Electrode of submerged arc furnace

By preparing a submerged arc furnace electrode without a central through-hole and using a specific ratio of carbonaceous material and liquid material, the problems of low flexural strength and high oxidation consumption of existing electrodes are solved, thereby improving the performance adaptability and service life of the electrode.

CN118973006APending Publication Date: 2024-11-15SHANXI SANYUAN CARBON CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411334809.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing carbon electrodes for electric arc furnaces suffer from problems such as low flexural strength, high resistivity, easy cracking, electrode breakage, and high oxidation consumption. Furthermore, the central hole affects current carrying capacity and smelting purity.

Method used

The electrode is made of a submerged arc furnace without a central through hole. It is prepared by using a specific ratio of carbonaceous material and liquid material through processes such as screening, kneading, and molding to ensure that the particles inside the electrode are densely embedded, thereby improving its flexural strength and oxidation resistance.

Benefits of technology

It improves the flexural strength and oxidation resistance of the electrode, reduces the breakage rate and unit consumption, adapts to high-temperature environments, and improves electrode performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973006A_ABST
    Figure CN118973006A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of conductive materials for submerged arc furnaces, and provides a submerged arc furnace electrode, the center of the submerged arc furnace electrode is not provided with a through hole, the submerged arc furnace electrode is made of a solid material and a liquid material, the solid material is a carbon material, the liquid material is asphalt, the solid material accounts for 65-85% of the total mass, and the liquid material accounts for 10-20% of the total mass. The liquid material asphalt accounts for 15-35% of the total mass; the thermal shock resistance and the oxidation resistance of the produced electrode without the through hole in the center are obviously improved, and the stokehole fracture ratio and the oxidation consumption are greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive materials for submerged arc furnaces, in particular to an electrode used for feeding current into a submerged arc furnace. Background Art

[0002] Submerged arc furnace electrodes are essential functional materials for the smelting of industrial silicon, ferroalloys, yellow phosphorus, and calcium carbide by the carbon reduction method of submerged arc furnaces. At present, submerged arc furnaces all use carbon electrodes with central expansion holes. The solid materials required for the preparation of carbon electrodes include graphite fragments, thermal insulation coke (calcined petroleum coke, a thermal insulation material used in the graphitization process of lithium battery graphite negative electrode materials), calcined petroleum coke, and liquid material coal tar. The process flow is crushing, screening, batching, kneading, cooling, equalizing, dough, molding, cooling, roasting, machining, and inspection. The carbon electrode prepared by this process has a flexural strength of less than 6MPa and a resistivity of more than 30μΩ·m. It is easy to crack and break during use, and has high oxidation consumption. These phenomena of carbon electrodes seriously affect the normal progress of the submerged arc furnace smelting process;

[0003] In addition, although the existence of the central hole in the prior art can partially absorb the expansion and reduce the cracking of the electrode during the manufacturing and use process, the increased inner hole surface accelerates the oxidation consumption of the electrode; secondly, the existence of the inner hole reduces the cross-sectional area, which has a certain negative impact on the carrying current and resistance to bending; thirdly, the coke particles filled in the inner hole can easily bring in impurities, seriously affecting the purity of the smelted alloy.

[0004] To this end, the present invention provides a submerged arc furnace electrode without a through hole in the center. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a submerged arc furnace electrode without a central through hole to solve the problems mentioned in the background technology.

[0006] The utility model relates to an electrode for an electric arc furnace, which is characterized in that there is no through hole in the center of the electrode.

[0007] Preferably, the feedstock comprises solid material and liquid material.

[0008] Preferably, 400-5000 particles with a size of >1 mm are visually observed within an area of ​​10×10 cm taken from any position of the electrode.

[0009] Preferably, the electrode volume density is 1.58-1.68 g / cm 3 , flexural strength 6.0-15.0Mpa, resistivity 8.0-28.0μΩ·m, thermal expansion coefficient 2.2-3.8×10-6K.

[0010] Preferably, the solid material is a carbon material, and the liquid material is asphalt. In terms of mass percentage, the solid material accounts for 65%-85% of the total mass, and the liquid material asphalt accounts for 15%-35% of the total mass.

[0011] Preferably, the carbon material is one or a combination of two or more of artificial graphite, calcined petroleum coke, electrically calcined anthracite, needle coke, pitch coke, and carbon fiber.

[0012] Preferably, the carbonaceous materials artificial graphite, calcined petroleum coke, electric calcined anthracite, needle coke, asphalt coke, and carbon fiber are calculated by mass percentage, with artificial graphite accounting for 20%-100%, calcined petroleum coke accounting for 0%-100%, electric calcined anthracite accounting for 0-10%, needle coke accounting for 0%-50%, asphalt coke accounting for 0-10%, and carbon fiber accounting for 0-10%.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. The flexural strength and oxidation resistance of the electric arc furnace electrode without a central through hole prepared by the present invention are greatly improved, and the electrode can better adapt to the sudden change from room temperature to high temperature, so that the performance of the product is greatly improved, and the breakage rate and unit consumption are greatly reduced.

[0015] 2. The central non-through-hole ore-forming furnace electrode prepared by the present invention can ensure that the product will not have use defects due to its own poor performance in a very harsh working environment, and can better adapt to temperature, electromagnetic and mechanical vibrations. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a process flow chart for preparing a graphite electrode for a mineral heating furnace without a central through hole according to the present invention.

[0017] Figure 2 The present invention is a process flow chart for preparing graphite coke electrodes for a submerged arc furnace without a central through hole.

[0018] Figure 3 The present invention is a process flow chart for preparing graphite electrodes for a mineral heating furnace without a central through hole. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are only used to illustrate the present invention, but cannot be used to limit the scope of the present invention.

[0020] As attached Figure 1 As shown:

[0021] Embodiment 1: This embodiment provides a graphite electrode for a submersible arc furnace without a through hole in the center, which is characterized in that there is no through hole in the center of the electrode.

[0022] The graphite electrode of the electric heating furnace without a central through hole is made of solid material and liquid material.

[0023] Sampling and preparing samples at any position of the electrode, visually observing that the number of particles larger than 1 mm in an area of ​​10×10 cm is 400-900. Within this range, the particles can form an embedded and dense gradation, thereby obtaining a greater flexural strength.

[0024] Electrode volume density 1.58-1.64g / cm 3 , flexural strength 6.0-9.0Mpa, resistivity 22.0-28.0μΩ·m, thermal expansion coefficient 3.3-3.8×10 -6 K.

[0025] The solid material is carbon material, and the liquid material is coal tar. Calculated by mass percentage, the solid material accounts for 77%-79% of the total mass, and the liquid material accounts for 21%-23% of the total mass.

[0026] The carbon raw materials are artificial graphite and calcined petroleum coke. In terms of mass percentage, the artificial graphite accounts for 45%-65% and the calcined petroleum coke accounts for 35%-55%.

[0027] The carbonaceous material is screened and classified into: particle size less than 32 mm and greater than 4 mm, less than 4 mm and greater than 2 mm, less than 2 mm and greater than 1 mm, less than 1 mm and greater than 0.075 mm, and particle size less than 0.075 mm and greater than 0 mm.

[0028] The solid materials of different particle sizes are calculated by percentage of total mass, and the mass proportion of the particle size less than 32mm and greater than 4mm is 10-30%, the mass proportion of the particle size less than 4mm and greater than 2mm is 10-30%, the mass proportion of the particle size less than 2mm and greater than 1mm is 5-15%, the mass proportion of the particle size less than 1mm and greater than 0.075mm is 15-25%, and the mass proportion of the particle size less than 0.075mm is 25-35%. Among them, the mass proportion of the particle size less than 32mm and greater than 4mm is preferably 24%, the mass proportion of the particle size less than 4mm and greater than 2mm is 17%, the mass proportion of the particle size less than 2mm and greater than 1mm is 12%, the mass proportion of the particle size less than 1mm and greater than 0.075mm is 17%, and the mass proportion of the particle size less than 0.075mm is 30%.

[0029] Graphite material of 2-32 mm is preferred as aggregate, and calcined petroleum coke with a particle size range of 0-4 mm is selected as filler; after screening and grading, the ingredients are mixed, the adhesive coal tar is added and kneaded, and then formed, roasted, machined, and inspected to become a graphite electrode for a mineral heating furnace with no through holes in the center.

[0030] The coal tar pitch is added to the ingredients according to the proportion and kneaded in the following manner: the mass of the coal tar pitch accounts for 21-23% of the total mass of all the ingredients, and the preferred proportion of the coal tar pitch is 22%. The mixture is fully stirred and kneaded in a kneading pot to allow the coal tar pitch to fully penetrate into the micropores of the carbon material and form an asphalt film on the surface.

[0031] Through the above process, the use of larger particles of artificial graphite makes it possible for the finished graphite electrode to use the spherical stress dispersion principle to disperse thermal stress, mechanical force, and electromagnetic force, which greatly reduces the breakage rate during use. Secondly, the use of larger particles reduces the contact resistance at the same length, and its own consumption is also reduced.

[0032] like Figure 2 As shown:

[0033] Embodiment 2: This embodiment also provides a graphite coke electrode for an electric arc furnace, which is characterized in that there is no through hole in the center of the electrode.

[0034] The graphite coke electrode for submerged arc furnace is made of solid material and liquid material.

[0035] Sampling and sample preparation are performed at any position of the electrode. Within an area of ​​10×10 cm, the number of particles larger than 1 mm is visually observed to be 1000-3000. Since all solid materials are treated at a high temperature of more than 1800°C, better product performance can be obtained within this range.

[0036] Graphite coke electrode volume density 1.62-1.68g / cm 3 , flexural strength 9.0-15Mpa, resistivity 18.0-24.0μΩ·m, thermal expansion coefficient 3.3-3.7×10 -6 K.

[0037] The solid material is carbon material, and the liquid material is coal tar. In terms of mass percentage, the solid material accounts for 77%-79% of the total mass, and the liquid material accounts for 21%-23% of the total mass. Preferably, the solid material accounts for 77% of the total mass, and the liquid material accounts for 23% of the total mass.

[0038] The carbon material is a combination of calcined petroleum coke and needle coke, wherein the calcined petroleum coke is 70%-100% by mass and the needle coke is 0-30% by mass.

[0039] The calcined petroleum coke and needle coke treated at a high temperature of more than 1800°C are selected and crushed into suitable particle sizes. After batching, coal tar pitch is added into the batching according to the proportion and kneaded. The kneaded paste is cooled, and then the temperature is evenly kneaded. The kneaded paste is molded, and the molded product is cooled, roasted, machined, and inspected to become a graphite coke electrode without a through hole in the center.

[0040] like Figure 3 As shown:

[0041] Embodiment 3: This embodiment also provides a graphite electrode for an electric arc furnace, which is characterized in that there is no through hole in the center of the electrode.

[0042] The graphite electrode of the electric arc furnace without a central through hole is made of solid material and liquid material.

[0043] Sampling and preparing samples at any position of the electrode, visually observing that the number of particles larger than 1 mm in an area of ​​10×10 cm is 600-1200. Within this range, the particles can still form an embedded and dense gradation, thereby obtaining a larger volume density and flexural strength.

[0044] The volume density of the electrode of the submerged arc furnace without a through hole in the center is 1.59-1.63g / cm 3 , flexural strength 6.0-9.0Mpa, resistivity 7-15μΩ·m, thermal expansion coefficient 2.2-3.2×10 -6 K.

[0045] The solid material is carbon material, and the liquid material is coal tar. In terms of mass percentage, the solid material accounts for 77%-79% of the total mass, and the liquid material accounts for 21%-23% of the total mass. Preferably, the solid material accounts for 79% of the total mass, and the liquid material accounts for 21% of the total mass.

[0046] The carbon material is a combination of calcined petroleum coke, artificial graphite and needle coke, wherein by mass percentage, calcined petroleum coke is 50-90%, graphite is 10-20% and needle coke is 0-30%. Preferably, calcined petroleum coke is 60%, graphite is 10% and needle coke is 30%.

[0047] The calcined petroleum coke, artificial graphite and needle coke are crushed into suitable particle sizes, and then the coal tar is added into the ingredients according to the proportion and kneaded. The kneaded paste is cooled, and then the temperature is uniformed. The kneaded paste is formed, and the formed product is cooled, roasted, graphitized, machined, and inspected to become a graphite electrode without a through hole in the center.

[0048] Importantly, it should be noted that the construction and arrangement of the present application shown in a number of different exemplary embodiments are only exemplary. Although only a few embodiments are described in detail in this disclosure, it should be easily understood by those who refer to this disclosure that many modifications are possible (for example, shapes, sizes, dimensions, structures, and product index values ​​of various specifications) without substantially departing from the novel teachings and advantages of the subject matter described in the application. For example, it is used in scenes such as electrolytic aluminum tank linings and ore-heating furnace linings. Therefore, all such modifications are intended to be included in the scope of the present invention. The order or sequence of any process or method steps can be changed or reordered according to alternative embodiments. In the claims, any "device plus function" clause is intended to cover the structure described herein that performs the function, and is not only structurally equivalent but also equivalent structure. Without departing from the scope of the present invention, other replacements, modifications, changes, and omissions can be made in the design, operating conditions, and arrangement of the exemplary embodiments. Therefore, the present invention is not limited to a specific embodiment, but extends to a variety of modifications that still fall within the scope of the appended claims.

[0049] Additionally, in order to provide a concise description of exemplary embodiments, all features of an actual embodiment (ie, those features that are not relevant to the best mode presently contemplated for carrying out the invention or those that are not relevant to implementing the invention) may not be described.

[0050] It will be appreciated that in the development of any actual implementation, as in any engineering or design project, numerous implementation-specific decisions may be made. Such a development effort may be complex and time-consuming, but will be a routine task of design, fabrication, and production for those of ordinary skill having the benefit of this disclosure without undue experimentation.

[0051] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A submerged arc furnace electrode, characterized in that: There is no through hole in the center.

2. The electrode for a submerged arc furnace as claimed in claim 1, characterized in that: Sampling was performed at any position of the electrode and within an area of ​​10×10 cm, visual observation showed that there were 400-5000 particles larger than 1 mm.

3. The electrode for a submerged arc furnace as claimed in claim 1, characterized in that: The electrode volume density is 1.58-1.68 g / cm 3 , flexural strength 6.0-15.0Mpa, resistivity 8.0-28.0μΩ·m, thermal expansion coefficient 2.2-3.8×10 -6 K.

4. The electrode for a submerged arc furnace as claimed in claim 1, characterized in that: The raw materials include solid materials and liquid materials.

5. The electrode for a submerged arc furnace as claimed in claim 4, characterized in that: The solid material is carbon material, and the liquid material is asphalt. In terms of mass percentage, the solid material accounts for 65%-85% of the total mass, and the liquid material asphalt accounts for 15%-35% of the total mass.

6. The electrode for a submerged arc furnace as claimed in claim 5, characterized in that: The carbon material is one or a combination of two or more of artificial graphite, calcined petroleum coke, electrically calcined anthracite, needle coke, pitch coke and carbon fiber.

7. The electrode for a submerged arc furnace as claimed in claim 6, characterized in that: The carbonaceous materials artificial graphite, calcined petroleum coke, electric calcined anthracite, needle coke, asphalt coke and carbon fiber are calculated by mass percentage, with artificial graphite accounting for 20%-100%, calcined petroleum coke accounting for 0%-100%, electric calcined anthracite accounting for 0-10%, needle coke accounting for 0%-50%, asphalt coke accounting for 0-10% and carbon fiber accounting for 0-10%.

Citation Information

Cited By

  • Male and female buckle graphite electrode for electric arc furnace

    CN120008356A