Composite fiber brush with micro-spring structure and preparation method thereof

By fabricating composite fiber brushes with micro-spring structures, the problems of low hardness and poor wear resistance of brush materials were solved, achieving high conductivity and wear resistance, thus meeting the requirements of high power transmission and long life.

CN118970568APending Publication Date: 2024-11-15XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411229202.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing brush materials have low hardness, poor wear resistance, and insufficient current-carrying friction properties, making it difficult to meet the requirements of high-power transmission and long life.

Method used

A method for preparing composite fiber brushes with micro-spring structures includes pretreatment of conductive fibers/films, twisting into a spring configuration, stretching to fix the deformation rate, depositing metal layers inside and on the surface, and annealing to prepare composite fiber brushes with high conductivity and wear resistance.

Benefits of technology

The manufacturing process is simple, safe, and inexpensive. The composite fiber brush has high conductivity, high current carrying capacity, friction reduction, and wear resistance, meeting the requirements for high power transmission and long life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970568A_ABST
    Figure CN118970568A_ABST
Patent Text Reader

Abstract

The invention discloses a composite fiber brush with a micro-spring structure and a preparation method thereof. The preparation method comprises the following steps: pretreating conductive fibers / films; then twisting operation is carried out, and spring-configuration prefabricated fibers are obtained; stretching the obtained spring-configuration prefabricated fiber to obtain a set deformation rate, and fixing the two ends of the spring-configuration prefabricated fiber to ensure that the deformation rate is unchanged; s3, the spring configuration prefabricated fiber obtained in the step S3 is used as a substrate, metal layers are deposited in internal pores and the surface of the spring configuration prefabricated fiber, and composite fiber of a micro-spring structure is obtained; and performing annealing treatment on the obtained composite fiber, eliminating internal stress generated in the preparation process, and preparing the composite fiber electric brush with the micro-spring structure. The preparation process is simple, safe and low in cost; and the composite fiber electric brush with the micro-spring structure has the advantages of high conductivity, high current-carrying density, friction reduction and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of sliding electric contact materials, and in particular relates to a composite fiber brush with a micro-spring structure and a preparation method thereof. Background Art

[0002] As a sliding electrical contact material, brushes are usually used to conduct current between fixed parts and rotating parts - commutators or conductive slip rings. They are widely used in electrical equipment, aerospace, rail transportation and other fields. Sliding electrical contact is the process of conducting current between friction pairs during relative sliding, also known as current-carrying friction. The service life, current transmission capacity, chemical stability and friction resistance of sliding electrical contact materials are all affected by their basic properties. Therefore, the ideal brush material should have good electrical and thermal conductivity, self-lubricating properties, wear resistance and arc resistance.

[0003] At present, the commonly used brush materials are mainly precious metal wire brushes, metal-based solid self-lubricating brushes and carbon-based brushes. The metals commonly used in precious metal wire brushes are precious metals with high conductivity such as gold, silver, and platinum. Precious metals are expensive and have poor arc erosion resistance under high power. Metal-based solid self-lubricating brushes are composite materials with copper, silver and other metals with good conductivity as the matrix, and solid lubricants such as MoS2 and WS2 added. As the brush wears, the lubricant adheres to the friction interface and easily forms an insulating layer, which affects the conductive properties of the friction pair. Carbon-based brushes are less used in high-power equipment due to their low hardness and poor wear resistance. With the development of equipment technology, the transmission power of commutators and conductive slip rings is getting larger and larger, and higher requirements are also placed on the performance of brush materials.

[0004] Therefore, how to improve the current-carrying friction performance of existing brush materials and develop a new generation of high-power and long-life brush materials is a key issue that needs to be solved urgently. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a composite fiber brush with a micro-spring structure and a preparation method thereof in view of the deficiencies in the above-mentioned prior art, so as to solve the technical problems of low hardness, poor wear resistance and insufficient friction performance of brush materials for high-power current carrying, and meet the dual requirements of high-power transmission and long life of brush materials.

[0006] The present invention adopts the following technical solutions:

[0007] A composite fiber brush with a micro-spring structure and a preparation method thereof, comprising the following steps:

[0008] S1. Pre-treating the conductive fiber / film;

[0009] S2, twisting the conductive fiber / film pretreated in step S1 to obtain a spring-shaped prefabricated fiber;

[0010] S3, after stretching the spring configuration prefabricated fiber obtained in step S2 to obtain a set deformation rate, fixing both ends thereof to ensure that the deformation rate remains unchanged;

[0011] S4, using the spring-shaped prefabricated fiber obtained in step S3 as a substrate, depositing metal layers on the internal pores and surface of the spring-shaped prefabricated fiber to obtain a composite fiber with a microspring structure;

[0012] S5, annealing the composite fiber obtained in step S4 to eliminate the internal stress generated in the preparation process, and prepare a composite fiber brush with a micro-spring structure.

[0013] Preferably, in step S1, the diameter of the conductive fiber is 5 to 200 μm, and the thickness of the film is 5 to 500 μm.

[0014] Preferably, in step S1, the pretreatment method includes one or more of chemical pretreatment and electrochemical pretreatment.

[0015] Preferably, the chemical pretreatment includes one or more of deoiling, degreasing, purification and acidification; and the electrochemical pretreatment includes one or more of anodic oxidation and current shock.

[0016] Preferably, in step S2, the number of the conductive fibers / films to be twisted is 1 to 50, and the twisting degree is 10 to 100 r / cm.

[0017] Preferably, in step S3, the deformation rate is set to be 1% to 400%.

[0018] Preferably, in step S4, the thickness of the deposited metal layer is 1-2000 μm, and the deposited metal includes one or more of gold, silver, copper, platinum, palladium, nickel and tin.

[0019] Preferably, the metal layer is deposited by one or more of electrochemical deposition, chemical plating and magnetron sputtering.

[0020] Preferably, in step S5, the atmosphere of the annealing treatment is one of vacuum, argon and nitrogen, the temperature of the annealing treatment is 200-1400° C., and the time is 20-600 min.

[0021] Another technical solution of the present invention is a composite fiber brush with a micro-spring structure, which is prepared according to the method.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects:

[0023] A composite fiber brush with a micro-spring structure and a preparation method thereof, wherein the raw conductive fiber / film is pretreated; a spring-shaped prefabricated fiber is prepared by rotating and twisting the fiber / film; the spring-shaped prefabricated fiber is stretched to obtain a certain deformation rate; a metal layer is deposited inside and on the surface of the spring-shaped prefabricated fiber with a certain deformation rate to obtain a micro-spring structure composite fiber; the composite fiber is annealed to prepare a micro-spring structure composite fiber brush. This method has a simple and safe preparation process and low cost; it gives full play to the advantages of composite materials, the internal fiber has high strength, high current density, and has a certain friction reduction effect, and the external metal layer has high hardness and wear resistance; and the composite fiber brush has a lower elastic modulus and good shock absorption performance due to its spring configuration, which is conducive to obtaining better resistance to current-carrying friction and wear, and meets the dual requirements of high power transmission and long life of the brush material.

[0024] Furthermore, the raw materials are carbon nanotube fibers, carbon fibers, carbon nanotube films and other conductive fibers or films because carbon nanotube fibers / films or carbon fibers have the advantages of high strength, good conductivity and high current density, and carbon materials can play a role in lubrication and friction reduction during friction and wear.

[0025] Furthermore, the raw material fiber has a diameter of 5 to 200 μm and the raw material film has a thickness of 5 to 500 μm, which is convenient for subsequent stranding, overlapping and twisting operations.

[0026] Furthermore, the main purpose of pre-treating the film / fiber is to remove impurities adsorbed on the fiber / film.

[0027] Chemical pretreatment is one or more of degreasing, degreasing, purification and acidification. The chemical pretreatment method is to immerse the raw fiber / film in a chemical pretreatment reagent, which can remove amorphous carbon on the surface of the fiber / film and introduce defects on its surface. The chemical pretreatment reagent is one or a mixture of acetone solution, sulfuric acid solution, nitric acid solution, hydrochloric acid solution, sulfuric acid-nitric acid mixed solution, sulfuric acid-hydrochloric acid mixed solution, nitric acid-hydrochloric acid mixed solution, potassium hydroxide solution, sodium hydroxide solution, potassium hydroxide-sodium hydroxide solution.

[0028] Electrochemical pretreatment is anodic oxidation or current shock treatment, in which anodic oxidation generates oxygen on the surface of the fiber / film, introduces defects in the surface layer and grafts oxygen-containing groups at the defects. Current shock treatment uses a large current density and a short treatment time. While grafting oxygen-containing groups, it can also use the overflow of a large amount of oxygen to increase the internal pores of the fiber / film, which is beneficial to the subsequent deposition of metals.

[0029] Furthermore, the number of twisted fibers / films is 1 to 50, and when multiple fibers are twisted, their diameters can be the same or different, and the same length facilitates the stranding operation; when multiple layers of carbon films are twisted, their thicknesses can be the same or different, and the same length and width facilitate the overlapping operation.

[0030] Furthermore, the twist is the original fiber / film per unit length, and the twist is the number of convolutions of the spring-configured prefabricated fiber, that is, the number of motor rotations, in units of r / cm.

[0031] Furthermore, the device for twisting the pretreated fiber / film is a twisting machine or a rotary motor, and the twisting twist is 10 to 100 r / cm. If the twist is too small, the complete spring configuration prefabricated fiber cannot be formed, and if the twist is too large, the spring structure is easily destroyed. The optimal twist range is related to the number and size of the original fiber / film. The twist is one of positive twist and reverse twist. The specific twisting operation is: after multiple fibers are stranded or multiple layers of carbon films are overlapped, one end is fixed and the other end is connected to the twisting machine or rotary motor, and the motor rotation direction and number of rotations are controlled to obtain spring configuration prefabricated fibers with different twists.

[0032] Furthermore, the gaps between the single-loop fibers of the twisted spring-shaped prefabricated fiber are small, and the metal layer is easily adhered when the metal layer is directly deposited, which affects the role of the spring configuration in current-carrying friction. After the spring-shaped prefabricated fiber is stretched to obtain a certain deformation rate, the gaps between the single-loop fibers become larger, and the spring structure can still be maintained after depositing a certain thickness of the metal layer. The fiber deformation rate is guaranteed to be 1% to 400%. If the deformation rate is too small, there will be insufficient space between the single-loop fibers, and if the deformation rate is too large, the fiber spring structure will be damaged.

[0033] Furthermore, in order to obtain a composite fiber brush with good current-carrying friction performance, the metal / alloy deposited on the surface of the spring-shaped prefabricated fiber is required to have advantages such as good electrical and thermal conductivity and wear resistance, and is one or more of gold, silver, copper, platinum, palladium, nickel and tin.

[0034] Furthermore, the metal deposition method includes one or more of electrochemical deposition, chemical plating and magnetron sputtering. Among them, electrochemical deposition is low in cost, chemical plating has a dense coating, and magnetron sputtering has a good interface bonding. In the electrochemical deposition and magnetron sputtering processes, by controlling the current size and deposition time, coatings of different thicknesses can be obtained.

[0035] Furthermore, the thickness of the metal layer is 1-2000 μm. If the metal layer is too thin, the wear resistance of the composite fiber is poor, and if the metal layer is too thick, the friction coefficient of the composite fiber is large.

[0036] Furthermore, annealing can eliminate the internal stress generated in the composite fiber during the preparation process. Annealing process parameters are: atmosphere is one of vacuum, argon and nitrogen, temperature is 200-1400°C, time is 20-600min.

[0037] In summary, the preparation process of the method of the present invention is simple, safe and low-cost; the advantages of composite materials are fully utilized, and the composite fiber brush with a microspring structure has the advantages of high conductivity, high current density, friction reduction and wear resistance.

[0038] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a flow chart of the preparation method of the present invention;

[0040] Figure 2 The process of preparing micro spring structure fiber by twisting carbon nanotube film;

[0041] Figure 3 The morphology of the micro-spring structure carbon nanotube / copper composite fiber brush, where (a) is the side view and (b) is the cross section. DETAILED DESCRIPTION

[0042] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] In the present invention, unless otherwise specified, all the embodiments and preferred implementation methods mentioned herein can be combined with each other to form a new technical solution.

[0044] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0045] In the present invention, unless otherwise specified, percentage (%) or part refers to the weight percentage or weight part relative to the composition.

[0046] In the present invention, unless otherwise specified, the components or preferred components involved can be combined with each other to form a new technical solution.

[0047] In the present invention, unless otherwise specified, the numerical range "a-b" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "6-22" means that all real numbers between "6-22" have been listed in this document, and "6-22" is just an abbreviation of these numerical combinations.

[0048] The “range” disclosed in the present invention is in the form of a lower limit and an upper limit, which can be one or more lower limits, and one or more upper limits, respectively.

[0049] In the present invention, the term "and / or" used herein refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0050] In the present invention, unless otherwise specified, each reaction or operation step can be carried out sequentially or in accordance with the sequence. Preferably, the reaction method herein is carried out sequentially.

[0051] Unless otherwise specified, the professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the described content may also be applied to the present invention.

[0052] The present invention provides a composite fiber brush with a micro-spring structure and a preparation method thereof, wherein the raw fiber / film is pretreated; a spring-shaped prefabricated fiber is prepared by rotating and twisting the fiber / film; the spring-shaped prefabricated fiber is stretched to obtain a certain deformation rate; a metal layer is deposited inside and on the surface of the spring-shaped prefabricated fiber with a certain deformation rate to obtain a micro-spring structure composite fiber; and the composite fiber is annealed to prepare a micro-spring structure composite fiber brush. Due to its micro-spring configuration, the composite fiber brush has a lower elastic modulus and good shock absorption performance, which is conducive to obtaining better resistance to current-carrying friction and wear, and can meet the dual requirements of high-power transmission and long life of the brush material.

[0053] See also Figure 1 The present invention provides a method for preparing a composite fiber brush with a micro-spring structure, comprising the following steps:

[0054] S1. Pre-treating the conductive fiber / film;

[0055] The conductive fiber / film is one or more of carbon nanotube fiber, carbon fiber, carbon nanotube film and other conductive fibers or films.

[0056] The diameters of carbon nanotube fibers, carbon fibers and other conductive fibers are 5 to 200 μm, and the thicknesses of carbon nanotube films and other conductive films are 5 to 500 μm.

[0057] The pretreatment method includes one or more of chemical pretreatment and electrochemical pretreatment.

[0058] Among them, chemical pretreatment includes one or more of deoiling, degreasing, purification and acidification.

[0059] The specific operations of chemical pretreatment are:

[0060] Immerse the fiber / film in the reagent, take it out after 5 to 300 seconds, rinse it with running water for 10 to 120 seconds, and then dry it.

[0061] The reagent is one of acetone solution, sulfuric acid solution, nitric acid solution, hydrochloric acid solution, sulfuric acid-nitric acid mixed solution, sulfuric acid-hydrochloric acid mixed solution, nitric acid-hydrochloric acid mixed solution, potassium hydroxide solution, sodium hydroxide solution, potassium hydroxide-sodium hydroxide solution;

[0062] The electrochemical pretreatment includes one or more of anodization and current shock.

[0063] The specific operation of electrochemical pretreatment is:

[0064] The conductive fiber / film is connected to the anode of a DC power supply, and after a set tension is applied to the bottom of the film / fiber, it is immersed in an electrolyte solution together with the cathode, with a current of 0.1 mA to 5 A and a time of 1 to 120 seconds.

[0065] S2, twisting the conductive fiber / film pretreated in step S1 to obtain a spring-shaped prefabricated fiber;

[0066] Twisting is a process in which one end of the fiber / narrow ribbon is fixed and the other end is rotated about its own axis, so that an inclined spiral twist is generated on the outer layer of the fiber / narrow ribbon and the twist is transmitted in the entire axial direction.

[0067] The number of the twisted conductive fibers / films is 1 to 50. When multiple fibers are twisted, their diameters can be the same or different and their lengths can be the same. When multiple carbon films are twisted, their thicknesses can be the same or different and their lengths and widths can be the same.

[0068] The device for twisting the pretreated conductive fiber / film is a twisting machine or a rotary motor, the twisting twist is 10 to 100 r / cm, and the twist is one of a positive twist and a reverse twist.

[0069] The tilt direction of the fiber / film in positive twist is consistent with the middle of the letter S, which is the right-hand direction or clockwise direction;

[0070] The inclination direction of the fiber / film in the reverse twist is consistent with the middle of the letter Z, which is the left-hand direction or counterclockwise direction.

[0071] Twisting is specifically:

[0072] After a plurality of conductive fibers are stranded or a plurality of carbon films are overlapped, one end is fixed and the other end is connected to a twisting machine or a rotating motor to control the rotation direction and number of revolutions of the motor to obtain prefabricated fibers with spring configurations of different twists.

[0073] S3, after stretching the spring configuration prefabricated fiber obtained in step S2 to obtain a set deformation rate, fixing both ends thereof to ensure that the deformation rate remains unchanged;

[0074] After the spring-shaped prefabricated fiber is stretched, the deformation rate (ε=L2 / L1-1) is 1% to 400%, and both ends are fixed with glass sheets or plastic sheets to ensure that the deformation rate remains unchanged.

[0075] S4, using the spring-shaped prefabricated fiber obtained in step S3 as a substrate, depositing a metal layer with a thickness of 1 to 2000 μm on the internal pores and surface of the spring-shaped prefabricated fiber to obtain a composite fiber with a microspring structure;

[0076] The metal in the deposited metal layer includes one or more of gold, silver, copper, platinum, palladium, nickel and tin.

[0077] The metal layer may be deposited by one or more of electrochemical deposition, chemical plating and magnetron sputtering.

[0078] The specific operation of electrochemical deposition is:

[0079] Prepare the corresponding electrolyte solution and metal anode according to the type of deposited metal, connect the spring-shaped prefabricated fiber to the cathode of the DC power supply, immerse it in the electrolyte solution together with the metal anode, and connect the circuit. Electrochemical deposition parameters: current 0.01~10 3 mA, time 10~10 4 s.

[0080] The specific operation of chemical plating is:

[0081] The spring-configuration prefabricated fiber is first placed in a sensitizing solution and magnetically stirred for 10 to 60 minutes for sensitization, then washed and placed in an activation solution and magnetically stirred for 10 to 60 minutes for activation, a crystalline nucleation core is formed on the surface after a reduction reaction, then washed and placed in a corresponding metal precursor solution and magnetically stirred for 20 to 100 minutes to deposit a metal coating on the fiber surface.

[0082] The specific operation of magnetron sputtering is:

[0083] The corresponding target material is prepared according to the type and content of the deposited metal, and the spring-configured prefabricated fiber is placed in a vacuum sputtering instrument. The bombardment parameters are: argon pressure <10Pa, working voltage 1000V, and working current 0.1A; sputtering parameters are: argon pressure 1Pa, bias voltage -500~500V, substrate heating temperature 100~1000℃, and sputtering time 20~1000min.

[0084] S5, annealing the composite fiber obtained in step S4 to eliminate the internal stress generated in the preparation process, and prepare a composite fiber brush with a micro-spring structure.

[0085] The composite fiber obtained in step S4 is placed in a heat treatment furnace for annealing treatment. The annealing atmosphere is one of vacuum, argon and nitrogen. The annealing temperature is 200 to 1400° C. and the time is 20 to 600 minutes.

[0086] The invention discloses a composite fiber brush with a micro-spring structure, which is prepared by adopting the preparation method of the invention.

[0087] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can usually be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0088] Example 1

[0089] First, a carbon nanotube film strip with a thickness of 20 μm, a width of 500 μm and a length of 6 cm was completely immersed in an acetone solution with a volume fraction of 80%, taken out after 30 minutes, rinsed with running water for 120 seconds and then dried.

[0090] Secondly, the right end of the pretreated carbon nanotube film narrow strip is fixed, and the left end is connected to a rotating motor, and the motor is controlled to rotate 90 times in the forward direction, so that the film narrow strip is curled to obtain a spring-shaped prefabricated fiber with a positive twist of 15r / cm.

[0091] Then, the spring-shaped prefabricated fiber is stretched to a deformation rate of 100%, and both ends are fixed with plastic sheets.

[0092] Subsequently, a copper sulfate electroplating solution was prepared, the spring-shaped prefabricated fiber was connected to the cathode of a DC power supply, and immersed in the copper sulfate electroplating solution together with a pure copper anode. The circuit was turned on, the deposition current was 3 mA, and the deposition time was 3600 s to prepare the carbon nanotube / copper composite fiber.

[0093] Finally, the carbon nanotube / copper composite fiber was annealed in a vacuum furnace with a vacuum degree of 10 -3 Pa, temperature 300℃, time 20min, and obtain carbon nanotube / copper composite fiber brush.

[0094] See also Figure 3 , Figure 3 The carbon nanotube / copper composite fiber obtained in Example 1 of the present invention has a copper layer thickness of 50 μm.

[0095] Example 2

[0096] First, a carbon nanotube fiber with a diameter of 5 μm and a length of 20 cm was connected to a DC power anode. After tension was applied to the bottom of the fiber, it was immersed in a 10% sulfuric acid solution together with the cathode, with an anodic oxidation current of 5 mA and a time of 60 s.

[0097] Secondly, the right end of the pretreated carbon nanotube fiber is fixed, and the left end is connected to the twisting machine, and the motor is controlled to reverse 2000 times, so that the carbon nanotube fiber is curled to obtain a spring configuration prefabricated fiber with a reverse twist of 100r / cm.

[0098] Then, the spring-shaped prefabricated fiber was stretched to a deformation rate of 400%, and both ends were fixed with plastic sheets.

[0099] Subsequently, the fiber was first placed in a sensitizing solution and magnetically stirred for 15 minutes for sensitization, then washed and placed in an activation solution and magnetically stirred for 15 minutes for activation, then washed again and placed in a AgNO3-NH3·H2O-HCHO-C2H5OH mixed solution and magnetically stirred at 50°C for 30 minutes to achieve silver plating on the surface of the prefabricated fiber.

[0100] Finally, the carbon nanotube / silver composite fiber was annealed in a vacuum furnace with a vacuum degree of 10 -3 Pa, temperature 200℃, time 600min.

[0101] A carbon nanotube / silver composite fiber brush was obtained, and the thickness of the silver coating was 1 μm.

[0102] Example 3

[0103] First, a carbon nanotube fiber with a diameter of 200 μm and a length of 20 cm was connected to a DC power anode. After tension was applied to the bottom of the fiber, it was immersed in a 10% sulfuric acid solution together with the cathode. The anodic oxidation current was 5 mA and the time was 60 s.

[0104] Secondly, the right end of the pretreated carbon nanotube fiber is fixed, and the left end is connected to the twisting machine, and the motor is controlled to reverse 2000 times, so that the carbon nanotube fiber is curled to obtain a spring configuration prefabricated fiber with a reverse twist of 100r / cm.

[0105] Then, the spring-shaped prefabricated fiber was stretched to a deformation rate of 400%, and both ends were fixed with plastic sheets.

[0106] Subsequently, the fiber was first placed in a sensitizing solution and magnetically stirred for 15 minutes for sensitization, then washed and placed in an activation solution and magnetically stirred for 15 minutes for activation, then washed again and placed in a AgNO3-NH3·H2O-HCHO-C2H5OH mixed solution and magnetically stirred at 50°C for 30 minutes to achieve silver plating on the surface of the prefabricated fiber.

[0107] Finally, the carbon nanotube / silver composite fiber was annealed in a vacuum furnace with a vacuum degree of 10 -3 Pa, temperature 200℃, time 600min.

[0108] A carbon nanotube / silver composite fiber brush was obtained, and the thickness of the silver coating was 2000 μm.

[0109] Example 4

[0110] First, 50 carbon nanotube film narrow strips with a thickness of 5 μm, a width of 10 μm, and a length of 20 cm were immersed in a 10% sulfuric acid solution by volume, taken out after 60 minutes, rinsed with running water for 10 seconds, and then dried.

[0111] Secondly, 50 carbon nanotube film narrow strips are overlapped and fixed at both ends, and the left end is connected to a rotating motor, which is controlled to rotate 200 times in the forward direction. The film narrow strips are curled to obtain a spring-shaped prefabricated fiber with a positive twist of 10r / cm.

[0112] Then, the spring-shaped prefabricated fiber was stretched to a deformation rate of 1%, and both ends were fixed with plastic sheets.

[0113] Subsequently, an AuAg sputtering target was prepared, and the spring-configured prefabricated fiber was placed in a vacuum sputtering instrument with bombardment parameters: argon pressure 10Pa, working voltage 1000V, and working current 0.1A; sputtering parameters: argon pressure 1Pa, bias voltage -200V, substrate heating temperature 300°C, and sputtering time 30min.

[0114] Finally, the carbon nanotube / gold / silver composite fibers were annealed in a vacuum furnace with a vacuum degree of 10 -3 Pa, temperature 1400℃, time 20min.

[0115] A carbon nanotube / gold / silver composite fiber brush was obtained, and the thickness of the silver coating was 10 μm.

[0116] Example 5

[0117] First, five carbon nanotube film narrow strips with a diameter of 200 μm and a length of 10 cm were immersed in a 10% sulfuric acid-nitric acid mixed solution, taken out after 120 minutes, rinsed with running water for 60 seconds and then dried.

[0118] Secondly, five conductive fibers were stranded and fixed at both ends, and the left end was connected to a rotating motor. The motor was controlled to rotate forward 300 times, and the fiber was further curled to obtain a spring-shaped prefabricated fiber with a positive twist of 30 r / cm.

[0119] Then, the spring configuration prefabricated fiber was stretched to 120% of its original length and fixed at both ends with plastic sheets.

[0120] Subsequently, a nickel sulfate electroplating solution was prepared, the spring-shaped prefabricated fiber was connected to the cathode of a DC power supply, and immersed in the nickel sulfate electroplating solution together with a pure nickel anode, and the circuit was turned on. The deposition current was 10 3 mA, deposition time 10 4 s, preparation of carbon nanotube / copper composite fibers.

[0121] Finally, the carbon nanotube / nickel composite fiber was annealed in a vacuum furnace with a vacuum degree of 10 -3 Pa, temperature 500℃, time 60min.

[0122] A carbon nanotube / nickel composite fiber brush is obtained, and the thickness of the nickel plating layer is 2000 μm.

[0123] In summary, the present invention provides a composite fiber brush with a micro-spring structure and a preparation method thereof, wherein the fibers / films are rotationally twisted to prepare a spring-shaped prefabricated fiber; the spring-shaped prefabricated fiber is stretched to obtain a certain deformation rate; a metal layer is deposited inside and on the surface of the spring-shaped prefabricated fiber with a certain deformation rate to obtain a micro-spring structure composite fiber; the composite fiber is annealed to prepare a micro-spring structure composite fiber brush. The preparation process of the method of the present invention is simple, safe, and low-cost. In addition, due to its micro-spring configuration, the composite fiber brush has a lower elastic modulus and good shock-absorbing performance, which is conducive to obtaining better resistance to current-carrying friction and wear, and can meet the dual requirements of high-power transmission and long life of the brush material.

[0124] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite fiber brush with a micro-spring structure and a preparation method thereof, characterized in that: The following steps are involved: S1. Pre-treating the conductive fiber / film; S2, twisting the conductive fiber / film pretreated in step S1 to obtain a spring-shaped prefabricated fiber; S3, after stretching the spring configuration prefabricated fiber obtained in step S2 to obtain a set deformation rate, fixing both ends thereof to ensure that the deformation rate remains unchanged; S4, using the spring-shaped prefabricated fiber obtained in step S3 as a substrate, depositing metal layers on the internal pores and surface of the spring-shaped prefabricated fiber to obtain a composite fiber with a microspring structure; S5, annealing the composite fiber obtained in step S4 to eliminate the internal stress generated in the preparation process, and prepare a composite fiber brush with a micro-spring structure.

2. The composite fiber brush with micro spring structure and the preparation method thereof according to claim 1, characterized in that: In step S1, the diameter of the conductive fiber is 5 to 200 μm, and the thickness of the film is 5 to 500 μm.

3. The composite fiber brush with micro spring structure and the preparation method thereof according to claim 1, characterized in that: In step S1, the pretreatment method includes one or more of chemical pretreatment and electrochemical pretreatment.

4. The composite fiber brush with a micro-spring structure and the preparation method thereof according to claim 3, characterized in that: Chemical pretreatment includes one or more of deoiling, degreasing, purification and acidification; electrochemical pretreatment includes one or more of anodic oxidation and current shock.

5. The composite fiber brush with micro spring structure and the preparation method thereof according to claim 1, characterized in that: In step S2, the number of the conductive fibers / films to be twisted is 1 to 50, and the twisting degree is 10 to 100 r / cm.

6. The composite fiber brush with a micro-spring structure and the preparation method thereof according to claim 1, characterized in that: In step S3, the deformation rate is set to be 1% to 400%.

7. The composite fiber brush with a micro-spring structure and the preparation method thereof according to claim 1, characterized in that: In step S4, the thickness of the deposited metal layer is 1-2000 μm, and the deposited metal includes one or more of gold, silver, copper, platinum, palladium, nickel and tin.

8. The composite fiber brush with a micro-spring structure and the preparation method thereof according to claim 7, characterized in that: The metal layer may be deposited by one or more of electrochemical deposition, chemical plating and magnetron sputtering.

9. The composite fiber brush with a micro-spring structure and the preparation method thereof according to claim 1, characterized in that: In step S5, the atmosphere of the annealing treatment is one of vacuum, argon and nitrogen, the temperature of the annealing treatment is 200-1400° C., and the time is 20-600 min.

10. A composite fiber brush with a micro spring structure, characterized in that: Prepared according to the method according to any one of claims 1 to 9.