High-heat-resistance lithium battery diaphragm and preparation method thereof

By using ceramic powder and four-point zinc oxide whiskers in the lithium battery separator, a high heat resistance slurry is formed, which solves the problem of insufficient heat resistance of the lithium battery separator at high temperatures and improves the heat resistance of the separator and ionic conductivity enhance the safety performance and endurance of lithium batteries.

CN118970371AInactive Publication Date: 2024-11-15HEBEI GELLEC NEW ENERGY MATERIAL SCI&TECHNOLOY CO LTD

Patent Information

Application Number
CN202411004224.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium battery separators lack heat resistance at high temperatures, resulting in high short-circuit rate, low heat resistance, high internal resistance, small ion conductivity, and poor separator wetting, affecting the safety performance and battery life of lithium-ion batteries.

Method used

Using a high heat-resistant slurry combining ceramic powder and four-point zinc oxide whiskers, the ceramic powder is filled with four-point zinc oxide whiskers to form a dense and stable diaphragm structure, which improves the heat resistance of the diaphragm and Ion conductivity and reduces membrane internal resistance and coating surface tension through a unique needle-like structure.

Benefits of technology

It significantly improves the heat resistance, ionic conductivity and wetting properties of the diaphragm, ensures that it is not easy to deform under high temperatures, enhances the mechanical properties and dimensional uniformity of the diaphragm, reduces internal resistance, and improves the safety performance and battery life of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970371A_ABST
    Figure CN118970371A_ABST
Patent Text Reader

Abstract

The invention discloses a high-heat-resistance lithium battery diaphragm and a preparation method thereof.The high-heat-resistance lithium battery diaphragm comprises a base membrane and a coating coated on the base membrane, the coating is formed by coating high-heat-resistance slurry, and the preparation method of the high-heat-resistance slurry comprises the steps that tetrapod-like zinc oxide whiskers, ceramic powder, water, an adhesive and a dispersing agent are mixed to be uniform, and a mixture is obtained; the high-heat-resistance slurry is obtained. The tetrapod-like zinc oxide whiskers and the ceramic powder are used for modification, so that the heat resistance, the ionic conductivity and the wettability of the diaphragm are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery separators, and in particular relates to a high-heat-resistant lithium battery separator and a preparation method thereof. Background Art

[0002] As environmental problems become increasingly severe, more and more new energy projects have attracted social attention, among which electric vehicles are particularly popular. As the power source of electric vehicles, the safety and endurance of lithium-ion batteries are the focus of scientific research. As one of the key inner components of lithium-ion batteries, the performance of the diaphragm determines the interface structure and internal resistance of the battery, which directly affects the capacity, cycle and safety performance of lithium-ion batteries. In lithium-ion batteries, after the diaphragm absorbs electrolyte, it can prevent short circuits and allow the conduction of lithium ions; when overcharged or the temperature rises, the diaphragm blocks the conduction of current through closed pores to prevent explosion. The advantages of diaphragm performance determine the key characteristics of lithium-ion batteries, such as capacity, cycle performance, and charging current density. Thermal shrinkage, ionic conductivity and wettability are important indicators for characterizing diaphragms, and are also important performance related to the safety performance of lithium-ion batteries.

[0003] Based on the above, the high temperature resistance of lithium-ion batteries has become the focus of more attention. Conventional lithium battery separators are PP separators or PE films + coatings. Conventional lithium battery separators have average high heat resistance, high short circuit rate, low heat resistance, high internal resistance, low ion conductivity, and poor separator wettability. Summary of the invention

[0004] In view of the deficiencies of the prior art, an object of the present invention is to provide a high heat-resistant slurry.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned high heat-resistant slurry.

[0006] Another object of the present invention is to provide a high heat-resistant lithium battery separator.

[0007] Another object of the present invention is to provide a method for preparing the above-mentioned high heat-resistant lithium battery separator.

[0008] The purpose of the present invention is achieved through the following technical solutions.

[0009] A diaphragm comprises ceramic powder and four-needle zinc oxide whiskers, wherein the four-needle zinc oxide whiskers are filled in the pores between the ceramic powders.

[0010] In the above technical solution, the ceramic powder is alumina powder.

[0011] In the above technical solution, the center (core) diameter of the four-needle zinc oxide whisker is 0.7-1.4 μm, the root diameter of the needle is 0.5-5 μm, and the length of the needle is 3-10 μm.

[0012] In the above technical solution, the ceramic powder has a D50 of less than 0.9 microns and a D90 of less than 1.5 microns.

[0013] A high heat-resistant slurry comprises: ceramic powder, tetrapod-shaped zinc oxide whisker and water, wherein the ratio of the ceramic powder, tetrapod-shaped zinc oxide whisker and water is (3-7): (2-3): (81.5-89.9) by mass.

[0014] The above technical solution also includes: an adhesive and a dispersant. In terms of mass fractions, the ratio of the ceramic powder, the adhesive and the dispersant is (3-7): (5-8): (0.1-0.5).

[0015] In the above technical solution, the adhesive is an acrylate solution, and the concentration of polyacrylate in the acrylate solution is 25-50wt%.

[0016] In the above technical solution, the dispersant is ammonium polyacrylate.

[0017] The preparation method of the above-mentioned high heat-resistant slurry comprises: mixing four-needle zinc oxide whiskers, ceramic powder, water, adhesive and dispersant until uniform to obtain a high heat-resistant slurry, wherein, by weight, the ratio of the four-needle zinc oxide whiskers, ceramic powder, water, adhesive and dispersant is (2-3): (3-7): (81.5-89.9): (5-8): (0.1-0.5).

[0018] In the above technical solution, the preparation method comprises the following steps:

[0019] Step 1, mixing a dispersant, water, tetrapod-shaped zinc oxide whiskers and ceramic powder until uniform to obtain a first solution;

[0020] In step 1, a dispersant, water, four-needle zinc oxide whiskers and ceramic powder are mixed, first stirred at a rotation speed of 1500-3100 r / min and a revolution speed of 20-50 r / min for 10-20 min, and then ultrasonicated at a frequency of 10-50 KHz for 10-20 min until uniform.

[0021] Step 2: Mix the first solution and the adhesive, and stir and ultrasonicate them simultaneously under a vacuum environment to obtain a high heat-resistant slurry.

[0022] In step 2, the time of simultaneous stirring and ultrasonication under vacuum environment is 10 to 20 minutes.

[0023] In step 2, the stirring rotation speed is 1000-3800 r / min, and the stirring revolution speed is 20-40 r / min.

[0024] In step 2, the ultrasonic wave frequency of the ultrasound is 5 to 8 kHz.

[0025] In step 2, the vacuum degree of the vacuum environment is 0.06-0.08 KPA.

[0026] A high heat-resistant lithium battery separator comprises a base film and a coating coated on the base film, wherein the coating is formed by coating with a high heat-resistant slurry.

[0027] In the above technical solution, the thickness of the coating is 1.5 to 2.5 μm.

[0028] The method for preparing the above-mentioned high heat-resistant lithium battery separator comprises: coating the high heat-resistant slurry on a base film, and drying to obtain the high heat-resistant lithium battery separator.

[0029] In the above technical solution, the drying temperature is 50-70° C., and the drying time is 1-3 minutes.

[0030] In the above technical solution, the coating speed is 30 to 50 m / min.

[0031] Ceramic powder and four-needle zinc oxide whiskers are used together in a diaphragm to improve the heat resistance, ion conductivity, liquid absorption rate and / or liquid retention rate of the diaphragm.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The invention uses four-needle zinc oxide whiskers and ceramic powders for modification. A diaphragm prepared by using a high heat-resistant slurry mixed with the four-needle zinc oxide whiskers and aluminum oxide powder is more compact and stable, has good structural stability, increases the heat resistance of the diaphragm, ensures the isotropy of the diaphragm in terms of mechanical properties, dimensional uniformity, thermal shrinkage, thermal deformation and other use properties, and makes the diaphragm not easy to deform at high temperatures; on the surface of the base film, the special needle-like structure enables it to be dispersed between the ceramic powders and efficiently overlap to form a network structure, forming a good conductive path, and its unique four-needle structure and good semiconductor properties can not only give the diaphragm efficient antistatic performance, but also reduce the internal resistance of the diaphragm, thereby increasing the ionic conductivity of the diaphragm; the four-needle zinc oxide whiskers have a large specific surface area, are easy to disperse, and present a three-dimensional four-needle stereoscopic structure at a microscopic level. They are distributed between the aluminum oxide powders to increase the porosity of the diaphragm coating, more easily reduce the surface tension of the coating and the solid-liquid interface energy, and increase the wettability of the diaphragm. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the SEM of the diaphragm prepared in Example 4;

[0035] Figure 2 This is the SEM of the diaphragm prepared in Comparative Example 3;

[0036] Figure 3 This is the SEM of the separator prepared in Comparative Example 4. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0038] In the following embodiments, the four-needle zinc oxide whisker has a center (core) diameter of 0.7 to 1.4 μm, a root diameter of the needle-shaped body of 0.5 to 5 μm, and a length of the needle-shaped body of 3 to 10 μm;

[0039] Alumina: purity 99.9%;

[0040] Acrylate solution: an aqueous binder containing polyacrylate, wherein the concentration of polyacrylate in the acrylate solution is 45wt%;

[0041] Ammonium polyacrylate: polyvinyl alcohol.

[0042] The instruments and models involved in the tests in the following embodiments are:

[0043] Double planetary mixer, XFZH-30L.

[0044] In the following examples, the base film is a PE film, and the thickness of the base film is 9 μm.

[0045] In the following examples, water is pure water.

[0046] Ionic conductivity: tested at 26°C and dew point -30°C.

[0047] Contact angle: The electrolyte used in the contact angle test is Mojes KPF6 potassium ion electrolyte.

[0048] Four-needle zinc oxide whisker: It has a white loose powder appearance and a three-dimensional four-needle structure. That is, the whisker has a core, and four needle-like crystals extend radially from the core. Each needle-like body is a single crystal microfiber, and the angle between any two needle-like bodies is 109°. Its unique three-dimensional four-needle structure can easily achieve uniform distribution in the matrix material, thereby isotropically improving the physical properties of the material and giving the material a variety of unique functional properties. Four-needle zinc oxide whiskers can withstand high temperatures of 1720°C. Due to its special three-dimensional four-needle structure, it has a completely isotropic enhancement and modification effect, and stabilizes the coating structure. Four-needle zinc oxide whiskers have excellent properties that ordinary zinc oxide cannot match. Such as wear resistance, enhancement, vibration reduction, anti-slip, noise reduction, wave absorption, anti-aging, antistatic, antibacterial and other properties.

[0049] Example 1

[0050] A method for preparing a high heat-resistant slurry comprises the following steps:

[0051] Step 1, mixing a dispersant, water, four-needle zinc oxide whiskers and ceramic powder in a double planetary mixer, first stirring at a rotation speed of A1 and a revolution speed of A2 for 15 minutes, and then ultrasonicating at a frequency of B1 for 15 minutes until uniform, to obtain a first solution, wherein the ceramic powder is aluminum oxide powder, the dispersant is polyacrylate ammonium salt, and the particle size of the ceramic powder is C;

[0052] Step 2, mixing the first solution and the adhesive, stirring and ultrasonicating for 15 minutes (high-speed dispersion) in a double planetary mixer under a vacuum environment with an ultrasonic oscillation function (vacuum degree is 0.07KPA) to obtain a high heat-resistant slurry, wherein the ratio of four-needle zinc oxide whiskers, ceramic powder, water, adhesive and dispersant is X by mass, the adhesive is an acrylate solution, and in step 2, the stirring rotation speed is A3, the stirring revolution speed is A4, and the ultrasonic frequency of the ultrasound is B2.

[0053] The values ​​of X, A1, A2, A3, A4, B1, B2 and C are shown in Table 1.

[0054] Table 1

[0055]

[0056]

[0057] Comparative Example 1

[0058] A method for preparing an alumina slurry comprises: mixing alumina, water and a dispersant in a double planetary mixer, blending at a rotation speed of 3100 r / min and a revolution speed of 20 r / min for 15 min, ultrasonicating at a frequency of 50 kHz for 15 min, adding an adhesive and simultaneously ultrasonically oscillating (ultrasonic frequency of 5 kHz) for 15 min under stirring conditions (rotation speed of 1000 r / min, revolution speed of 40 r / min) to obtain an alumina slurry, wherein, by mass, the ratio of alumina, water, dispersant and adhesive is 5:89.8:0.2:5, the adhesive is an acrylate solution, the dispersant is polyacrylate ammonium salt, and the D50 of the alumina (particles) is 0.599 microns and the D90 is 1.273 microns.

[0059] Comparative Example 2

[0060] A method for preparing an aluminum oxide slurry is basically the same as the method for preparing a high heat-resistant slurry in Example 1, except that the "four-needle zinc oxide whisker" is replaced by "zinc oxide (granular)". The particle size of zinc oxide is: D50: 0.501 micrometer; D90: 1.226 micrometer.

[0061] The particle sizes of the alumina slurry prepared in Comparative Example 2 are: D50: 0.602 μm; D90: 1.279 μm.

[0062] Examples 4 to 6 and Comparative Examples 3 to 4

[0063] A method for preparing a diaphragm, comprising: placing a base film on a coating machine equipped with a slurry, coating the base film on one side at a coating speed of Dm / min, pulling the base film into a drying device through a traction roller after coating, drying at E℃ for F min, obtaining a coating on the base film, and obtaining a diaphragm, wherein the slurry is one of the high heat-resistant slurry prepared in Examples 1 to 3 and the aluminum oxide slurry prepared in Comparative Examples 1 to 2, and the diaphragm prepared in Examples 4 to 6 is a high heat-resistant lithium battery diaphragm, that is, the diaphragms obtained in sequence from the high heat-resistant slurries prepared in Examples 1 to 3 are high heat-resistant lithium battery diaphragms of Examples 4 to 6, and the diaphragms obtained in sequence from the aluminum oxide slurries prepared in Comparative Examples 1 to 2 are Comparative Examples 3 to 4. The values ​​of D, E and F are shown in Table 2.

[0064] Table 2

[0065] Examples and Comparative Examples D(m / min) E(℃) F(min) Example 4 30 50 3 Example 5 40 60 2 Example 6 50 70 1 Comparative Example 3 30 50 3 Comparative Example 4 30 50 3

[0066] The parameters for preparing the diaphragm obtained in Example 4 are as follows:

[0067]

[0068] The parameters for preparing the membrane obtained in Example 5 are as follows:

[0069]

[0070]

[0071] The parameters for preparing the diaphragm obtained in Example 6 are as follows:

[0072]

[0073] The diaphragm prepared in Comparative Example 3 was tested, and the test results are shown in the following table:

[0074]

[0075]

[0076] The diaphragm prepared in Comparative Example 4 was tested, and the test results are shown in the following table:

[0077]

[0078] Figure 1 This is the SEM of the diaphragm prepared in Example 4; Figure 2 This is the SEM of the diaphragm prepared in Comparative Example 3; Figure 3 This is the SEM of the diaphragm prepared in Comparative Example 4. Figure 1 It can be seen that the four-needle zinc oxide whiskers filled in the gaps of alumina powder can support the coating structure, which is better than the single alumina powder ( Figure 2 ) is more solid, has better density and stability, is less likely to deform at high temperatures, and has better heat resistance (smaller thermal shrinkage at 150°C / 1h); the needle-like structure of the four-needle zinc oxide whisker enables it to be dispersed between the ceramic powders, and can be efficiently overlapped to form a network structure, which not only forms a good conductive path, but also achieves the effect of reducing the internal resistance of the diaphragm, thereby increasing the ionic conductivity of the diaphragm (the ionic conductivity of the diaphragm prepared in Examples 4 to 6 of the present invention is greater than that of the comparative example), and also reduces the solid-liquid interface energy on the coating surface, making it easier to reduce the surface tension of the coating, reduce the wetting angle of the diaphragm, and increase the wettability of the diaphragm (the contact angle data of the diaphragm prepared in Examples 4 to 6 are lower than those in the comparative example, which shows that the diaphragm prepared in Examples 4 to 6 is more easily wetted by the electrolyte).

[0079] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A diaphragm, include: Ceramic powder and tetrapod-shaped zinc oxide whiskers, wherein the tetrapod-shaped zinc oxide whiskers are filled in pores between the ceramic powders.

2. The diaphragm according to claim 1, It is characterized in that The central diameter of the four-needle zinc oxide whisker is 0.7-1.4 μm, the root diameter of the needle is 0.5-5 μm, and the length of the needle is 3-10 μm.

3. The diaphragm according to claim 1, It is characterized in that The ceramic powder is alumina powder, and the ceramic powder has D50 < 0.9 micron and D90 < 1.5 micron.

4. A high heat-resistant slurry, It is characterized in that include: The ceramic powder, the tetrapod-shaped zinc oxide whisker and the water are present in a ratio of (3-7): (2-3): (81.5-89.9) by weight.

5. The high heat-resistant slurry according to claim 4, It is characterized in that Also includes: The adhesive and the dispersant are in a ratio of (3-7): (5-8): (0.1-0.5) by weight.

6. The high heat-resistant slurry according to claim 5, It is characterized in that The adhesive is an acrylate solution, in which the concentration of polyacrylate is 25-50wt%; and the dispersant is polyacrylate ammonium salt.

7. The method for preparing the high heat-resistant slurry according to claim 6, include: The tetrapod-shaped zinc oxide whiskers, ceramic powder, water, adhesive and dispersant are mixed until uniform to obtain a high heat-resistant slurry, wherein the ratio of the tetrapod-shaped zinc oxide whiskers, ceramic powder, water, adhesive and dispersant is (2-3): (3-7): (81.5-89.9): (5-8): (0.1-0.5) by mass.

8. The preparation method according to claim 7, It is characterized in that The preparation method comprises the following steps: Step 1, mixing a dispersant, water, tetrapod-shaped zinc oxide whiskers and ceramic powder until uniform to obtain a first solution; Step 2: Mix the first solution and the adhesive, and stir and ultrasonicate them simultaneously under a vacuum environment to obtain a high heat-resistant slurry.

9. A high heat-resistant lithium battery separator, include: A base film and a coating coated on the base film, wherein the coating is formed by coating the high heat-resistant slurry according to claim 4.

10. The ceramic powder and the tetrapod-shaped zinc oxide whisker are used together in a diaphragm to improve the heat resistance, ion conductivity, liquid absorption rate and / or liquid retention rate of the diaphragm.

Citation Information

Patent Citations

  • High-heat-resistance and high-wettability lithium battery diaphragm and preparation method thereof

    CN116979218A

  • Coating diaphragm structure and lithium ion battery and battery pack comprising same

    CN216903238U

Cited By

  • Double-ceramic modified polymer-based heat-conducting composite diaphragm as well as preparation method and application thereof

    CN121261057A