:1).

[0069] 3. Using the negative electrode sheet to make a battery: The negative electrode sheet prepared in step 2 is wound or stacked with the positive electrode sheet and the separator to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is a non-woven fabric.

[0070] Comparative Example Comparative Example 1 The difference from Example 1 is that there are no punching pits and corrosion blind holes.

[0071] 1. A method for preparing foil Take a piece of aluminum foil with a thickness of 15μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 10mm; the width of the processing area 2 is 6mm; and the width of the coating area is 400mm.

[0072] The treatment method of the treatment area is: prepare a slurry of the coating layer 1, the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 6 μm; the graphene is a single layer, the tube diameter is 3 nm, and the tube length is 5 μm. The mass ratio of lithium titanate to graphene is 98:2. The slurry prepared above is coated on the treatment area to form a coating layer 1, the coating thickness of one side is 2 μm, and the double-sided coating is performed.

[0073] 2. Use foil to make negative electrode sheets The negative electrode active material is mixed evenly with a binder, a conductive agent, and a solvent, dispersed at high speed to form a negative electrode active material slurry, which is evenly coated on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 24 with a smooth surface to obtain a negative electrode sheet.

[0074] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0075] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0076] Comparative Example 2 The difference from Example 1 is that there are punched pits but no corrosion blind holes.

[0077] 1. A method for preparing foil Take a piece of aluminum foil with a thickness of 15μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 10mm; the width of the processing area is 6mm; and the width of the coating area is 400mm.

[0078] The treatment method for the treatment area is: (1) Stamping pits A punching machine is used to punch out pits on the surface of the treatment area. A single pit is a spherical segment, the horizontal size of the spherical segment is 1.5 times the particle size D50 of lithium titanate, and the depth of a single pit is 2 μm, accounting for 13% of the thickness of the foil.

[0079] Several pits are arranged in adjacent rows, and two rows are arranged in a rectangular array. The spacing between adjacent pits is 60 μm; the total area of ​​the pits on a single surface accounts for 60% of the area of ​​the processing area.

[0080] The front and back sides of the foil are both punched with pits, and the pits on the front and back sides are symmetrically arranged. The punching machine is a double-sided continuous circular hole punching machine.

[0081] (2) Coating The slurry for coating layer 1 is prepared, and the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 6 μm; the graphene is a single layer, the tube diameter is 3 nm, and the tube length is 5 μm. The mass ratio of lithium titanate to graphene is 98:2.

[0082] The slurry prepared above is coated on the treated area to form a coating layer 1, the coating thickness on one side is 2 μm, and the coating is performed on both sides.

[0083] 2. Use the foil to make negative electrode sheets: Evenly mix the negative electrode active material with the binder, conductive agent and solvent, disperse them at high speed to make negative electrode active material slurry, and evenly coat the slurry on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0084] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0085] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0086] Comparative Example 3 The difference from Example 1 is that there are no punching pits but there are corrosion blind holes.

[0087] 1. A method for preparing foil Take a piece of aluminum foil with a thickness of 15μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 10mm; the width of the processing area is 6mm; and the width of the coating area is 400mm.

[0088] The treatment method for treatment area 2 is: (1) Etching blind holes with chemical reagents A mixed solution of silver sulfate and silver nitrate with a mass fraction of 10% was prepared, wherein the molar ratio of silver sulfate to silver nitrate was 1:1, and heated to 100° C. The treated area of ​​the foil was treated with the heated mixed solution for 10 minutes to form small blind holes on the surface of the treated area; the total area of ​​the blind holes accounted for 40% of the total area of ​​the treated area.

[0089] (2) Coating The slurry for coating layer 1 is prepared, and the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 6 μm; the graphene is a single layer, the tube diameter is 3 nm, and the tube length is 5 μm. The mass ratio of lithium titanate to graphene is 98:2.

[0090] The slurry prepared above is coated on the treated area to form a coating layer 1, the coating thickness on one side is 2 μm, and the coating is performed on both sides.

[0091] 2. Use the foil to make negative electrode sheets: Evenly mix the negative electrode active material with the binder, conductive agent and solvent, disperse them at high speed to make negative electrode active material slurry, and evenly coat the slurry on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0092] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0093] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0094] Comparative Example 4 The difference from Example 1 is that the size of the pit is too large, which is 3 times of lithium titanate D50 and exceeds the preferred range by 1.1-2 times.

[0095] Comparative Example 5 The difference from Example 1 is that the size of the blind holes is too large, and the size of a single blind hole accounts for 30% of the size of a single pit, which exceeds the preferred range of 1-20%.

[0096] 1. A method for preparing foil Take a piece of aluminum foil with a thickness of 15μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 10mm; the width of the processing area is 6mm; and the width of the coating area is 400mm.

[0097] The treatment method for treatment area 2 is: (1) Punching pit 21 A punching machine is used to punch out pits 21 on the surface of the treatment area. A single pit is a spherical segment, and the horizontal size of the spherical segment is 1.5 times the particle size D50 of lithium titanate. The depth of a single pit is 2 μm, accounting for 13% of the thickness of the foil.

[0098] Several pits are arranged in adjacent rows, and two rows are arranged in a rectangular array. The spacing between adjacent pits is 60 μm; the total area of ​​the pits on a single surface accounts for 60% of the area of ​​the processing area.

[0099] The front and back sides of the foil are punched with pits, and the pits on the front and back sides are symmetrically arranged. The punching machine is a double-sided continuous round hole type punching machine.

[0100] (2) Etching blind holes with chemical reagents A mixed solution of silver sulfate and silver nitrate with a mass fraction of 20% is prepared, wherein the molar ratio of silver sulfate to silver nitrate is 1:1, and heated to 100° C. The treated area of ​​the foil punched in step (1) is treated with the heated mixed solution for 20 minutes to form small blind holes on the surface of the treated area, wherein the size of a single blind hole is approximately 30% of the size of a single pit 21; and the total area of ​​the blind holes accounts for 50% of the total area of ​​the treated area.

[0101] (3) Coating a slurry for coating layer 1, the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 6 μm; the graphene is a single layer, the tube diameter is 3 nm, and the tube length is 5 μm. The mass ratio of lithium titanate to graphene is 98:2.

[0102] The slurry prepared above is coated on the treated area to form a coating layer 1, with a coating thickness of 2 μm on one side and double-sided coating.

[0103] 2. Use foil to make negative electrode sheets The negative electrode active material is mixed evenly with a binder, a conductive agent, and a solvent, dispersed at high speed to form a negative electrode active material slurry, which is evenly coated on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0104] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0105] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0106] Comparative Example 6 The difference from Example 1 is that the etching reagents are acid solution and alkali solution in sequence. The pickling solution is 1.1wt% HF and 2.9wt% H 2 SO 4 , the alkaline washing solution is 0.8wt%Ca(OH) 2 and 3.2 wt% LiOH.

[0107] 1. A method for preparing foil Take a piece of aluminum foil with a thickness of 15μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 10mm; the width of the processing area is 6mm; and the width of the coating area is 400mm.

[0108] The treatment method for treatment area 2 is: (1) Punching pit 21 A punching machine is used to punch out pits 21 on the surface of the treatment area. A single pit is a spherical segment, and the horizontal size of the spherical segment is 1.5 times the particle size D50 of lithium titanate. The depth of a single pit is 2 μm, accounting for 13% of the thickness of the foil.

[0109] Several pits are arranged in adjacent rows, and two rows are arranged in a rectangular array. The spacing between adjacent pits is 60 μm; the total area of ​​the pits on a single surface accounts for 60% of the area of ​​the processing area.

[0110] The front and back sides of the foil are punched with pits, and the pits on the front and back sides are symmetrically arranged. The punching machine is a double-sided continuous round hole type punching machine.

[0111] (2) Etching blind holes with chemical reagents Prepare 1.1wt% HF and 2.9wt% H 2 SO 4 Mixed pickling solution, 0.8wt% Ca(OH) 2 and a mixed alkaline washing solution containing 3.2 wt % LiOH, and the treated area of ​​the foil punched in step (1) is treated with the mixed acid washing solution and the mixed alkaline washing solution for 10 min each, to form small blind holes on the surface of the treated area.

[0112] (3) Coating The slurry for coating layer 1 is prepared, and the slurry is composed of a mixture of lithium titanate and graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type, the particle size D50 of lithium titanate is 6 μm; the graphene is a single layer, the tube diameter is 3 nm, and the tube length is 5 μm. The mass ratio of lithium titanate to graphene is 98:2.

[0113] The slurry prepared above is coated on the treated area to form a coating layer 1, with a coating thickness of 2 μm on one side and double-sided coating.

[0114] 2. Use the foil to make negative electrode sheets: Evenly mix the negative electrode active material with the binder, conductive agent and solvent, disperse them at high speed to make negative electrode active material slurry, and evenly coat the slurry on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0115] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0116] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0117] Comparative Example 7 The difference from Example 1 is that there is no coating layer 1 on the surface of the pit.

[0118] Comparative Example 8 The difference from Example 1 is that the coating layer 1 contains lithium titanate but no graphene.

[0119] 1. A method for preparing foil Take a piece of aluminum foil with a thickness of 15μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 10mm; the width of the processing area is 6mm; and the width of the coating area is 400mm.

[0120] The treatment method for treatment area 2 is: (1) Punching pit 21 A punching machine is used to punch out pits 21 on the surface of the treatment area. A single pit is a spherical segment, and the horizontal size of the spherical segment is 1.5 times the particle size D50 of lithium titanate. The depth of a single pit is 2 μm, accounting for 13% of the thickness of the foil.

[0121] Several pits are arranged in adjacent rows, and two rows are arranged in a rectangular array. The spacing between adjacent pits is 60 μm; the total area of ​​the pits on a single surface accounts for 60% of the area of ​​the processing area.

[0122] The front and back sides of the foil are punched with pits, and the pits on the front and back sides are symmetrically arranged. The punching machine is a double-sided continuous round hole type punching machine.

[0123] (2) Etching blind holes with chemical reagents A mixed solution of silver sulfate and silver nitrate with a mass fraction of 10% is prepared, wherein the molar ratio of silver sulfate to silver nitrate is 1:1, and heated to 100° C. The treated area of ​​the foil punched in step (1) is treated with the heated mixed solution for 10 minutes to form small blind holes on the surface of the treated area, wherein the size of a single blind hole accounts for 20% of the size of a single pit 21; and the total area of ​​the blind holes accounts for 40% of the total area of ​​the treated area.

[0124] (3) Coating a slurry for coating layer 1, the slurry is composed of lithium titanate, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The molecular formula of the lithium titanate is Li 4 Ti 5 O 12 The structure is spinel type and the particle size D50 of lithium titanate is 6μm.

[0125] The slurry prepared above is coated on the treated area to form a coating layer 1, with a coating thickness of 2 μm on one side and double-sided coating.

[0126] 2. Use the foil to make negative electrode sheets: Evenly mix the negative electrode active material with the binder, conductive agent and solvent, disperse them at high speed to make negative electrode active material slurry, and evenly coat the slurry on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0127] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0128] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0129] Comparative Example 9 The difference from Example 1 is that the coating layer contains graphene instead of lithium titanate.

[0130] 1. A method for preparing foil Take a piece of aluminum foil with a thickness of 15μm as the foil material. From one side to the corresponding side, the foil material is the tab blank area, the processing area and the coating area. The width of the tab blank area is 10mm; the width of the processing area is 6mm; and the width of the coating area is 400mm.

[0131] The treatment method for treatment area 2 is: (1) Punching pit 21 A punching machine is used to punch out pits 21 on the surface of the treatment area. Each pit is a spherical segment with a horizontal dimension of 9 μm and a depth of 2 μm, accounting for 13% of the thickness of the foil.

[0132] Several pits are arranged in adjacent rows, and two rows are arranged in a rectangular array. The spacing between adjacent pits is 60 μm; the total area of ​​the pits on a single surface accounts for 60% of the area of ​​the processing area.

[0133] The front and back sides of the foil are punched with pits, and the pits on the front and back sides are symmetrically arranged. The punching machine is a double-sided continuous round hole type punching machine.

[0134] (2) Etching blind holes with chemical reagents A mixed solution of silver sulfate and silver nitrate with a mass fraction of 10% is prepared, wherein the molar ratio of silver sulfate to silver nitrate is 1:1, and heated to 100° C. The treated area of ​​the foil punched in step (1) is treated with the heated mixed solution for 10 minutes to form small blind holes on the surface of the treated area, wherein the size of a single blind hole accounts for 20% of the size of a single pit 21; and the total area of ​​the blind holes accounts for 40% of the total area of ​​the treated area.

[0135] (3) Coating a slurry for coating layer 1, the slurry is composed of graphene, conductive carbon black, and polyacrylic acid in a mass ratio of 90:5:5. The graphene is a single layer with a tube diameter of 3nm and a tube length of 5μm. The mass ratio of lithium titanate to graphene is 98:2.

[0136] The slurry prepared above is coated on the treated area to form a coating layer 1, with a coating thickness of 2 μm on one side and double-sided coating.

[0137] 2. Use foil to make negative electrode sheets The negative electrode active material is mixed evenly with a binder, a conductive agent, and a solvent, dispersed at high speed to form a negative electrode active material slurry, which is evenly coated on the foil obtained in step 1 (the blank area of ​​the tab is not coated) to form a coating layer 2 with a smooth surface to obtain a negative electrode sheet.

[0138] The mass ratio of the negative electrode active material, the conductive agent and the binder is 93:3:3. The negative electrode active material is hard carbon, the binder is polytetrafluoroethylene, and the conductive agent is conductive carbon black.

[0139] 3. Using the negative electrode sheet to make batteries The negative electrode sheet and the positive electrode sheet and the separator prepared in step 2 are wound or stacked to form a battery core, which is then baked to remove water and then filled with liquid and formed to form a battery. The separator is PP.

[0140] Performance Testing A 10Ah soft-packaged battery cell was prepared, and the battery cell performance of each embodiment and comparative example was tested. The test method was as follows: 1. Whether the head has sodium precipitation was determined by whether the head position bulged during the battery cell cycle. The sodium precipitation position had obvious bulging due to the generation of lithium metal; 2. Discharge temperature rise at the head position: a temperature recorder was used to test the temperature rise at the head position from the beginning of discharge to the end of discharge during 2C 20A discharge; 3. Adhesion of active material at the head position: a peeling force tester was used to test the adhesion; 4. Cycle performance: 0.5C 5A charging, 10min standby, 1.0C 10A discharge, 10min standby, and the above steps were repeated. The results are shown in the following table. Is there sodium precipitation in the head? Discharge temperature rise at head position / ℃ Active substance adhesion at head position / N Cycle performance / times Example 1 no 12 55 1550 Example 2 no 11 56 1610 Example 3 no 13 53 1520 Comparative Example 1 yes 23 10 590 Comparative Example 2 yes 21 28 720 Comparative Example 3 yes 19 21 780 Comparative Example 4 yes 18 24 830 Comparative Example 5 yes 16 33 840 Comparative Example 6 yes 19 49 790 Comparative Example 7 yes 28 20 620 Comparative Example 8 yes 26 50 980 Comparative Example 9 yes 14 45 760

[0141] It can be seen from the above table that the battery cells prepared in various embodiments of the present invention have excellent cycle performance.

[0142] Compared with Example 1, Comparative Examples 1-9 are not within the preferred range because the temperature rise of the head is too high and the head adhesion is poor. During the long-term cycle process, sodium is easily precipitated from the head of the battery cell, which accelerates the deterioration of the battery cell cycle performance and eventually causes the battery cell to fail. Specifically: ① Comparative Example 2 has pits but no blind holes. Although the pits can provide better adhesion than the untreated foil, the volume of the negative electrode plate changes continuously as the active lithium / sodium is continuously deintercalated during the cycle, which requires higher adhesion of the plate. Smaller blind holes can better adsorb fine slurries, improve adhesion and heat generation, and reduce the resistance to lithium / sodium insertion. If there are no blind holes, the head of the battery cell will heat up severely, the active material will peel off, and the cycle performance will not be as good as Example 1; Comparative Example 3 has blind holes but no pits. The blind holes are smaller in size, which can improve the adhesion of local points, but due to the lack of large pits, there is no improvement in the adhesion of surface contact, the active material is easy to peel off, and the cycle performance is not as good as Example 1. Therefore, the pits and blind holes cooperate with each other to achieve the effect of 1+1>2.

[0143] ② The pit size of Comparative Example 4 is too large. Because of the large size, the lithium titanate particle size is relatively small and cannot match it, and the surface contact adhesion is poor; the blind hole size of Comparative Example 5 is too large. Because the corrosion size is too large, the adhesion to the local point of the active material is poor, the active material is easy to peel off, and the cycle performance is not as good as Example 1. Therefore, the size of the pit and the blind hole is within a reasonable range, which is conducive to exerting the best beneficial effect.

[0144] ③ In Comparative Example 6, after the corrosion reagent is replaced by acid solution and alkali solution from the mixed solution of silver sulfate and silver nitrate, the blind hole size required by the present invention cannot be obtained; and without silver, the electrical and thermal conductivity of the foil in the treatment area will also decrease.

[0145] ④ Comparative Example 8: There is no graphene in the coating layer 1, because graphene can not only improve the conductivity of lithium titanate, but also reduce the accumulation of heat. Without graphene, the internal resistance of the coating area is large, the resistance to the deintercalation of active lithium / sodium increases, the temperature rise of the head becomes larger, and sodium is easily precipitated. The cycle performance is not as good as that of Example 1; Comparative Example 9: There is no lithium titanate in the coating layer 1, because lithium titanate has excellent rate performance, can achieve charging and discharging under high rate current, and lithium titanate has a high lithium / sodium intercalation potential, and will not precipitate lithium / sodium. Without lithium titanate, the negative electrode potential is low under high current or at the end of charging, and sodium is easily precipitated, causing the battery cell to fail. Therefore, the combination of graphene and lithium titanate in the coating layer 1 is better.

[0146] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A foil material for inhibiting lithium or sodium deposition at the head, characterized in that: The foil surface is provided with pits, the pit surface is provided with blind holes, the pit surface is provided with a coating layer 1, the coating layer 1 contains lithium titanate, the pit size is 1.1-2 times the lithium titanate particle size D50, and the blind hole size is 1-20% of the pit size.

2. A foil material for inhibiting lithium or sodium deposition at the head according to claim 1, characterized in that: The depth of a single pit is 5-37% of the thickness of the foil; and / or pits are provided on both the front and back sides of the foil.

3. The foil material for inhibiting lithium or sodium deposition at the head according to claim 1, characterized in that: Several pits are arranged adjacent to each other in rows, and several rows are arranged in a rectangular array, and the spacing between adjacent pits is 10-100 μm.

4. A foil material for inhibiting lithium or sodium deposition at the head according to claim 1 or 3, characterized in that: The pit is located at the head of the foil, 5-20 mm away from the edge of the foil head, and the width of the area where the pit is located is 2-10 mm.

5. The foil material for inhibiting lithium or sodium deposition at the head according to claim 1, characterized in that: The coating layer 1 contains lithium titanate and graphene; the particle size D50 of the lithium titanate is 1-10 μm; the graphene is a single-layer graphene with a tube diameter of 1-5 nm and a tube length of 1-10 μm; the mass ratio of lithium titanate to graphene is (98-99.9):(0.1-2), and the thickness of the coating layer 1 is 1-5 μm.

6. The foil material for inhibiting lithium or sodium deposition at the head according to claim 5, characterized in that: The slurry of the coating layer 1 is composed of a mixture of lithium titanate and graphene, a conductive agent, and a binder in a mass ratio of (85-95):(3-7):(2-8).

7. A method for preparing a foil material for inhibiting lithium or sodium deposition at the head according to any one of claims 1 to 6, characterized in that: The following steps are involved: The foil is punched to form pits on the surface of the foil; the location of the pits is corroded by chemical reagents to form blind holes on the surface of the pits; and slurry is coated on the surface of the pits.

8. The method for preparing a foil material for inhibiting lithium or sodium deposition at the head according to claim 7, characterized in that: The chemical reagent is a mixed solution of silver sulfate and silver nitrate, the mass fraction of the mixed solution is 3-10%, and the molar ratio of silver sulfate to silver nitrate is (1-2):1; the corrosion conditions are: the chemical reagent is heated to 70-100°C and treated for 3-10 min.

9. Use of the foil material for inhibiting lithium or sodium deposition at the head as described in any one of claims 1 to 6 in a negative electrode sheet or a battery.

10. The use according to claim 9, characterized in that: A 5-20 mm wide tab blank area is left at the edge of the foil, and a 2-10 mm wide processing area is provided adjacent to the tab blank area; the pits and blind holes are located in the processing area; a coating layer 1 is provided in the processing area; and the positions on the foil except the tab blank area are coated with negative electrode active material slurry to obtain a negative electrode sheet.