Formation method of battery and battery

Through the multi-stage generation method, the current and voltage intervals are adjusted according to the capacity proportion of lithium manganese iron phosphate materials, and the problem of poor membrane performance during the mixing of lithium manganese iron phosphate and ternary materials in the prior art is solved, and the film performance is achieved. Improved battery performance and reduced risk of manganese dissolution.

CN118970238APending Publication Date: 2024-11-15HEFEI GUOXUAN HIGH TECH POWER ENERGY

Patent Information

Application Number
CN202411038260.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing chemical composition method cannot be applied to batteries including lithium manganese iron phosphate blended with ternary materials, resulting in poor performance of the formed CEI/SEI film, increasing the irreversible capacity loss and the risk of manganese dissolution.

Method used

The multi-stage production method is adopted to adjust the current and voltage intervals according to the capacity proportion of lithium manganese iron phosphate material, and charge through a combination of small current and large current to form a stable and dense film, reducing manganese dissolution and gas production, and optimizing the production process.

Benefits of technology

It improves the cycle life and storage performance of the battery, reduces the initial DC internal resistance, avoids lithium evolution during the battery transformation stage, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970238A_ABST
    Figure CN118970238A_ABST
Patent Text Reader

Abstract

The invention discloses a battery formation method and a battery, and belongs to the technical field of battery formation. The formation method comprises the following steps: S1, first formation: carrying out constant-current charging to a first voltage interval by using a first formation current; s2, performing second formation: performing constant-current charging to a second voltage interval by using a second formation current; s3, performing third formation: performing constant-current charging to a third voltage interval by using third formation current; s4, performing fourth formation: performing constant-current and constant-voltage charging to a fourth voltage interval by using a fourth formation current; wherein the first formation current is smaller than the second formation current and the fourth formation current; the third formation current is smaller than the second formation current and the fourth formation current; a positive active material of the battery positive electrode comprises a lithium manganese iron phosphate material and a ternary material. The main purpose of the invention is to be suitable for formation of a battery with a positive electrode formed by mixing lithium manganese iron phosphate and a ternary material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery formation, and more specifically, to a battery formation method and a battery. Background Art

[0002] Lithium iron manganese phosphate cathode material is expected to become the next generation of large-scale power battery cathode material due to its advantages of low cost, high voltage platform, and high safety. However, due to the relatively low ion conductivity and electronic conductivity of lithium iron manganese phosphate, the use of a single lithium iron manganese phosphate as the cathode will result in poor rate performance of the battery cell, making it difficult to promote it on a large scale in the market. Since the voltage platform of lithium iron manganese phosphate is relatively close to that of ternary materials, the two materials can be mixed, which can not only improve the kinetic performance, but also take into account the advantages of lithium iron manganese phosphate's own low cost and high safety. At the same time, the energy density of the battery cell can be improved by mixing ternary materials, so it has a broad prospect for commercial application.

[0003] The formation process of lithium-ion batteries is the process in which the CEI / SEI film is first formed at the electrode interface, which is crucial to the subsequent charge and discharge process of the battery. A thin and dense CEI / SEI film can reduce the irreversible capacity loss of lithium-ion batteries, reduce the risk of lithium precipitation, and reduce the impedance of the battery. The existing formation method is to formulate a segmented formation method based on the formation gas production curve and dQ / dV curve of the ternary positive electrode, using a small current at the initial stage of low-voltage film formation, and then gradually increasing the current to shorten the formation time; at the same time, a high vacuum is applied to exhaust in the early gas production stage of formation, and normal pressure is restored after the gas production is completed, so that a stable and dense SEI film is formed during the formation process, and the gas inside the battery is completely exhausted. For example, a negative pressure formation method and battery disclosed in China CN111554991B.

[0004] The electrodes in the battery are composed of two positive electrode materials, lithium iron manganese phosphate and ternary. The film formation and gas production processes of the two positive electrode materials are inconsistent during the formation process, resulting in poor performance of the formed CEI / SEI film; and lithium iron manganese phosphate has manganese dissolution, Mn 3+ The reduction and decomposition of the catalytic electrolyte produces serious gas, which leads to an increase in irreversible capacity loss during charging and discharging. Therefore, the existing formation method is not applicable to batteries including lithium manganese iron phosphate and ternary mixed electrodes. Summary of the invention

[0005] 1. Technical problem to be solved by the invention

[0006] Aiming at the problem that the prior art ternary positive electrode formation method cannot be applied to batteries whose positive electrode is a mixture of lithium manganese iron phosphate and ternary materials, a battery formation method and a battery are provided.

[0007] 2. Technical solution

[0008] In order to achieve the above object, the technical solution provided by the present invention is:

[0009] A battery formation method of the present invention comprises the following steps:

[0010] S1. First formation: using the first formation current constant current charging to the first voltage range V1 ~ V2;

[0011] S2. Second formation: using the second formation current constant current charging to the second voltage range V2 ~ V3;

[0012] S3. The third formation: charging with a third formation current constant current to a third voltage range V3 to V4;

[0013] S4. Fourth formation: using the fourth formation current constant current constant voltage charging to the fourth voltage range V4 ~ V5;

[0014] Wherein, the first formation current is smaller than the second formation current and the fourth formation current;

[0015] The third formation current is smaller than the second formation current and the fourth formation current;

[0016] Said V1<V2<V3<V4<V5;

[0017] The positive electrode of the battery includes a positive electrode active material, and the positive electrode active material includes a lithium manganese iron phosphate material and a ternary material.

[0018] It should be noted that the V1, V2, V3, V4, and V5 are obtained according to the curve of the capacity ratio of the lithium manganese iron phosphate material in the positive electrode of the battery with the change of voltage, wherein, according to the change curve, the voltage interval in which the capacity ratio of the lithium manganese iron phosphate material is greater than X is V1-V2, V3-V4, and the voltage interval in which the capacity ratio of the lithium manganese iron phosphate material is less than X is V2-V3, V4-V5; the formation current is adjusted according to the different capacities of the lithium manganese iron phosphate material. When the capacity ratio of the lithium manganese iron phosphate material is greater than X, the lithium manganese iron phosphate material has a greater amount of lithium de-lithium. The use of a small current for charging can increase the stability and density of the film on the positive electrode surface, reduce the dissolution of manganese in the positive electrode material, and also reduce gas production, avoiding excessive gas production rate and lithium precipitation of the negative electrode caused by the failure to remove the gas in time. When the capacity ratio of the lithium manganese iron phosphate material is less than X, a large current is used for charging, which can shorten the overall formation time and improve production efficiency; specifically, the value range of X is 45%-55%, and the preferred value of X is 50%.

[0019] Furthermore, the first formation current is less than or equal to the third formation current.

[0020] It should be noted that the first formation current should be less than or equal to the third formation current, because the LMFP capacity ratio in the first stage (close to 100% in the initial stage) is greater than that in the third stage. The higher the LMFP ratio, the smaller the current, which is conducive to forming a stable and dense film on the positive electrode surface, reducing manganese dissolution and reducing gas production.

[0021] Further, the first formation current is 0.01C to 0.05C;

[0022] The second formation current is 0.05C to 0.1C;

[0023] The third formation current is 0.01C to 0.05C;

[0024] The fourth formation current is 0.1C to 0.3C.

[0025] By controlling the first formation current, the second formation current, the third formation current and the fourth formation current within the above range, a battery whose positive electrode includes lithium iron manganese phosphate material and a ternary material can be formed, and the stability and density of the film formed on the surface of the positive electrode can be increased during the formation, the manganese dissolution of the positive electrode can be reduced, and the formation time can be shortened to improve the efficiency of the formation.

[0026] Furthermore, in the positive electrode active material, the mass ratio of lithium manganese iron phosphate material to ternary material is 1:9 to 9:1.

[0027] By controlling the mass ratio of lithium manganese iron phosphate material to ternary material within the above range, a dense and stable film is formed on the surface of the positive electrode after formation, which reduces the increase of manganese dissolution in the positive electrode and avoids excessive gas production and the resulting lithium plating at the negative electrode.

[0028] Further, the V1 is 0.08-0.2V;

[0029] The V2 is 3.0-3.6V;

[0030] The V3 is 3.7-4.0V;

[0031] The V4 is 4.0-4.2V;

[0032] The V5 is 4.2-4.5V.

[0033] It should be noted that when the mass ratio of lithium manganese iron phosphate material and ternary material is 1:9 to 9:1, the above curve is obtained according to the LMFP capacity ratio curve. Controlling V1, V2, V3, V4, and V5 within the above range can make the film on the positive electrode surface denser and more stable, and achieve better formation effect, reduce manganese dissolution and gas production, and avoid lithium precipitation at the negative electrode.

[0034] Furthermore, in step S4, the cut-off current of constant current and constant voltage charging is 0.01-0.1C.

[0035] Controlling the cut-off current of constant current and constant voltage charging within the above range can prevent the battery from being overcharged, avoid the generation of a large amount of gas and lithium deposition at the negative electrode; it also makes the charge distribution in the battery more uniform, which is conducive to reducing polarization.

[0036] Furthermore, in step S1, the temperature of the first formation is 25 to 35°C, and the negative pressure vacuum is -70 to -100 KPa.

[0037] Furthermore, in step S2, the temperature of the second formation is 35 to 45°C, and the negative pressure vacuum is -50 to -85 KPa.

[0038] Furthermore, in step S3, the temperature of the third formation is 25 to 35° C., and the negative pressure vacuum is -70 to -100 KPa.

[0039] Furthermore, in step S4, the temperature of the fourth formation is 35-45° C., and the negative pressure vacuum is 0--70 KPa.

[0040] It should be noted that the study found that when the capacity of lithium manganese iron phosphate material accounts for a high proportion, if the formation temperature is too high, it will also aggravate the side reactions on the surface of the lithium manganese iron phosphate positive electrode, increase manganese dissolution, and intensify the formation gas production. Using a higher vacuum degree is conducive to the discharge of gas; when the capacity of lithium manganese iron phosphate material accounts for a low proportion, by increasing the temperature, the battery formation speed can be accelerated and the formation time can be shortened, and at the same time, the side reactions of the positive electrode will not increase, causing manganese dissolution.

[0041] Furthermore, before performing steps S1, S2, S3, and S4, the steps are all put on hold.

[0042] The shelf time is 0 to 60 minutes, the temperature is 25 to 45° C., and the negative pressure vacuum degree is 0 to -5 KPa.

[0043] The process is put on hold before steps S1, S2, S3 and S4 to facilitate the switching of the temperature and vacuum degree of the equipment, so that the battery can be formed under the optimal conditions, which is conducive to forming a film with high density and stability on the surface of the positive electrode.

[0044] Furthermore, the lithium iron manganese phosphate material is LiMn Z Fe 1-Z PO4, where Z = 0.5, 0.6, 0.7 or 0.8;

[0045] The ternary material is LiNi x Co y Mn (1-x-y)O2, wherein 0<x<1, 0<y≤0.5, 0.5<x+y<1.

[0046] Furthermore, the positive electrode further includes a first conductive agent and a first binder.

[0047] The mass ratio of the positive electrode active material, the first conductive agent and the first binder is (90-98):(1-5):(1-5).

[0048] Furthermore, the first conductive agent is one, two or more of conductive carbon black, carbon nanotubes, graphene, conductive graphite, acetylene black, Ketjen black, and vapor phase carbon fiber.

[0049] Furthermore, the first binder is one or both of PVDF (polyvinylidene fluoride) and PTFE (polytetrafluoroethylene).

[0050] Furthermore, the battery includes a negative electrode, and the negative electrode includes a negative electrode active material, a second conductive agent, and a second binder.

[0051] Furthermore, the mass ratio (or molar ratio or other proportional relationship) of the negative electrode active material, the second conductive agent, and the second binder is (90-97):(1-5):(1-5).

[0052] Furthermore, the negative electrode active material is one, two or more of artificial graphite, natural graphite and mesophase carbon microspheres.

[0053] Furthermore, the second conductive agent is one, two or more of conductive carbon black, carbon nanotubes and graphene.

[0054] Furthermore, the second binder is one, two or more of SBR (styrene-butadiene rubber), CMC (carboxymethyl cellulose), and PAA (polyacrylic acid).

[0055] The present invention also provides a battery, characterized in that the battery is obtained by forming the battery using the above-mentioned battery formation method.

[0056] After the battery is formed by the formation method, a film with excellent performance is formed at the positive electrode. Compared with a battery formed by a traditional formation method, the cycle life of the formed battery is improved, the initial direct current internal resistance (DCR) of the battery is reduced, lithium precipitation is avoided in the battery formation stage, and the battery storage performance is improved.

[0057] 3. Beneficial effects

[0058] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0059] (1) The battery formation method provided by the present invention is applicable to a battery whose positive electrode includes a lithium iron manganese phosphate material and a ternary material. The formation method includes the steps of first formation, second formation, third formation and fourth formation. Different voltage intervals are obtained according to the curve of the capacity ratio of the lithium iron manganese phosphate material in the positive electrode changing with the voltage. The battery is charged with constant current or constant current and constant voltage at different steps by different currents for formation. This method can better adapt to batteries whose positive electrode is a mixture of lithium iron manganese phosphate material and ternary material.

[0060] When the capacity ratio of lithium manganese iron phosphate material is greater than X, the lithium iron phosphate material removes more lithium. Using a small current for charging can reduce the dissolution of manganese in the positive electrode material, and at the same time reduce gas production, thereby avoiding lithium precipitation at the negative electrode caused by excessive gas production rate and failure to remove gas in time. When the capacity ratio of lithium manganese iron phosphate material is less than X, using a large current for charging can shorten the overall formation time and improve production efficiency, wherein the value range of X is 45% to 55%.

[0061] (2) The battery provided by the present invention is obtained by the formation method. After the battery is formed by the formation method, a membrane with excellent performance is formed. Compared with the battery formed by the traditional formation method, the cycle life and battery storage performance of the formed battery are improved, the initial direct current internal resistance (DCR) of the battery is reduced, and lithium precipitation in the battery formation stage is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is a curve showing the change in capacity ratio of lithium iron manganese phosphate material in the positive electrode sheet of the battery in Example 1 of the present application as a function of voltage. DETAILED DESCRIPTION

[0063] The present disclosure may be more easily understood by reference to the following description in conjunction with examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or illustrated herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise indicated.

[0064] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.

[0065] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".

[0066] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.

[0067] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.

[0068] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.

[0069] In general, the use of the term "about" indicates an approximate value that can vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values ​​can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to a value in a range includes each value within that range.

[0070] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.

[0071] In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be purchased commercially.

[0072] The present invention is further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The essential characteristics and remarkable effects of the present invention can be reflected from the following examples, and the described embodiments are part of the embodiments of the present invention, rather than all the embodiments, and therefore, they do not limit the present invention in any way, and those skilled in the art make some non-essential improvements and adjustments based on the content of the present invention, which all belong to the protection scope of the present invention.

[0073] The test method of the cycle performance in the present invention is: at room temperature, charge and discharge at a rate of 1C, and perform a cycle test until the cell capacity decays to 80% of the initial capacity and the number of cycles of the cell;

[0074] The test method for initial DCR is: 50% SOC, 2C, 10S;

[0075] The test method for whether lithium is deposited on the initial fully charged interface is: disassemble and confirm the negative electrode interface at 100% SOC.

[0076] Example 1

[0077] 1) Preparation of positive electrode

[0078] The positive electrode active material, the first conductive agent, PVDF, and NMP are mixed in a mass ratio of 96:2.2:1.8:54 to obtain a positive electrode slurry, wherein the positive electrode active material is LiMn 0.6 Fe 0.4 PO4 and ternary material LiNi 0.5 Co 0.2 Mn 0.3 O2, of which LiMn6Fe4PO4 accounts for 70wt% of the positive electrode active material, and the rest is the ternary material LiNi 0.5 Co 0.2 Mn 0.3 O2, the first conductive agent is conductive carbon black; the above slurry is transferred to a current collector of a certain thickness and dried in an oven to obtain a positive electrode sheet, wherein the current collector is an Al foil with a thickness of 12 μm.

[0079] The curve of the capacity ratio of lithium manganese iron phosphate material in the positive electrode sheet as a function of voltage is shown in the figure below: Figure 1 shown.

[0080] 2) Preparation of negative electrode

[0081] The negative electrode active material, the second conductive agent, SBR, CMC and water are mixed evenly in a mass ratio of 96:1:1.8:1.2:90 to obtain a negative electrode slurry, wherein the negative electrode active material is artificial graphite, accounting for 96wt% of the mass of the negative electrode sheet, and the second conductive agent is carbon nanotubes; then the mixture is transferred to a current collector of a certain thickness to obtain a negative electrode sheet, wherein the current collector is a Cu foil with a thickness of 6μm.

[0082] 3) Battery assembly

[0083] The positive electrode sheet, separator, and negative electrode sheet are stacked together in order, with the negative electrode active material layer extending 3 mm beyond the positive electrode active material layer and the separator extending 4 mm beyond the negative electrode active material layer. The battery is assembled into a square aluminum shell battery with dimensions of 28 mm thick × 148 mm long × 115 mm high.

[0084] 4) Battery baking and liquid filling

[0085] The packaged batteries were baked in an oven at 95°C until the water content in the batteries was <200ppm. After cooling, the batteries were injected with 1M LiPF carbonate electrolyte at a ratio of 3.0g / Ah for 48h.

[0086] The battery with a capacity of 50 Ah after the above-mentioned assembly and injection was formed using the parameters of the formation process in Table 1. After formation, the capacity was divided and the cycle, storage and other performances were tested.

[0087] Among them, the specific process of formation is:

[0088] Step 1: Place the battery after liquid injection at 25°C and negative pressure vacuum degree 0KPa for 30 minutes, and the voltage during the placement is 0.1V;

[0089] Step 2: First formation: 35°C, negative pressure vacuum -85KPa, charge to 3.2V at a constant current of 0.03C;

[0090] Step 3: Place at 25℃ and negative pressure vacuum degree 0KPa for 30 minutes;

[0091] Step 4: Second formation: at 45°C and negative pressure vacuum -55KPa, charge to 3.7V at a constant current of 0.08C;

[0092] Step 5: Place at 25℃ and negative pressure vacuum degree 0KPa for 30 minutes;

[0093] Step 6: Third formation: 35°C, negative pressure vacuum -85KPa, charge to 4.0V with a constant current of 0.03C;

[0094] Step 7: Place at 25℃ and negative pressure vacuum degree 0KPa for 30 minutes;

[0095] Step 8: Fourth formation: At 45°C and negative pressure vacuum of -45KPa, charge to 4.2V with a constant current of 0.3C, then charge to 0.05C with a constant voltage, and the formation is completed.

[0096] Table 1 Example 1 Formation process

[0097] Step No. Control Type Magnification (C) Voltage (V) Cutoff ratio (C) Negative pressure vacuum Temperature(℃) Time (min) 1 Shelf / 0.1 / 0 25 30 2 Constant current charging 0.03 3.2 / -85KPa 35 / 3 Shelf / / / 0 25 30 4 Constant current charging 0.08 3.7 / -55KPa 45 / 5 Shelf / / / 0 25 30 6 Constant current charging 0.03 4.0 / -85KPa 35 / 7 Shelf / / / 0 25 30 8 Constant current and constant voltage charging 0.3 4.2 0.05 -45KPa 45 /

[0098] Example 2

[0099] The assembled and injected battery is obtained basically in the same manner as in Example 1, except that the formation is performed using the parameters of the formation process shown in Table 2, and after formation, the capacity is divided and the cycle, storage and other performances are tested.

[0100] Table 2 Example 2 Formation Process

[0101] Step No. Control Type Magnification (C) Voltage (V) Cutoff ratio (C) Negative pressure vacuum Temperature(℃) Time (min) 1 Shelf / 0.1 / 0 25 30 2 Constant current charging 0.01 3.2 / -85KPa 35 / 3 Shelf / / / 0 25 30 4 Constant current charging 0.08 3.7 / -55KPa 45 / 5 Shelf / / / 0 25 30 6 Constant current charging 0.02 4.0 / -85KPa 35 / 7 Shelf / / / 0 25 30 8 Constant current and constant voltage charging 0.2 4.2 0.05 -45KPa 45 /

[0102] Example 3

[0103] The assembled and injected battery is obtained in the same manner as in Example 1, except that the formation is performed using the parameters of the formation process in Table 3, and after formation, the capacity is divided and the cycle, storage and other performances are tested.

[0104] Table 3 Example 3 Formation Process

[0105]

[0106]

[0107] Example 4

[0108] The assembled and injected battery is obtained in the same manner as in Example 1, except that the formation is performed using the parameters of the formation process in Table 4, and after formation, the capacity is divided and the cycle, storage and other performances are tested.

[0109] Table 4 Example 4 Formation Process

[0110] Step No. Control Type Magnification (C) Voltage (V) Cutoff ratio (C) Negative pressure vacuum Temperature(℃) Time (min) 1 Shelf / 0.1 / 0 25 30 2 Constant current charging 0.03 3.2 / -85KPa 30 / 3 Shelf / / / 0 25 30 4 Constant current charging 0.08 3.7 / -55KPa 40 / 5 Shelf / / / 0 25 30 6 Constant current charging 0.03 4.0 / -85KPa 35 / 7 Shelf / / / 0 25 30 8 Constant current and constant voltage charging 0.3 4.2 0.05 -45KPa 40 /

[0111] Comparative Example 1

[0112] The assembled and injected battery is obtained in the same manner as in Example 1, except that the formation is performed using the parameters of the formation process in Table 5, and after formation, the capacity is divided and the cycle, storage and other performances are tested.

[0113] Table 5 Comparative Example 1 Formation Process

[0114] Step No. Control Type Magnification (C) Voltage (V) Cutoff ratio (C) Negative pressure vacuum Temperature(℃) Time (min) 1 Shelf / 0.1 / 0 25 30 2 Constant current charging 0.01 3.2 / -85KPa 35 / 3 Shelf / / / 0 25 30 4 Constant current charging 0.08 3.7 / -55KPa 45 / 5 Shelf / / / 0 25 30 6 Constant current charging 0.1 4.0 / -85KPa 35 / 7 Shelf / / / 0 25 30 8 Constant current and constant voltage charging 0.2 4.2 0.05 -45KPa 45 /

[0115] The performance test results of the above embodiments and comparative examples are specifically shown in Table 6.

[0116] Table 6 Electrochemical performance test results of the battery after formation

[0117]

[0118] According to the data in Table 6, compared with Comparative Example 1, the cycle performance of the battery cells in Examples 1-4 is improved by more than 10%, the initial DCR is reduced, and the initial full charge interface is improved. No lithium plating is found in Examples 1-4, and the capacity retention rate and recovery rate stored at 45°C for 7 days are increased by more than 1%.

Claims

1. A battery formation method, characterized in that: The following steps are involved: S1. First formation: using the first formation current constant current charging to the first voltage range V1 ~ V2; S2. Second formation: using the second formation current constant current charging to the second voltage range V2 ~ V3; S3. The third formation: charging with a third formation current constant current to a third voltage range V3 to V4; S4. Fourth formation: using the fourth formation current constant current constant voltage charging to the fourth voltage range V4 ~ V5; Wherein, the first formation current is smaller than the second formation current and the fourth formation current; The third formation current is smaller than the second formation current and the fourth formation current; And / or, V1<V2<V3<V4<V5; And / or, the positive electrode of the battery includes a positive electrode active material, and the positive electrode active material includes lithium manganese iron phosphate material and a ternary material.

2. The battery formation method according to claim 1, characterized in that: The first formation current is less than or equal to the third formation current.

3. The battery formation method according to claim 1 or 2, characterized in that: The first formation current is 0.01C to 0.05C; The second formation current is 0.05C to 0.1C; The third formation current is 0.01C to 0.05C; The fourth formation current is 0.1C to 0.3C.

4. The battery formation method according to claim 3, characterized in that: In the positive electrode active material, the mass ratio of lithium manganese iron phosphate material to ternary material is 1:9 to 9:

1.

5. The battery formation method according to claim 4, characterized in that: The V1 is 0.08-0.2V; The V2 is 3.0-3.6V; The V3 is 3.7-4.0V; The V4 is 4.0-4.2V; The V5 is 4.2-4.5V.

6. The battery formation method according to claim 2, characterized in that: In step S2, the temperature of the second formation is 35 to 45°C, and the negative pressure vacuum is -50 to -85 KPa; and / or, In step S4, the temperature of the fourth formation is 35-45° C., and the negative pressure vacuum is 0--70 KPa.

7. The battery formation method according to claim 6, characterized in that: In step S1, the temperature of the first formation is 25 to 35°C, and the negative pressure vacuum is -70 to -100 KPa; and / or, In step S3, the temperature of the third formation is 25 to 35°C, and the negative pressure vacuum is -70 to -100 KPa.

8. The battery formation method according to claim 7, characterized in that: In step S4, the cut-off current of the constant current and constant voltage charging is 0.01-0.1C.

9. The battery formation method according to any one of claims 6 to 8, characterized in that: Before performing steps S1, S2, S3, and S4, a pause is included. The shelf time is 0 to 60 minutes, the temperature is 25 to 45° C., and the negative pressure vacuum degree is 0 to -5 KPa.

10. A battery, characterized in that: The battery is obtained by forming the battery using the battery forming method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • A negative pressure formation method and a battery

    CN111554991B

  • Formation method for lithium ion battery and lithium ion battery

    CN103187590A

  • Formation method and application of battery

    CN113851744A

  • Cathode active material, secondary battery and preparation method

    CN116504961A

  • Double-layer positive plate, preparation method thereof and lithium ion battery

    CN117219756A

Cited By

  • Formation method of sodium ion battery

    CN119650913A

  • A formation method of a sodium ion battery

    CN119650913B

  • Formation process and application of lithium manganese iron phosphate battery

    CN119725819A