Rubidium / cesium-containing low-temperature battery electrolyte and battery thereof
By adding rubidium/cesium compounds and other additives to the battery electrolyte, the problem of battery performance attenuation at low temperatures is solved, and the efficient circulation and rate performance of the battery in cold environments is achieved.
Patent Information
- Application Number
- CN202411049862.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-01
AI Technical Summary
Under low temperature conditions, the electrolyte viscosity of polyanionic positive electrode materials increases and the conductivity decreases, resulting in severe attenuation of the application performance of batteries in cold areas and extreme fields. The improvement of the existing technology through SEI film cannot effectively ensure the low temperature ratio of the battery and Cyclic performance.
Using a low-temperature battery electrolyte containing rubidium/cesium, the viscosity and conductivity of the electrolyte are adjusted to inhibit carbonates by adding cesium compounds and/or rubidium compounds, film-forming additives, lithium salts or sodium salts and organic solvents to the electrolyte. Side reaction of solvents reduces desolvation of active ions and improves the fluidity and conductivity of the electrolyte.
It effectively extends the cycle life of the battery under low temperature conditions, improves the low temperature rate performance, reduces dendrite generation, and improves the electrochemical performance of the battery in low temperature environments.
Smart Images

Figure BDA0004974607510000091 
Figure BDA0004974607510000101 
Figure BDA0004974607510000102
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of secondary batteries, and in particular to a rubidium / cesium-containing low-temperature battery electrolyte and a battery thereof. Background Art
[0002] Polyanion positive electrode materials are widely used in electric vehicles, electrochemical energy storage and other fields due to their high safety, green environmental protection and long cycle life. However, under low temperature conditions, the viscosity of the electrolyte increases, the conductivity decreases, the electrolyte / electrode interface film impedance and charge transfer impedance increase, and the electron and ion mobility are low due to the coupling phenomenon of electrons and lattices in polyanion positive electrode materials, which leads to serious attenuation of their capacity and cycle performance under low temperature environments. Functional electrolytes can have lower viscosity and higher conductivity under low temperature conditions, reduce interface impedance, increase the migration rate of ions, slow down the formation of dendrites on the surface of the negative electrode, and improve the electrical performance of the battery under low temperature operation. This is of great significance to breaking the application barriers of polyanion positive electrode materials in cold regions and extreme fields, so it is extremely important to develop a low-temperature electrolyte and battery.
[0003] Chinese patent application CN106159324A discloses a non-aqueous electrolyte and a lithium secondary battery using the non-aqueous electrolyte. Through the cesium salt compound additive, the low temperature performance and rate performance are significantly improved while maintaining the good cycle stability of the lithium secondary battery. The functional electrolyte prepared by Chinese patent application CN108878980A significantly improves the number of charge and discharge times of the battery after adding cesium ions, effectively extending the battery life. Chinese patent application CN115842158A provides an electrolyte for a secondary battery, comprising one or more cations selected from potassium ions, rubidium ions, cesium ions, barium ions, strontium ions and calcium ions, which improves the retention of the cycle capacity and cycle life of the battery cell.
[0004] In the above scheme, the amount of rubidium and cesium ions added is relatively small, and their main function is to promote the formation of a stable and firm SEI film at the negative electrode. However, under low temperature conditions, the viscosity and conductivity of the electrolyte have a greater impact on the low temperature performance of the battery. Improving the SEI film alone cannot guarantee the rate and cycle performance of the battery at low temperatures. The conductivity, viscosity and impedance of the electrolyte are usually improved by optimizing the composition and ratio of the solvent. EC and PC promote the low temperature performance of the electrolyte, but will cause an increase in impedance, graphite co-embedded side reactions and barriers to active ion desolvation, thereby affecting the low temperature cycle performance of the battery. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention aims to provide a rubidium / cesium-containing low-temperature battery electrolyte and a battery thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A rubidium / cesium-containing low-temperature battery electrolyte comprises a cesium compound and / or a rubidium compound, a film-forming additive, a lithium salt or a sodium salt, and an organic solvent; the total molar concentration of the cesium compound and / or the rubidium compound is 0.3-1 mol / L; the content of the film-forming additive is 0.5-5wt%; and the content of the lithium salt or the sodium salt is 0-15wt%.
[0008] Furthermore, the cesium compound includes one or more of cesium hexafluorophosphate, cesium tetrafluoroborate, cesium bis(fluorosulfonyl)imide, and cesium trifluoromethanesulfonyl imide.
[0009] Furthermore, the rubidium compound includes one or more of rubidium hexafluorophosphate, rubidium tetrafluoroborate, rubidium bis(fluorosulfonyl)imide, and rubidium trifluoromethanesulfonyl imide.
[0010] Furthermore, the film-forming additive includes one or more of vinylene carbonate, fluoroethylene carbonate, tris(trimethylsilyl)phosphate, tris(trifluoroethyl)carbonate, tris(trimethylsilyl)borate, lithium difluorophosphate, and lithium difluorobisoxalatophosphate.
[0011] Furthermore, the lithium salt includes one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluorosulfonyl)imide, lithium difluorooxalatoborate, and lithium dioxalatoborate.
[0012] Furthermore, the sodium salt includes one or more of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and sodium bis(fluorosulfonyl)imide salt.
[0013] Furthermore, the organic solvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, acetonitrile, propionitrile, and butyronitrile.
[0014] The present invention also provides a battery, comprising a positive electrode, a negative electrode, a separator and the rubidium / cesium-containing low-temperature battery electrolyte according to any one of claims 1 to 7.
[0015] Furthermore, the positive electrode is composed of a positive electrode active material, a positive electrode conductive agent and a positive electrode binder; the positive electrode active material includes one or more of lithium iron phosphate, lithium iron manganese phosphate, sodium iron phosphate, sodium iron pyrophosphate, and sodium iron pyrophosphate; the positive electrode conductive agent includes one or more of single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, carbon fiber, conductive graphite, and conductive carbon black; the positive electrode binder includes polyvinylidene fluoride; the weight ratio of the positive electrode active material, the positive electrode conductive agent and the positive electrode binder is 90-94:3-5:3-5; the surface density of the positive electrode is 290-340g / m 2 ;
[0016] The negative electrode is composed of a negative electrode active material, a negative electrode conductive agent and a negative electrode binder; the negative electrode active material includes one or more of natural graphite, artificial graphite, hard carbon, lithium titanate, silicon carbon, and silicon oxygen; the negative electrode conductive agent includes one or more of single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, carbon fiber, conductive graphite, and conductive carbon black; the negative electrode binder includes one or more of sodium carboxymethyl cellulose, styrene-butadiene rubber, acrylate, modified acrylate, and polyvinylidene fluoride; the weight ratio of the negative electrode active material, the negative electrode conductive agent, and the negative electrode binder is 90-96:2-4:2-6; the surface density of the negative electrode is 130-190g / m 2 ;
[0017] The base material of the diaphragm is one of polyethylene and polypropylene, and the thickness of the diaphragm is 6 μm-14 μm.
[0018] Furthermore, the surface of the base material of the diaphragm has a ceramic coating or a high molecular polymer coating.
[0019] The beneficial effects of the present invention are as follows: the method of the present invention makes full use of the positive effects of rubidium and cesium compounds, and by adding cesium compounds and / or rubidium compounds, effectively inhibits the side reaction of carbonate solvents co-embedded in the negative electrode, reduces the barrier of active ion desolvation, and prolongs the cycle life of the battery under low temperature conditions. In addition, the addition of high concentrations of rubidium / cesium compounds reduces the glass transition temperature of the electrolyte, improves the fluidity and viscosity of the electrolyte, increases the conductivity of the electrolyte, and the active ions have better migration performance, inhibits the formation of dendrites, thereby improving the low temperature rate performance of the battery. DETAILED DESCRIPTION
[0020] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0021] Example 1
[0022] In a glove box filled with argon, ethylene carbonate, propylene carbonate and ethyl methyl carbonate were uniformly mixed in a mass ratio of 1:1:8 to obtain an organic solvent, and then 13wt% of lithium bis(fluorosulfonyl)imide, 3wt% of vinylene carbonate and 0.5wt% of fluoroethylene carbonate based on the total mass of the electrolyte were slowly added to the organic solvent, and after stirring until completely dissolved, cesium bis(fluorosulfonyl)imide with a molar concentration of 0.5 mol / L was added to obtain a cesium-containing lithium ion battery electrolyte.
[0023] Preparation of lithium-ion batteries:
[0024] After lithium iron phosphate, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) are fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93.5:3.5:3, they are coated on a 12μm aluminum foil current collector, dried and rolled, and then die-cut into 80mm*100mm positive electrode sheets. After graphite, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) are fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93:2:5, they are coated on a copper foil current collector, dried and rolled, and then die-cut into 83mm*104mm negative electrode sheets. Using 14μm polyethylene (PE) as a separator, the positive electrode sheet, separator, and negative electrode sheet are placed in order, and the stacked sheets are assembled into a 10Ah lithium-ion soft-pack battery. After liquefaction and capacity, the electrochemical performance test is carried out on a new Wei cabinet.
[0025] Example 2
[0026] The difference between this embodiment and embodiment 1 is that the molar concentration of cesium bis(fluorosulfonyl)imide added is 0.3 mol / L.
[0027] Example 3
[0028] The difference between this embodiment and embodiment 1 is that the molar concentration of cesium bis(fluorosulfonyl)imide added is 0.8 mol / L.
[0029] Example 4
[0030] The difference between this embodiment and embodiment 1 is that cesium bis(fluorosulfonyl)imide is not added, but rubidium bis(fluorosulfonyl)imide is added, and the molar concentration of rubidium bis(fluorosulfonyl)imide in the electrolyte is 0.5 mol / L, and the prepared lithium ion battery electrolyte contains rubidium.
[0031] Example 5
[0032] The difference between this embodiment and embodiment 1 is that cesium bis(fluorosulfonyl)imide is not added, but rubidium trifluoromethanesulfonylimide is added, and the molar concentration of rubidium trifluoromethanesulfonylimide in the electrolyte is 0.5 mol / L, and the prepared lithium ion battery electrolyte contains rubidium.
[0033] Example 6
[0034] The difference between this embodiment and embodiment 1 is that in the preparation of the electrolyte, 12 wt% of lithium hexafluorophosphate, 1 wt% of lithium bis(fluorosulfonyl)imide, 3 wt% of vinylene carbonate, and 0.5 wt% of fluoroethylene carbonate based on the total mass of the electrolyte are added to the organic solvent, and cesium hexafluorophosphate is used instead of cesium bis(fluorosulfonyl)imide, and the molar concentration of cesium hexafluorophosphate in the electrolyte is 0.5 mol / L.
[0035] Example 7
[0036] The difference between this embodiment and embodiment 1 is that in the preparation of the electrolyte, instead of only adding cesium bis(fluorosulfonyl)imide, cesium bis(fluorosulfonyl)imide and rubidium bis(fluorosulfonyl)imide are added, and the molar concentrations of cesium bis(fluorosulfonyl)imide and rubidium bis(fluorosulfonyl)imide in the electrolyte are 0.5 mol / L, respectively.
[0037] Example 8
[0038] The difference between this embodiment and embodiment 1 is that in the preparation of the lithium-ion battery, the active material lithium iron phosphate is replaced by lithium manganese iron phosphate.
[0039] Example 9
[0040] Preparation of cesium sodium ion battery electrolyte:
[0041] In a glove box filled with argon, ethylene carbonate, propylene carbonate and ethyl methyl carbonate are uniformly mixed in a mass ratio of 1:1:8 to obtain an organic solvent, and then 13wt% of sodium bis(fluorosulfonyl)imide, 3wt% of vinylene carbonate and 0.5wt% of fluoroethylene carbonate based on the total mass of the electrolyte are slowly added to the organic solvent, and after stirring until completely dissolved, cesium bis(fluorosulfonyl)imide is added, and the molar concentration of cesium bis(fluorosulfonyl)imide in the electrolyte is 0.5mol / L, to obtain a cesium-containing sodium ion battery electrolyte.
[0042] Preparation of sodium ion batteries:
[0043] Sodium iron pyrophosphate, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) were fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93.5:3.5:3, and then coated on a 12μm aluminum foil current collector. After drying and rolling, they were die-cut into 80mm*100mm positive electrode sheets. Hard carbon, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) were fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93:2:5, and then coated on a copper foil current collector. After drying and rolling, they were die-cut into 83mm*104mm negative electrode sheets. With 14μm polyethylene (PE) as the separator, the positive electrode sheet, separator, and negative electrode sheet were placed in order, and the sheets were stacked to assemble into a 10Ah sodium ion soft pack battery. After liquefaction and filling, the electrochemical performance test was carried out on the new Wei cabinet.
[0044] Comparative Example 1
[0045] Preparation of lithium-ion battery electrolyte:
[0046] In a glove box filled with argon, ethylene carbonate, propylene carbonate and ethyl methyl carbonate were uniformly mixed in a mass ratio of 1:1:8 to obtain an organic solvent, and then 13 wt% of lithium bis(fluorosulfonyl)imide, 3 wt% of vinylene carbonate and 0.5 wt% of fluoroethylene carbonate based on the total mass of the electrolyte were slowly added to the organic solvent, and the mixture was stirred until completely dissolved to obtain a lithium ion battery electrolyte.
[0047] Preparation of lithium-ion batteries:
[0048] After lithium iron phosphate, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) are fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93.5:3.5:3, they are coated on a 12μm aluminum foil current collector, dried and rolled, and then die-cut into 80mm*100mm positive electrode sheets. After graphite, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) are fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93:2:5, they are coated on a copper foil current collector, dried and rolled, and then die-cut into 83mm*104mm negative electrode sheets. With 14μm polyethylene (PE) as the separator, the positive electrode sheet, separator, and negative electrode sheet are placed in order, and the stacked sheets are assembled into a 10Ah lithium-ion soft-pack battery. After liquefaction and capacity, the electrochemical performance test is carried out on the new Wei cabinet.
[0049] Comparative Example 2
[0050] The difference from Comparative Example 1 is the preparation of the lithium-ion battery, in that the active material lithium iron phosphate is replaced by lithium manganese iron phosphate.
[0051] Comparative Example 3
[0052] Preparation of sodium ion battery electrolyte:
[0053] In a glove box filled with argon, ethylene carbonate, propylene carbonate and ethyl methyl carbonate were uniformly mixed in a mass ratio of 1:1:8, and then 13 wt% of sodium bis(fluorosulfonyl)imide, 3 wt% of vinylene carbonate and 0.5 wt% of fluoroethylene carbonate based on the total mass of the electrolyte were slowly added to the mixed solution, and the mixture was stirred until completely dissolved to obtain a sodium ion battery electrolyte.
[0054] Preparation of sodium ion batteries:
[0055] Sodium iron pyrophosphate, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) were fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93.5:3.5:3, coated on a 12μm aluminum foil current collector, dried and rolled, and then die-cut into 80mm*100mm positive electrode sheets. Hard carbon, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) were fully mixed in N-methylpyrrolidone (NMP) at a mass ratio of 93:2:5, coated on a copper foil current collector, dried and rolled, and then die-cut into 83mm*104mm negative electrode sheets. Using 14μm polyethylene (PE) as a separator, the positive electrode sheet, separator, and negative electrode sheet were placed in order, and the stacked sheets were assembled into a 10Ah sodium ion soft pack battery. After liquefaction and filling, the electrochemical performance test was carried out on the new Wei cabinet.
[0056] The electrolyte and battery components of the above embodiments and comparative examples are shown in Table 1.
[0057] Table 1
[0058]
[0059]
[0060] The performance test results of the above embodiments and comparative examples are shown in Table 2.
[0061] Table 2
[0062]
[0063]
[0064] It can be seen from Examples 1-7 and Comparative Example 1 that the addition of rubidium / cesium compounds reduces the glass transition temperature of the electrolyte, improves the viscosity and conductivity at low temperatures, and increases the conductivity of the electrolyte, so that lithium iron phosphate has a higher discharge capacity at low temperatures. In addition, rubidium ions and cesium ions can effectively inhibit the side reaction of PC co-embedded in the graphite negative electrode, improve the compatibility of PC and graphite, and also reduce the barrier of lithium ion desolvation in EC solvents, so that the cycle performance of the battery under low temperature conditions is significantly improved. It can be seen from Examples 8, 9 and Comparative Examples 2 and 3 that electrolytes containing rubidium / cesium compounds generally improve the low temperature properties of polyanion positive electrode materials.
[0065] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A rubidium / cesium-containing low-temperature battery electrolyte, characterized in that: The invention comprises cesium compound and / or rubidium compound, film-forming additive, lithium salt or sodium salt, and organic solvent; the total molar concentration of cesium compound and / or rubidium compound is 0.3-1 mol / L; the content of film-forming additive is 0.5-5wt%; the content of lithium salt or sodium salt is 0-15wt%.
2. The rubidium / cesium low-temperature battery electrolyte according to claim 1, characterized in that: The cesium compound includes one or more of cesium hexafluorophosphate, cesium tetrafluoroborate, cesium bis(fluorosulfonyl)imide, and cesium trifluoromethanesulfonyl imide.
3. The rubidium / cesium low-temperature battery electrolyte according to claim 1, characterized in that: The rubidium compound includes one or more of rubidium hexafluorophosphate, rubidium tetrafluoroborate, rubidium bis(fluorosulfonyl)imide, and rubidium trifluoromethanesulfonyl imide.
4. The rubidium / cesium low-temperature battery electrolyte according to claim 1, characterized in that: The film-forming additive includes one or more of vinylene carbonate, fluoroethylene carbonate, tris(trimethylsilyl)phosphate, tris(trifluoroethyl)carbonate, tris(trimethylsilyl)borate, lithium difluorophosphate, and lithium difluorobisoxalophosphate.
5. The rubidium / cesium-containing low-temperature battery electrolyte according to claim 1, characterized in that: The lithium salt includes one or more of lithium tetrafluoroborate, lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluorosulfonyl)imide, lithium difluorooxalatoborate, and lithium dioxalatoborate.
6. The rubidium / cesium low-temperature battery electrolyte according to claim 1, characterized in that: The sodium salt includes one or more of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and sodium bis(fluorosulfonyl)imide.
7. The rubidium / cesium low-temperature battery electrolyte according to claim 1, characterized in that: The organic solvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, acetonitrile, propionitrile, and butyronitrile.
8. A battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a separator and the rubidium / cesium-containing low-temperature battery electrolyte as described in any one of claims 1 to 7.
9. The battery according to claim 8, characterized in that The positive electrode is composed of a positive electrode active material, a positive electrode conductive agent and a positive electrode binder; the positive electrode active material includes one or more of lithium iron phosphate, lithium iron manganese phosphate, sodium iron phosphate, sodium iron pyrophosphate, and sodium iron pyrophosphate; the positive electrode conductive agent includes one or more of single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, carbon fiber, conductive graphite, and conductive carbon black; the positive electrode binder includes polyvinylidene fluoride; the weight ratio of the positive electrode active material, the positive electrode conductive agent and the positive electrode binder is 90-94:3-5:3-5; the surface density of the positive electrode is 290-340g / m 2 ; The negative electrode is composed of a negative electrode active material, a negative electrode conductive agent and a negative electrode binder; the negative electrode active material includes one or more of natural graphite, artificial graphite, hard carbon, lithium titanate, silicon carbon, and silicon oxygen; the negative electrode conductive agent includes one or more of single-walled carbon nanotubes, multi-walled carbon nanotubes, graphene, carbon fiber, conductive graphite, and conductive carbon black; the negative electrode binder includes one or more of sodium carboxymethyl cellulose, styrene-butadiene rubber, acrylate, modified acrylate, and polyvinylidene fluoride; the weight ratio of the negative electrode active material, the negative electrode conductive agent, and the negative electrode binder is 90-96:2-4:2-6; the surface density of the negative electrode is 130-190g / m 2 ; The base material of the diaphragm is one of polyethylene and polypropylene, and the thickness of the diaphragm is 6 μm-14 μm.
10. The battery according to claim 9, characterized in that The surface of the base material of the diaphragm has a ceramic coating or a high molecular polymer coating.
Citation Information
Patent Citations
New use of rubidium cesium compound, high-voltage electrolyte additive, high-voltage electrolyte and lithium ion battery
CN106450452A
Sodium-ion battery electrolyte additive containing rubidium and / or caesium cations, and applications thereof
CN107275672A
Cesium-containing high-voltage lithium ion battery electrolyte composite additive, electrolyte and battery thereof
CN112086684A
Electrolyte for lithium / carbon fluoride battery and application
CN116264286A
Lithium bis (fluorosulfonyl) imide salt containing cesium ion or rubidium ion
CN117120367A