Method for infiltrating battery cell

By using the inclination angle and positive and negative pressure cycle technology of the incoming disk during the battery cell infiltration, the problem of long infiltration time and poor effect of the battery cell is solved, and the efficient and sufficient infiltration and rapid discharge of the electrolyte is achieved, and the battery cell is improved infiltration efficiency and stability.

CN118970398AActive Publication Date: 2024-11-15ZHEJIANG JINKO ENERGY STORAGE CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411448888.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
2044-10-16

AI Technical Summary

Technical Problem

The existing battery cell infiltration methods have the problem of long infiltration time and poor results, especially due to the low liquid injection method and liquid absorption efficiency, the electrolyte cannot be fully absorbed, and gas is easily introduced, affecting the wetting effect.

Method used

By loading the battery cell on the incoming tray, combining the liquid injection hole with the liquid storage cup with the first and second inclination angles, excessive injection of the electrolyte is injected, and circulated through positive and negative pressure. The adjusted receiving hole controls the liquid level to ensure that the electrolyte is fully wet and discharged, and improves the wetting efficiency.

Benefits of technology

This method significantly shortens the battery cell infiltration time, improves the absorption speed and wetting efficiency of the electrolyte, reduces the risk of gas introduction and liquid injection costs, and ensures sufficient soaking of the battery cell and liquid distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970398A_ABST
    Figure CN118970398A_ABST
Patent Text Reader

Abstract

The invention provides a method for infiltrating a battery cell. The method comprises the following steps: S1, loading a battery cell on an incoming tray; s2, the liquid injection hole and the liquid storage cup are combined by inclining the feeding disc at the first inclination angle; step S3, returning the charging tray, and excessively injecting the electrolyte in the charging tray into the battery cell through a hole formed in the bottom of the liquid storage cup; the liquid injection cup is moved to the position above the liquid storage cup, and then electrolyte is supplemented into the liquid storage cup through the liquid injection cup; s4, inflating and exhausting air into the battery cell to complete positive and negative pressure circulation; s5, discharging redundant electrolyte in the battery cell into a liquid storage cup by inclining the feeding disc at a second inclination angle; and S6, the liquid injection hole is separated from the liquid storage cup, the feeding disc is reset, and infiltration is completed. By adopting the method provided by the invention, the cell infiltration time can be shortened, and the infiltration effect can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of energy storage technology, and in particular to a method for soaking a battery cell. Background Art

[0002] As a common energy storage device, batteries are widely used in various energy storage scenarios. Liquid injection is a key step in preparing batteries. At present, due to the fixed shell and the fixed core, in order to avoid slow liquid injection, one injection and two injections are usually used to avoid the electrolyte from not being absorbed in time and flowing out from the injection hole. One injection and two injections usually do not fill each battery cell after injection to avoid leakage when detached. In the prior art, one injection of 85% + two injections of 15% or one injection of 90% + two injections of 10% is usually used. After one injection, the battery liquid filling level accounts for about 1 / 5 of the battery cell. Taking LFP280 as an example, the injection height is 4cm and the shell height is 20cm. However, the battery cell is not in a liquid-rich state during liquid injection. When standing, absorption can only be carried out from the bottom. The liquid level will drop through the core suction, and then the positive and negative pressure cycles will introduce gas, affecting local infiltration and forming large brown spots. As the capacity of the battery cell becomes larger and larger, the compaction becomes larger and larger, and the infiltration becomes slower and slower, and the conventional infiltration method needs to be innovated.

[0003] The wetting of the electrode does not mean the wetting of the core. The wetting of the core depends on many factors such as tightness and temperature. The current reliable means are ICP element characterization and ultrasonic testing, but the ultrasonic probe equipment is expensive and cannot be clearly located, and the electrolyte distribution state cannot be observed with the naked eye. The existing technology usually adopts disassembly to measure the residual liquid to determine the amount of liquid absorbed or directly dry the core to absorb liquid to confirm the amount of liquid absorbed, but the disassembly process is cumbersome, the error of liquid absorption is large, and it is impossible to confirm whether the outer ring is soaked OK; the liquid absorption of the core is microscopic and difficult to characterize. When disassembling, it is impossible to confirm whether the bubbles introduced are bubbles themselves or introduced by disassembly; the liquid injection of the electrode, diaphragm or laminated core under conventional liquid injection can be accurately characterized, but the wetting characterization of the liquid-rich state of the wound core is less, and there is a lack of corresponding detection means. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for battery cell infiltration to solve the problems of long battery cell infiltration time and poor infiltration effect in the prior art battery cell infiltration method.

[0005] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for soaking a battery cell is provided, the method comprising: step S1, loading the battery cell on a material tray, the bottom of the battery cell is contacted and arranged on the material tray, and the bottom of the battery cell is parallel to the horizontal direction; step S2, a liquid injection hole is arranged on the top of the battery cell, and the liquid injection hole is combined with a liquid storage cup placed at the first inclination angle by tilting the material tray at a first inclination angle; step S3, returning the material tray to the right position, and injecting an excess amount of electrolyte in the liquid storage cup into the battery cell through the hole arranged at the bottom of the liquid storage cup ; Move the injection cup to above the storage cup, and then add electrolyte to the storage cup through the injection cup; the storage cup has a receiving hole for receiving electrolyte on the side away from the injection hole, and an adjustable block is provided at the receiving hole to adjust the opening and closing state of the receiving hole; Step S4, inflate and evacuate the battery cell to complete the positive and negative pressure cycle; Step S5, discharge the excess electrolyte in the battery cell into the storage cup by tilting the incoming material tray at a second tilt angle; Step S6, separate the injection hole from the storage cup, return the incoming material tray to the normal position, and complete the infiltration.

[0006] Furthermore, in the above step S3, the amount of electrolyte injected into the battery cell exceeds the theoretical filling amount by 20% to 50%.

[0007] Further, in the above step S4, the positive pressure of the positive and negative pressure cycle is 0.2~0.8MPa; and / or, the negative pressure of the positive and negative pressure cycle is -90~-30kPa; and / or, the number of positive and negative pressure cycles is 3~8 times.

[0008] Further, in the above step S2, the incoming material tray is tilted at a first inclination angle so that the angle between the bottom of the battery cell and the horizontal direction is 60°~90°; and / or, in step S5, the incoming material tray is tilted at a second inclination angle so that the angle between the bottom of the battery cell and the horizontal direction is 60°~100°.

[0009] Furthermore, the material tray is tilted at a first tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 90°.

[0010] Furthermore, the material tray is tilted at a second tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is determined according to the required discharge amount of the electrolyte.

[0011] Furthermore, in the above step S3, the injection rate of the electrolyte into the battery cell is 500mL / min~1L / min; and / or, in step S5, the discharge rate of excess electrolyte is 50mL / min~200mL / min.

[0012] Furthermore, the above step S6 also includes subjecting the cells in the returned incoming material tray to a static treatment for 12 to 16 hours to complete the infiltration.

[0013] Furthermore, a simulated battery cell is selected for wettability monitoring. Before injecting excess electrolyte into the simulated battery cell, step S3 also includes adding a fluorescent agent to the electrolyte. After the infiltration is completed, the simulated core roll in the simulated battery cell is taken out and unfolded, and the simulated core roll is irradiated with a fluorescent lamp. The wetting condition of the simulated core roll is observed through the fluorescent area. The larger the fluorescent area, the more sufficient the infiltration.

[0014] Furthermore, the concentration of the fluorescent agent in the above electrolyte is 1.3-2.6 mg / mL; and / or the type of the fluorescent agent is selected from any one or more of FITC, Cy2, Cy3, and Alexa Fluor 647.

[0015] By applying the technical solution of the present invention, in step S2, the liquid injection hole is combined with the liquid storage cup by tilting the incoming material tray at a first tilt angle, which helps to subsequently inject the electrolyte in the liquid storage cup into the battery cell through the liquid injection hole. In step S3, the electrolyte in the liquid storage cup is excessively injected into the battery cell through the hole provided at the bottom of the liquid storage cup, so that the electrolyte fills the entire battery cell and the entire coil is soaked, which helps to increase the speed at which the battery cell absorbs the electrolyte and helps to reduce the risk of gas storage. Since the electrolyte forms a seal on the liquid level surface, it helps to reduce the risk of external gas introduction under atmospheric airflow. An adjustable block is provided at the receiving hole, which helps to control the time for receiving the electrolyte and facilitates the regulation of the liquid level of the electrolyte. In step S4, the battery cell after liquid injection is subjected to positive and negative pressure circulation, which helps to further increase the speed at which the battery cell absorbs the electrolyte. In step S5, the excess electrolyte in the battery cell is discharged into the liquid storage cup by tilting the incoming material tray at a second tilt angle. On the one hand, the electrolyte is allowed to vertically infiltrate the battery cell and infiltrate in the direction of the thickness of the electrode sheet, which helps to further improve the efficiency of infiltration; on the other hand, it helps to accelerate the discharge of excess electrolyte, thereby helping to shorten the duration of infiltration. The liquid storage cup receives the discharged electrolyte and can use the electrolyte in the next round of injection, thereby helping to reduce the cost of injection. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0017] Figure 1 An optical photograph of a simulated winding core under fluorescent light in Example 1 of the present application is shown. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0019] As analyzed in the background technology of the present application, the method of battery cell infiltration in the prior art has the problems of long battery cell infiltration time and poor infiltration effect. In order to solve the above problems, the present application provides a method of battery cell infiltration.

[0020] In a typical embodiment of the present application, a method for soaking a battery cell is provided, the method comprising: step S1, loading the battery cell on a material tray, the bottom of the battery cell is contacted and arranged on the material tray, and the bottom of the battery cell is parallel to the horizontal direction; step S2, a liquid injection hole is arranged on the top of the battery cell, and the liquid injection hole is combined with a liquid storage cup placed at the first tilt angle by tilting the material tray at a first tilt angle; step S3, returning the material tray to the right position, and injecting an excess amount of electrolyte therein into the battery cell through the hole arranged at the bottom of the liquid storage cup; The injection cup is shifted to above the storage cup, and then the electrolyte is added to the storage cup through the injection cup; the storage cup has a receiving hole for receiving the electrolyte on the side away from the injection hole, and an adjustable block is provided at the receiving hole to adjust the opening and closing state of the receiving hole; step S4, inflate and evacuate the battery cell to complete the positive and negative pressure cycle; step S5, discharge the excess electrolyte in the battery cell into the storage cup by tilting the incoming material tray at a second tilt angle; step S6, separate the injection hole from the storage cup, return the incoming material tray to the normal position, and complete the infiltration.

[0021] In step S2, the liquid injection hole is combined with the liquid storage cup by tilting the incoming material tray at a first tilt angle, which helps to subsequently inject the electrolyte in the liquid storage cup into the battery cell through the liquid injection hole. In step S3, the electrolyte in the liquid storage cup is excessively injected into the battery cell through the hole set at the bottom of the liquid storage cup, so that the electrolyte fills the entire battery cell and the entire coil is soaked, which helps to increase the speed at which the battery cell absorbs the electrolyte and helps to reduce the risk of gas storage. Since the electrolyte forms a seal on the liquid level surface, it helps to reduce the risk of external gas introduction under atmospheric airflow. An adjustable block is provided at the receiving hole, which helps to control the time of receiving the electrolyte and facilitates the regulation of the liquid level of the electrolyte. In step S4, the battery cell after liquid injection is subjected to positive and negative pressure circulation, which helps to further increase the speed at which the battery cell absorbs the electrolyte. In step S5, the excess electrolyte in the battery cell is discharged into the liquid storage cup by tilting the incoming material tray at a second tilt angle. On the one hand, the electrolyte is allowed to vertically infiltrate the battery cell and infiltrate in the direction of the thickness of the electrode sheet, which helps to further improve the efficiency of infiltration; on the other hand, it helps to accelerate the discharge of excess electrolyte, thereby helping to shorten the duration of infiltration. The liquid storage cup receives the discharged electrolyte and can use the electrolyte in the next round of injection, thereby helping to reduce the cost of injection.

[0022] In one embodiment of the present application, in the above step S3, a manually openable cover is provided at the hole at the bottom of the liquid storage cup, and a sealing rubber ring is provided between the cover and the hole. When the liquid storage cup is tilted, the cover is closed so that the cover covers the hole to prevent the electrolyte from leaking from the hole at the bottom of the liquid storage cup; when injecting liquid, the cover is opened so that the electrolyte in the liquid storage cup is injected into the battery cell.

[0023] In one embodiment of the present application, in the above step S3, an adjustable block is provided at the receiving hole, and a sealing rubber ring is provided between the block and the receiving hole. When it is not necessary to receive electrolyte, the block is pushed so that the block covers the receiving hole; when it is necessary to receive electrolyte, the block is pushed so that the block is separated from the receiving hole.

[0024] In one embodiment of the present application, in the above step S3, the amount of electrolyte injected into the battery cell is 20% to 50% more than the theoretical filling amount, which helps to further increase the speed at which the core absorbs the electrolyte, improve the wetting effect and reduce the risk of gas storage.

[0025] The purpose of positive and negative pressure cycles is to accelerate the infiltration of the electrolyte into the battery cell. In order to better exert the above-mentioned effects, in an embodiment of the present application, in the above-mentioned step S4, the positive pressure of the positive and negative pressure cycles is 0.2~0.8MPa; and / or, the negative pressure of the positive and negative pressure cycles is -90~-30kPa; and / or, the number of positive and negative pressure cycles is 3~8 times.

[0026] Controlling the positive pressure of the positive and negative pressure cycles, the negative pressure of the positive and negative pressure cycles, and the number of positive and negative pressure cycles within the above ranges will help further increase the speed at which the core absorbs the electrolyte.

[0027] In one embodiment of the present application, in the above-mentioned step S2, the incoming material tray is tilted at a first inclination angle so that the angle between the bottom of the battery cell and the horizontal direction is 60°~100°; and / or, in step S5, the incoming material tray is tilted at a second inclination angle so that the angle between the bottom of the battery cell and the horizontal direction is 60°~90°.

[0028] By controlling the angle between the bottom of the battery cell and the horizontal direction within the above range when tilting at the first tilt angle, it is helpful to improve the efficiency and stability of the combination of the injection hole and the liquid storage cup, thereby ensuring production stability. By controlling the angle between the bottom of the battery cell and the horizontal direction within the above range when tilting at the second tilt angle, it is helpful to improve the degree of electrolyte infiltration into the battery cell and the efficiency of excess electrolyte discharge.

[0029] In order to further improve the efficiency of the combination of the liquid injection hole and the liquid storage cup, in one embodiment of the present application, the above-mentioned material tray is tilted at a first tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 90°.

[0030] In one embodiment of the present application, the tilting speed of the above-mentioned first tilting angle is 5° / min~10° / min.

[0031] By controlling the inclination speed of the first inclination angle within the above range, it is helpful to shorten the time for the liquid injection hole to be combined with the liquid storage cup while maintaining the overall stability of the battery cell.

[0032] In one embodiment of the present application, the above-mentioned material tray is tilted at a second tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is determined according to the required discharge amount of the electrolyte.

[0033] In order to better control the amount of electrolyte discharged, when the amount of electrolyte discharged is small, the second inclination angle is also small. Specifically, the amount of electrolyte discharged is A, and the incoming material tray is inclined at a second inclination angle so that the angle between the bottom of the battery cell and the horizontal direction is θ. When A<20% of the injection amount, 60°≤θ<70°; when 20% of the injection amount≤A<40% of the injection amount, 70°≤θ<80°; when 40% of the injection amount≤A, 80°≤θ≤90°.

[0034] In one embodiment of the present application, the tilting speed of the second tilting angle is 3° / min~5° / min.

[0035] Controlling the tilting speed of the second tilting angle within the above range helps to improve the efficiency of discharging excess electrolyte while ensuring the stability of the electrolyte in the battery cell, and at the same time, it also plays a better role in promoting the complete infiltration of the electrolyte.

[0036] In one embodiment of the present application, in the above-mentioned step S3, the injection rate of the electrolyte into the battery cell is 500mL / min~1L / min; and / or, in step S5, the discharge rate of excess electrolyte is 50mL / min~200mL / min.

[0037] If the injection speed of the electrolyte into the battery cell is too high, it is not conducive to the discharge of the gas in the battery cell. If the injection speed of the electrolyte into the battery cell is too low, it is not conducive to improving the injection efficiency of the electrolyte. Controlling the injection speed of the electrolyte into the battery cell within the above range will help improve the injection efficiency. If the discharge speed of the excess electrolyte is too slow, it is not conducive to shortening the discharge time. If the discharge speed of the excess electrolyte is too fast, it is not conducive to the full infiltration of the electrolyte into the battery cell. Controlling the discharge speed of the excess electrolyte within the above range will help shorten the discharge time and improve the infiltration efficiency of the battery cell.

[0038] In one embodiment of the present application, the above step S6 also includes subjecting the battery cells in the returned incoming material tray to a static treatment for 12 to 16 hours to complete the infiltration.

[0039] The static treatment helps the electrolyte to fully and evenly infiltrate the positive and negative materials and the separator of the battery cell, and helps the electrolyte to form a stable solid electrolyte interface film on the electrode surface, thereby helping to improve the cycle stability and service life of the battery cell. Controlling the static treatment time within the above range helps to improve the efficiency of the static treatment.

[0040] In one embodiment of the present application, the above-mentioned receiving hole is a circular receiving hole, and setting it as a circular receiving hole helps to improve the efficiency of electrolyte reception.

[0041] In one embodiment of the present application, the above-mentioned liquid injection cup is shifted to above the liquid storage cup by a robot; and / or, the replenishment speed of the electrolyte is 100mL / min~500mL / min.

[0042] The liquid injection cup is shifted by a robot so that the hole at the bottom of the liquid injection cup is combined with the hole at the top of the liquid storage cup to replenish the electrolyte into the liquid storage cup through the liquid injection cup, which helps to reduce labor costs and control the replenishment speed of the electrolyte within the above range, which helps to control the volume of the electrolyte in the liquid storage cup, thereby helping to control the amount of electrolyte in the liquid storage cup injected into the battery cell, thereby helping to improve the efficiency of liquid injection.

[0043] In one embodiment of the present application, a simulated battery cell can also be selected for wettability monitoring (the simulated battery cell can be normally arranged in the battery cell array). Before injecting excess electrolyte into the simulated battery cell, step S3 also includes adding a fluorescent agent to the electrolyte; after the infiltration is completed, the simulated core roll in the simulated battery cell is taken out and unfolded, and the simulated core roll is illuminated by a fluorescent lamp, and the wetting of the simulated core roll is observed through the fluorescent area. The larger the fluorescent area, the more sufficient the infiltration. The fluorescent area accounts for more than 95% of the simulated core roll, which is qualified.

[0044] In the production process of battery cells, it is helpful to observe the wetting condition of the battery cells by selecting a simulated battery cell for wettability monitoring. By adding a fluorescent agent to the electrolyte, the fluorescent agent can emit fluorescence under the irradiation of a fluorescent lamp, and the part of the core soaked in the electrolyte can emit fluorescence under the irradiation of a fluorescent lamp. The wetting condition of the electrolyte in the core can be confirmed through the part emitting fluorescence, thereby obtaining the wetting condition of the battery cell after the injection is completed. The wetting condition of the simulated core can guide the adjustment of the process parameters of the battery cell wetting to adjust the optimal process parameters.

[0045] In addition, the above-mentioned simulated battery cell can be used to adjust the process parameters before the battery cell production, and can also be set in the battery cell array in normal production to monitor the wetting condition of the battery cell in real time.

[0046] In order to improve the accuracy of wettability monitoring, in one embodiment of the present application, the concentration of the fluorescent agent in the above-mentioned electrolyte is 1.3~2.6 mg / mL; and / or the model of the fluorescent agent is selected from any one or more of FITC, Cy2, Cy3, and Alexa Fluor 647.

[0047] In order to make the simulated battery cell closer to the actual battery cell and reduce the cost of battery cell production, in one embodiment of the present application, the simulated core in the above-mentioned simulated battery cell has a winding structure formed by winding the core 1.5 turns in a stacked manner of diaphragm-positive electrode-diaphragm-negative electrode, and the shape of the winding structure is the same as the actual core, which is elliptical. The simulated core is placed in a transparent plastic shell to form a simulated battery cell.

[0048] Placing the simulated core in a transparent plastic shell helps to observe the wetting of the core in real time. The plastic shell has a lower cost than the actual aluminum shell, and it is easier to take out the simulated core that has been wetted.

[0049] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.

[0050] Example 1

[0051] The battery cells are loaded on the incoming material tray, and the bottom of the battery cells is in contact with the incoming material tray, and the bottom of the battery cells is parallel to the horizontal direction; a liquid injection hole is provided on the top of the battery cells, and the liquid injection hole is combined with the liquid storage cup by tilting the incoming material tray at a first tilt angle, the angle between the bottom of the battery cells and the horizontal direction is 90°, and the tilting speed of the first tilt angle is 5° / min; the incoming material tray is returned to the center, and the electrolyte therein is excessively injected into the battery cells through the hole set at the bottom of the liquid storage cup; the liquid injection cup is shifted to the top of the liquid storage cup by a manipulator, and then the electrolyte is replenished into the liquid storage cup through the liquid injection cup; a receiving hole for receiving the electrolyte is provided on the side of the liquid storage cup away from the liquid injection hole, and an adjustable block is provided at the receiving hole for adjusting the opening and closing state of the receiving hole; an electrolyte 20% in excess of the theoretical filling amount is injected into the battery cells through the liquid storage cup, and the injection speed of the electrolyte into the battery cells is 500mL / min, and replenish the electrolyte into the storage cup through the injection cup, the speed of replenishing the electrolyte is 500mL / min; the battery cell after injection is subjected to positive and negative pressure cycle, the positive pressure of the positive and negative pressure cycle is 0.4MPa, the negative pressure of the positive and negative pressure cycle is -60kPa, the number of positive and negative pressure cycles is 5 times, after the positive and negative pressure cycle is completed, the excess electrolyte in the battery cell is discharged into the storage cup by tilting the incoming material tray at a second tilt angle; the incoming material tray is tilted at a second tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 70°, the tilting speed of the second tilt angle is 3° / min, when discharging 20% ​​of the electrolyte injected into the battery cell, the discharge rate of the excess electrolyte is 50mL / min, the storage cup receives the discharged electrolyte, and after the excess electrolyte is discharged, the battery cell is left to stand for 14h to complete the infiltration. According to the above process, liquid injection, positive and negative pressure circulation, discharge of excess electrolyte and infiltration treatment are completed in sequence. The core is a simulated core with a winding structure formed by winding the core 1.5 turns in a stacked manner of diaphragm-positive electrode-diaphragm-negative electrode. The shell of the simulated battery cell is a transparent plastic shell. After the infiltration treatment is completed, the simulated core is unfolded and the infiltration of the simulated core is observed under fluorescent light. The length of the unfolded simulated core is 51 cm and the width is 18.7 cm. The observed infiltration conditions are as follows Figure 1 shown.

[0052] Example 2

[0053] The difference from Example 1 is that the electrolyte injection amount exceeds the theoretical filling amount by 50%.

[0054] Example 3

[0055] The difference from Example 1 is that the electrolyte injection amount exceeds the theoretical filling amount by 10%.

[0056] Example 4

[0057] The difference from Example 1 is that the positive pressure of the positive and negative pressure cycle is 0.8 MPa, the negative pressure of the positive and negative pressure cycle is -90 kPa, and the number of positive and negative pressure cycles is 8 times.

[0058] Example 5

[0059] The difference from Example 1 is that the positive pressure of the positive and negative pressure cycle is 0.2 MPa, the negative pressure of the positive and negative pressure cycle is -30 kPa, and the number of positive and negative pressure cycles is 3.

[0060] Example 6

[0061] The difference from Example 1 is that the positive pressure of the positive and negative pressure cycle is 0.6 MPa, the negative pressure of the positive and negative pressure cycle is -20 kPa, and the number of positive and negative pressure cycles is 2.

[0062] Example 7

[0063] The difference from Example 1 is that the static treatment time is 16 hours.

[0064] Example 8

[0065] The difference from Example 1 is that the static treatment time is 12 hours.

[0066] Example 9

[0067] The difference from Example 1 is that the static treatment time is 10 hours.

[0068] Example 10

[0069] The difference from Example 1 is that the material tray is tilted at a first tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 60°, and the tilted at a second tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 80°.

[0070] Embodiment 11

[0071] The difference from Example 1 is that the material tray is tilted at a first tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 50°, and the tilting at a second tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 50°.

[0072] Example 12

[0073] The difference from Example 1 is that the tilting speed at the first tilting angle is 10° / min, and the tilting speed at the second tilting angle is 5° / min.

[0074] Example 13

[0075] The difference from Example 1 is that the tilting speed at the first tilting angle is 15° / min, and the tilting speed at the second tilting angle is 4° / min.

[0076] Embodiment 14

[0077] The difference from Example 1 is that the injection rate of the electrolyte into the battery cell is 1 L / min, the discharge rate of the excess electrolyte is 200 mL / min, and the replenishment rate of the electrolyte is 100 mL / min.

[0078] Embodiment 15

[0079] The difference from Example 1 is that the injection rate of the electrolyte into the battery cell is 1.5 L / min, the discharge rate of the excess electrolyte is 300 mL / min, and the replenishment rate of the electrolyte is 50 mL / min.

[0080] Comparative Example 1

[0081] The difference from Example 1 is that the liquid is injected according to the theoretical injection amount of the battery.

[0082] The simulated core wetting conditions and the saturated liquid absorption of the battery cell in the above embodiments and comparative examples are shown in Table 1.

[0083] Table 1

[0084]

[0085] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0086] In step S2, the liquid injection hole is combined with the liquid storage cup by tilting the incoming material tray at a first tilt angle, which helps to subsequently inject the electrolyte in the liquid storage cup into the battery cell through the liquid injection hole. In step S3, the electrolyte in the liquid storage cup is excessively injected into the battery cell through the hole set at the bottom of the liquid storage cup, so that the electrolyte fills the entire battery cell and the entire coil is soaked, which helps to increase the speed at which the battery cell absorbs the electrolyte and helps to reduce the risk of gas storage. Since the electrolyte forms a seal on the liquid level surface, it helps to reduce the risk of external gas introduction under atmospheric airflow. An adjustable block is provided at the receiving hole, which helps to control the time of receiving the electrolyte and facilitates the regulation of the liquid level of the electrolyte. In step S4, the battery cell after liquid injection is subjected to positive and negative pressure circulation, which helps to further increase the speed at which the battery cell absorbs the electrolyte. In step S5, the excess electrolyte in the battery cell is discharged into the liquid storage cup by tilting the incoming material tray at a second tilt angle. On the one hand, the electrolyte is allowed to vertically infiltrate the battery cell and infiltrate in the direction of the thickness of the electrode sheet, which helps to further improve the efficiency of infiltration; on the other hand, it helps to accelerate the discharge of excess electrolyte, thereby helping to shorten the duration of infiltration. The liquid storage cup receives the discharged electrolyte and can use the electrolyte in the next round of injection, thereby helping to reduce the cost of injection.

[0087] The above are only embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for cell infiltration, characterized in that: The method comprises: Step S1, loading the battery cell on a material tray, with the bottom of the battery cell in contact with the material tray, and the bottom of the battery cell being parallel to the horizontal direction; Step S2, a liquid injection hole is provided on the top of the battery cell, and the liquid injection hole is combined with a liquid storage cup placed at the first inclination angle by tilting the incoming material tray at a first inclination angle; Step S3, returning the incoming material tray to the right position, and injecting an excess amount of electrolyte therein into the battery cell through the hole provided at the bottom of the liquid storage cup; shifting the injection cup to above the liquid storage cup, and then replenishing the electrolyte into the liquid storage cup through the injection cup; the liquid storage cup has a receiving hole for receiving the electrolyte on a side away from the injection hole, and an adjustable block is provided at the receiving hole for adjusting the opening and closing state of the receiving hole; Step S4, inflating and deflating the battery cell to complete a positive and negative pressure cycle; Step S5, discharging the excess electrolyte in the battery cell into the liquid storage cup by tilting the incoming material tray at a second tilt angle; Step S6, disengaging the liquid injection hole from the liquid storage cup, returning the incoming material tray to the normal position, and completing the infiltration.

2. The method according to claim 1, characterized in that In the step S3, the amount of the electrolyte injected into the battery cell exceeds the theoretical filling amount by 20% to 50%.

3. The method according to claim 1, characterized in that In step S4, the positive pressure of the positive and negative pressure cycle is 0.2~0.8MPa; and / or, the negative pressure of the positive and negative pressure cycle is -90~-30kPa; and / or, the number of positive and negative pressure cycles is 3~8 times.

4. The method according to claim 1, characterized in that: In the step S2, the material tray is tilted at a first tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 60°~100°; and / or, in the step S5, the material tray is tilted at a second tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 60°~90°.

5. The method according to claim 4, characterized in that The material tray is tilted at a first tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is 90°.

6. The method according to claim 4, characterized in that The material tray is tilted at a second tilt angle so that the angle between the bottom of the battery cell and the horizontal direction is determined according to the required discharge amount of the electrolyte.

7. The method according to any one of claims 1 to 6, characterized in that In the step S3, the injection rate of the electrolyte into the battery core is 500 mL / min~1 L / min; and / or, in the step S5, the discharge rate of excess electrolyte is 50 mL / min~200 mL / min.

8. The method according to any one of claims 1 to 6, characterized in that The step S6 also includes subjecting the cells in the returned material tray to a static treatment, wherein the static treatment time is 12 to 16 hours to complete the infiltration.

9. The method according to any one of claims 1 to 6, characterized in that A simulated battery cell is selected for wettability monitoring. Before injecting an excess amount of electrolyte into the simulated battery cell, the step S3 further includes adding a fluorescent agent to the electrolyte; After the infiltration is completed, the simulated core roll in the simulated battery cell is taken out and unfolded, and the simulated core roll is illuminated by a fluorescent lamp. The infiltration condition of the simulated core roll is observed through the fluorescent area. The larger the fluorescent area, the more complete the infiltration.

10. The method according to claim 9, characterized in that The concentration of the fluorescent agent in the electrolyte is 1.3-2.6 mg / mL; and / or the type of the fluorescent agent is selected from any one or more of FITC, Cy2, Cy3, and Alexa Fluor 647.

Citation Information

Patent Citations

  • Method for visually representing electrolyte seepage effect

    CN105932220A

  • Pole piece infiltration method of soft package lithium ion battery

    CN111416158A

  • Liquid injection device and liquid injection method of battery

    CN112736376A

  • Centrifugal liquid injection device and method

    CN114221097A

  • Battery liquid injection device

    CN217589370U