Flexible circuit board based on copper-titanium alloy and manufacturing method thereof
The base material opening is formed and etched through laser processing, which solves the problem that the existing technology cannot etch dumbbell-shaped lines, and realizes force-responsive lines to meet the mechanical performance needs of electronic consumer products.
Patent Information
- Application Number
- CN202410965873.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-15
AI Technical Summary
The existing copper etching process of substrates cannot etch lines with dumbbell-shaped cross-sections, resulting in the inability to form consumer electronics with sensitive force responses.
Laser processing is used to form the base material opening, dry film is applied and exposed to develop, and then etch and dedry film is carried out to form a hollow dumbbell-shaped circuit to achieve simultaneous etching of the front and back sides.
It realizes a dumbbell-shaped circuit with a cross-section, meets the requirements of more sensitive force reactions, is suitable for the transmission of electrical signals and mechanical signals, and meets the mechanical performance requirements of electronic consumer products such as camera modules.
Smart Images

Figure CN118973121A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of flexible circuit board manufacturing, and in particular to a flexible circuit board based on copper-titanium alloy and a manufacturing method thereof. Background Art
[0002] Flexible circuit boards have become an indispensable signal transmission accessory for electronic consumer products due to their unique flexibility. Conventional flexible circuit boards are mostly double-sided boards, with two outer surfaces of copper layers with a thickness of 12 to 50 μm and a dielectric layer in the middle (usually made of polyimide, PI for short), that is, the base material is mainly copper.
[0003] As the speed of electronic consumer product updates continues to increase, a flexible circuit board with certain flexibility and high strength is used as the core component of the camera module. This component has a hollow metal wire structure, which is used to transmit electrical and mechanical signals. The hollow metal wire needs to deform after a certain force is applied, and can return to its original state when the force disappears. This feature cannot be achieved by conventional flexible circuit boards. Therefore, based on the unique mechanical properties of this product, the substrate commonly used is a copper-titanium alloy of 100-150μm.
[0004] Since the structure of the hollowed-out metal wire in this product needs to be very sensitive to force feedback, the cross section of the circuit is required to be dumbbell-shaped (i.e. the circuit in the middle of the entire circuit is narrower, and the circuit at both ends is wider). The narrower circuit in the middle is more likely to deform when subjected to force. However, the existing substrate copper etching process often chooses single-sided etching, and the cross section of the etched circuit is mostly trapezoidal, and it is impossible to etch a circuit with a dumbbell-shaped cross section; if both sides are etched at the same time, the graphics on the front and back sides need to be aligned higher during exposure, and it is also impossible to etch a circuit with a dumbbell-shaped cross section. Summary of the invention
[0005] In view of this, the present invention provides a flexible circuit board based on copper-titanium alloy and a method for manufacturing the same, so as to solve the problem in the prior art that the copper etching process of the substrate is not suitable for the copper-titanium alloy substrate and cannot etch a circuit with a dumbbell-shaped cross-section, resulting in the inability to form electronic consumer products with sensitive force response.
[0006] The present invention provides a method for manufacturing a flexible circuit board based on copper-titanium alloy, comprising:
[0007] Providing a copper-titanium alloy substrate, and laser processing the copper-titanium alloy substrate to obtain a pre-processed alloy plate; wherein a substrate opening is formed on the pre-processed alloy plate;
[0008] Based on the substrate opening, the pre-processed alloy plate is sequentially subjected to dry film application, exposure and development to obtain an alloy plate to be etched; wherein a dry film opening is formed at the substrate opening;
[0009] The alloy plate to be etched is sequentially etched and the dry film is removed, so that a dumbbell-shaped circuit is formed at the opening of the substrate, thereby obtaining a target circuit board.
[0010] Optionally, in the dumbbell-shaped circuit, a first width of the circuit located in the middle region is smaller than a second width of the circuit located in the two end regions, and a difference between the second width and the first width is in a range of .
[0011] Optionally, the etching and dry film removal of the alloy plate to be etched in sequence comprises:
[0012] Provide initial etching solution and dry film removal solution;
[0013] Using the initial etching solution to etch the alloy plate to be etched, to obtain an initial circuit board;
[0014] The desiccant solution is used to desiccant the initial circuit board, so that the dumbbell-shaped circuit is formed at the opening of the substrate in the initial circuit board after the desiccant film is removed, thereby obtaining the target circuit board.
[0015] Optionally, before etching the alloy plate to be etched using the initial etching solution, the method further comprises:
[0016] Adding a revetment agent to the initial etching solution according to a preset ratio to form a target etching solution;
[0017] Correspondingly, the etching of the alloy plate to be etched by using the initial etching solution includes:
[0018] The target etching solution is used to etch the alloy plate to be etched.
[0019] Optionally, the initial etching solution is specifically an etching solution made of hydrochloric acid, cupric chloride and sodium chlorate; and / or, the dry film removing solution is specifically a strong alkaline solution.
[0020] Optionally, the copper-titanium alloy substrate is laser processed to obtain a pre-processed alloy plate, comprising:
[0021] Using a laser process, according to preset circuit design parameters, the copper-titanium alloy substrate is laser processed to form the substrate opening on the copper-titanium alloy substrate to obtain the pre-processed alloy plate;
[0022] The preset line design parameters include preset line position, preset line distance and preset line width.
[0023] Optionally, the laser processing process, according to preset circuit design parameters, performs laser processing on the copper-titanium alloy substrate, further includes:
[0024] The laser process is adopted to perform laser processing on the copper-titanium alloy substrate according to preset alignment through-hole parameters, so as to form a plurality of exposure alignment holes in the waste area of the copper-titanium alloy substrate.
[0025] Optionally, the size of the substrate opening is smaller than the size of the dry film opening.
[0026] Optionally, with the width direction of the dumbbell-shaped circuit as the x direction and the length direction of the dumbbell-shaped circuit as the y direction, the length of the substrate opening along the x direction is less than the length of the dry film opening along the x direction, and the length of the substrate opening along the y direction is less than or equal to the length of the dry film opening along the y direction.
[0027] Optionally, the difference between the length of the dry film opening along the x-direction and the length of the substrate opening along the x-direction is greater than or equal to 40 μm.
[0028] Optionally, the length of the substrate opening along the x-direction ranges from 20 to 40 μm; and / or the length of the dry film opening along the x-direction ranges from 60 to 80 μm.
[0029] In addition, the present invention also provides a flexible circuit board based on copper-titanium alloy, which is manufactured using the aforementioned manufacturing method.
[0030] The beneficial effects of the present invention are as follows: before the entire circuit production including dry film pasting, exposure, development and etching, the provided copper-titanium alloy substrate is firstly laser processed to form a pre-processed alloy plate with a substrate opening, which can realize simultaneous etching of the front and back sides, and can also facilitate subsequent circuit etching. Due to the side etching effect, a hollow circuit with a dumbbell-shaped cross section is formed at the substrate opening (i.e., a dumbbell-shaped circuit, wherein the circuit in the middle area of the dumbbell-shaped circuit is narrower and the circuit in the two end areas is wider); based on the dumbbell-shaped circuit, it can meet the requirements of more sensitive force response, better bear the transmission of electrical signals and mechanical signals, and thus meet the mechanical performance requirements of electronic consumer products such as camera modules. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The features and advantages of the present invention will be more clearly understood by referring to the accompanying drawings, which are schematic and should not be construed as limiting the present invention in any way. In the accompanying drawings:
[0032] Figure 1 The main production flow chart of etching circuits using conventional etching technology is shown;
[0033] Figure 2A flow chart showing a method for manufacturing a flexible circuit board based on copper-titanium alloy in Embodiment 1 of the present invention is shown;
[0034] Figure 3 The top view of the copper-titanium alloy substrate in the first embodiment of the present invention is shown;
[0035] Figure 4 The top view of the pre-processed alloy plate in the first embodiment of the present invention is shown;
[0036] Figure 5 The top view of the alloy plate to be etched in the first embodiment of the present invention is shown;
[0037] Figure 6 The cross-sectional structure diagram of the target circuit board obtained when no revetment agent is added to the initial etching solution in the first embodiment of the present invention is shown;
[0038] Figure 7 The cross-sectional structure diagram of the target circuit board obtained when the bank protection agent is added to the initial etching solution in the first embodiment of the present invention is shown;
[0039] Figure 8 The main flow chart of the method for manufacturing a flexible circuit board based on copper-titanium alloy of the present invention is shown.
[0040] The description of each reference numeral is as follows:
[0041] 1. Copper-titanium alloy substrate, 2. substrate opening, 3. dry film, 4. dry film opening, 5. dumbbell-shaped circuit. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0043] The core components of the camera module need to be made of flexible circuit boards with certain flexibility and high strength. In order to transmit electrical and mechanical signals, the flexible circuit boards need to be made into hollow metal wires. The hollow metal wires need to deform when a certain force is applied, and return to their original state when the force disappears. At this time, copper-titanium alloy is usually used as the base material.
[0044] For copper-titanium alloy substrates, traditional etching technology is used to etch circuits. The main production process is as follows: Figure 1As shown, it includes dry film lamination → exposure and development → etching → dry film removal. The cross-section of the circuits produced is mostly trapezoidal or has a wide circuit in the middle area and narrow circuits at both ends. It is impossible to etch a circuit with a dumbbell cross-section. Figure 1 In the figure, 1 is a copper-titanium alloy substrate, and 3 is a dry film.
[0045] In this regard, the present invention provides the following copper-titanium alloy-based flexible circuit board and its manufacturing method to solve the problem that the existing etching process is not suitable for the copper-titanium alloy substrate and cannot etch a dumbbell-shaped circuit, resulting in the inability to form electronic consumer products with sensitive force response.
[0046] Embodiment 1
[0047] This embodiment provides a method for manufacturing a flexible circuit board based on copper-titanium alloy, such as Figure 2 As shown, including:
[0048] S1: providing a copper-titanium alloy substrate, and laser processing the copper-titanium alloy substrate to obtain a pre-processed alloy plate; wherein a substrate opening is formed on the pre-processed alloy plate;
[0049] S2: Based on the substrate opening, sequentially applying a dry film and performing exposure and development on the pre-processed alloy plate to obtain an alloy plate to be etched; wherein a dry film opening is formed at the substrate opening;
[0050] S3: etching and removing the dry film of the alloy plate to be etched in sequence, so that a dumbbell-shaped circuit is formed at the opening of the substrate, thereby obtaining a target circuit board.
[0051] In this embodiment, before the entire circuit production including dry film pasting, exposure, development and etching, the provided copper-titanium alloy substrate is first laser processed to form a pre-processed alloy plate with a substrate opening, which can realize simultaneous etching of the front and back sides, and can also facilitate subsequent circuit etching. Due to the side etching effect, a hollow circuit with a dumbbell-shaped cross-section is formed at the substrate opening (i.e., a dumbbell-shaped circuit, the circuit in the middle area of the dumbbell-shaped circuit is narrower, and the circuit in the two end areas is wider); based on the dumbbell-shaped circuit, it can meet the requirements of more sensitive force response, better bear the transmission of electrical signals and mechanical signals, and thus meet the mechanical performance requirements required by electronic consumer products such as camera modules.
[0052] The following describes in detail each step of the manufacturing method of this embodiment.
[0053] Preferably, the material of the copper-titanium alloy substrate in the present embodiment S1 is copper-titanium alloy, wherein copper is the main element and its content is usually between 60% and 90%, and the content of titanium is usually between 1% and 40%; the thickness of the entire copper-titanium alloy substrate is 100 to 150 μm.
[0054] In the present embodiment S1, the copper-titanium alloy substrate is laser processed to obtain a pre-processed alloy plate, including:
[0055] Using a laser process, according to preset circuit design parameters, the copper-titanium alloy substrate is laser processed to form the substrate opening on the copper-titanium alloy substrate to obtain the pre-processed alloy plate;
[0056] The preset line design parameters include preset line position, preset line distance and preset line width.
[0057] According to the above steps, the copper-titanium alloy substrate is first laser processed before the formal etching of the circuit, which can ensure that the substrate opening is accurately formed at the position where the hollow dumbbell-shaped circuit needs to be formed later, so that the dumbbell-shaped circuit can be accurately formed by side etching later, so that the entire target circuit board has good electrical and mechanical properties.
[0058] Among them, the preset line position in the preset line design parameters specifies the specific positions of various lines (including dumbbell-shaped lines and other types of lines) in the line layer, and the preset line spacing and preset line width respectively specify the line spacing and line width of each line. Laser processing according to the preset line design parameters can effectively ensure the production accuracy of the dumbbell-shaped line.
[0059] Specifically, the number of the substrate openings formed in this embodiment is one or more.
[0060] Specifically, the top view structure of the copper-titanium alloy substrate of this embodiment is as follows: Figure 3 As shown, the top view structure of the pre-processed alloy plate obtained after laser processing is as follows Figure 4 As shown, in Figure 3 and Figure 4 In the figure, 1 is the copper-titanium alloy substrate, and 2 is the substrate opening (the number of the substrate openings is 3).
[0061] Preferably, the copper-titanium alloy substrate is laser processed by a laser process according to preset circuit design parameters, and further comprises:
[0062] The laser process is adopted to perform laser processing on the copper-titanium alloy substrate according to preset alignment through-hole parameters, so as to form a plurality of exposure alignment holes in the waste area of the copper-titanium alloy substrate.
[0063] In the laser process, multiple exposure alignment holes are also made according to the preset alignment through-hole parameters. These exposure alignment holes can be used for precise alignment between the exposure base plate and the pre-processed alloy plate in the subsequent exposure and development process, which can help improve the exposure accuracy and further improve the circuit production accuracy when etching both sides of the pre-processed alloy plate at the same time.
[0064] The number, diameter and specific location of the exposure alignment holes in the waste area of the copper-titanium alloy substrate can be determined according to the specific situation. In this embodiment, the number of exposure alignment holes is 4, which are respectively located in the waste areas of the four corners of the pre-processed alloy plate (the alloy plate is usually square), and the diameter of each hole is 2 mm ( Figure 4 The exposure alignment hole is not shown).
[0065] Specifically, in Figure 4 In the example, the width direction of the dumbbell-shaped circuit finally formed is taken as the x direction (i.e. Figure 4 The x direction in the figure), the length direction of the dumbbell-shaped line is the y direction (i.e. Figure 4 The length of the substrate opening along the x direction is in the range of 20 to 40 μm.
[0066] Specifically, in the present embodiment S2, the pre-processed alloy plate is subjected to dry film bonding and exposure and development based on the substrate opening, so that the areas that need to be etched in the entire pre-processed alloy plate are exposed from the dry film opening, while the areas that do not need to be etched are covered by the dry film, thereby ensuring the precise production of the dumbbell-shaped circuit.
[0067] It should be understood that the exposed areas of the dry film in the pre-processed alloy plate include not only the position areas corresponding to the dumbbell-shaped circuits, but also the position areas corresponding to other types of circuits, that is, the areas that need to be etched in the entire pre-processed alloy plate will be exposed and not covered by the dry film, while the areas that do not need to be etched will be covered by the dry film.
[0068] Specifically, during the exposure process, an LDI exposure machine or a fully automatic alignment exposure machine is used. When exposing the front and back sides, four 2.0mm exposure alignment through holes of the laser are used as reference holes, so that the alignment between the exposure base plate and the pre-processed alloy plate is more precise, and the position of the dry film opening and the substrate opening after development is more precise, effectively ensuring that an excellent dumbbell-shaped circuit is obtained after etching.
[0069] The top view structure of the alloy plate to be etched obtained after dry film lamination, exposure and development in this embodiment is as follows: Figure 5 As shown. Figure 5 In the figure, 3 is the dry film and 4 is the dry film opening.
[0070] like Figure 5 As shown, the size of the substrate opening 2 is smaller than the size of the dry film opening 4 .
[0071] Since there is a certain alignment offset in the exposure process, the substrate opening is smaller than the size of the dry film opening, and a certain offset can be reserved for exposure to prevent the dry film from covering the substrate opening after exposure and development, resulting in the substrate opening being unable to be etched, thereby making it impossible to produce precise dumbbell-shaped circuits.
[0072] Further, the length of the substrate opening along the x direction is smaller than the length of the dry film opening along the x direction, and the length of the substrate opening along the y direction is smaller than or equal to the length of the dry film opening along the y direction.
[0073] By limiting the lengths in the above two directions, it can be effectively ensured that the substrate opening is smaller than the size of the dry film opening, thereby effectively ensuring the manufacturing accuracy of the subsequent dumbbell-shaped circuit.
[0074] Furthermore, a difference between a length of the dry film opening along the x direction and a length of the substrate opening along the x direction is less than or equal to 40 μm.
[0075] The offset of the exposure equipment is usually ±20μm, and the length of the dry film opening along the x direction (i.e. Figure 5 The difference between d2 in the figure and the length of the substrate opening along the x direction (i.e. Figure 5 The d1) in the figure is greater than or equal to 40 μm, which can effectively ensure that after exposure and development, the dry film will not cover the substrate opening due to exposure offset, thereby ensuring the production of precise dumbbell-shaped circuits.
[0076] Specifically, in Figure 5 In the embodiment, the length of the substrate opening along the x direction ranges from 20 to 40 μm, and the length of the dry film opening along the x direction ranges from 60 to 80 μm.
[0077] Preferably, this embodiment S3 includes:
[0078] S31: providing initial etching solution and dry film removal solution;
[0079] S32: using the initial etching solution to etch the alloy plate to obtain an initial circuit board;
[0080] S33: using the desiccant solution to desiccant the initial circuit board, so that the dumbbell-shaped circuit is formed at the opening of the substrate in the initial circuit board after the desiccant is removed, thereby obtaining the target circuit board.
[0081] Through the above steps, a dumbbell-shaped circuit with high manufacturing accuracy and excellent quality can be formed at the opening of the substrate, thereby meeting the mechanical performance requirements of electronic consumer products such as camera modules.
[0082] Specifically, in S31, the initial etching solution is an etching solution made of hydrochloric acid, cupric chloride and sodium chlorate.
[0083] In the above etching solution, cupric chloride is the main copper source, providing copper ions (Cu 2+) undergoes an oxidation-reduction reaction with metallic copper, dissolving the copper and removing it from the metal surface. Hydrochloric acid plays a role in adjusting the acidity of the solution and promoting the dissolution of copper; at the same time, it can also react with the oxides on the metal surface, clean the metal surface, and improve the etching effect. Sodium chlorate is an oxidant in the etching solution. It can decompose under acidic conditions to produce substances with strong oxidizing properties. These oxidizing substances can accelerate the oxidation and dissolution process of copper, thereby improving the etching rate and uniformity. The above-mentioned initial etching solution can effectively etch the alloy plate to be etched.
[0084] Specifically, in S31, the dry film removing solution is a strong alkaline solution.
[0085] The strong alkaline solution effectively dissolves or decomposes the dry film material due to its strong corrosive property, thereby removing it from the surface of the pre-processed alloy plate, achieving an excellent dry film removal effect.
[0086] The strong alkaline solution can be selected according to the actual situation, and 3% to 5% NaOH solution is usually used.
[0087] Preferably, before S32, the method further includes:
[0088] S34: adding a revetment agent to the initial etching solution according to a preset ratio to form a target etching solution.
[0089] Correspondingly, S32 includes:
[0090] The target etching solution is used to etch the alloy plate to be etched.
[0091] During the etching process, etching will proceed in all directions, causing the copper on the side walls of the circuit edges to be etched away, causing the side walls of the circuit to be tilted. By adding a revetment agent to the initial etching solution, as an organic additive in the etching solution, the revetment agent can form a layer of film adhesion on both sides of the circuit where the water flow is weaker, slowing down the diffusion rate of ions in the etching solution, reducing the attack intensity of the etching solution on the metal layer, thereby reducing the degree of side corrosion. By adding the revetment agent to form a target etching solution, and using the target etching solution to etch the alloy plate to be etched, the circuit in the middle of the etched circuit cross section can be made thinner.
[0092] Among them, the main components of the shore protection agent include organic solvents (such as toluene), extractants, stabilizers, protective agents, etc. The appropriate material components and material proportions can be selected according to actual conditions and are not limited here.
[0093] Specifically, in the etching process of S32, the target etching solution is sprayed onto the upper and lower surfaces of the alloy plate to be etched by a spraying method, and the spraying time is 12 minutes.
[0094] Specifically, in the dumbbell-shaped circuit, a first width of the circuit located in the middle region is smaller than a second width of the circuit located in the two end regions, and a difference between the second width and the first width ranges from 5 to 20 μm.
[0095] The dumbbell-shaped circuit with the above-mentioned width difference can not only bear the transmission of electrical signals, but also has good force response performance. It can better bear the transmission of mechanical signals, deform after a certain force is applied, and can return to its original state when the force disappears. It is suitable for the mechanical performance requirements required by electronic consumer products such as camera modules.
[0096] Furthermore, when no revetment agent is added to the initial etching solution, the difference between the second width and the first width ranges from 5 to 15 μm; when a revetment agent is added to the initial etching solution, the difference between the second width and the first width ranges from 15 to 20 μm.
[0097] The cross-sectional structure of the target circuit board obtained after etching and removing the dry film in this embodiment is as follows: Figure 6 and Figure 7 As shown, Figure 6 It is the cross-sectional structure of the target circuit board obtained when no revetment agent is added to the initial etching solution. Figure 7 It is the cross-sectional structure of the target circuit board obtained when the initial etching solution contains a revetment agent. Figure 6 and Figure 7 5 is a dumbbell-shaped line, and the width of both ends (i.e., the second width, corresponding to Figure 6 and Figure 7 The width in the middle (i.e. the first width, corresponding to Figure 6 and Figure 7 w2) is narrower, Figure 6 The difference between w2 and w1 ranges from 5 to 15 μm. Figure 6 The difference between w2 and w1 ranges from 15 to 20 μm.
[0098] After the de-drying film is removed, the alloy plate to be etched can also be subjected to other conventional manufacturing processes, such as chemical nickel-gold, etc. These are conventional processes in the field of flexible circuit board manufacturing and will not be described in detail here.
[0099] The main process of the method for manufacturing a flexible circuit board based on copper-titanium alloy described in this embodiment is as follows: Figure 8 As shown, it includes laser opening → dry film lamination → exposure and development → etching → dry film removal.
[0100] By processing the copper-titanium alloy substrate using the method described in this embodiment, a copper-titanium alloy flexible circuit board with a metal wire structure having a line width of 30 to 70 μm, a line spacing of 130 to 170 μm, and a thickness of 100 to 150 μm can be obtained.
[0101] In this embodiment, the flexible circuit board is manufactured according to the following four specific implementation methods.
[0102] Implementation method 1: The copper-titanium alloy substrate is 100 μm thick, the width of the substrate opening is 20 μm, the dry film thickness is 40 μm, the width of the dry film on the circuit after development is 140 μm, and the width of the dry film opening exposing the substrate is 60 μm. Etching is performed using an etching solution with a revetment agent added. After removing the dry film, a target circuit board with a line width of 70 μm, a line spacing of 130 μm, and a hollow dumbbell-shaped circuit cross-section with a width of 50 μm in the middle position can be obtained.
[0103] Embodiment 2: The copper-titanium alloy substrate is 120 μm thick, the width of the substrate opening is 30 μm, the dry film thickness is 40 μm, the width of the dry film on the circuit after development is 130 μm, and the width of the dry film opening exposing the substrate is 70 μm. Etching is performed using an etching solution with a revetment agent added. After removing the dry film, a target circuit board with a line width of 50 μm, a line spacing of 150 μm, and a hollow dumbbell-shaped circuit cross-section with a width of 30 μm in the middle position can be obtained.
[0104] Embodiment 3: The copper-titanium alloy substrate is 120 μm thick, the width of the substrate opening is 30 μm, the dry film thickness is 40 μm, the dry film width on the circuit after development is 130 μm, and the width of the dry film opening exposing the substrate is 70 μm. After etching in an etching solution without adding a revetment agent, after removing the dry film, a target circuit board with a line width of 50 μm, a line spacing of 150 μm, and a hollow dumbbell-shaped circuit cross-section with a width of 45 μm in the middle position can be obtained.
[0105] Embodiment 4: The copper-titanium alloy substrate is 150μm thick, the width of the substrate opening is 40μm, the dry film thickness is 40μm, the dry film width on the circuit after development is 120μm, and the width of the dry film opening exposing the substrate is 80μm. Etching is performed using an etching solution with a revetment agent added. After removing the dry film, a target circuit board with a line width of 40μm, a line spacing of 160μm, and a hollow dumbbell-shaped circuit cross-section with a width of 25μm in the middle position can be obtained.
[0106] Embodiment 2
[0107] This embodiment provides a flexible circuit board based on copper-titanium alloy, which is manufactured by using the manufacturing method of the flexible circuit board based on copper-titanium alloy described in the first embodiment.
[0108] The flexible circuit board manufactured in this embodiment can be etched on both the front and back sides at the same time, and can form a hollow circuit with a dumbbell-shaped cross-section at the opening of the substrate; based on the dumbbell-shaped circuit, it can meet the requirements of more sensitive force response, better bear the transmission of electrical signals and mechanical signals, and thus can meet the mechanical performance requirements required by electronic consumer products such as camera modules.
[0109] The manufacturing method of the copper-titanium alloy-based flexible circuit board in this embodiment is the same as the method steps described in the first embodiment. Therefore, for details not provided in this embodiment, please refer to the first embodiment and the second embodiment. Figures 1 to 8 The specific description of this embodiment will not be repeated in detail.
[0110] Although the embodiments of the present invention have been described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.
Claims
1. A method for manufacturing a flexible circuit board based on copper-titanium alloy, characterized in that: The method comprises: Providing a copper-titanium alloy substrate, and laser processing the copper-titanium alloy substrate to obtain a pre-processed alloy plate; wherein a substrate opening is formed on the pre-processed alloy plate; Based on the substrate opening, the pre-processed alloy plate is sequentially subjected to dry film application, exposure and development to obtain an alloy plate to be etched; wherein a dry film opening is formed at the substrate opening; The alloy plate to be etched is sequentially etched and the dry film is removed, so that a dumbbell-shaped circuit is formed at the opening of the substrate, thereby obtaining a target circuit board.
2. The method according to claim 1, characterized in that: In the dumbbell-shaped circuit, a first width of the circuit located in the middle region is smaller than a second width of the circuit located in the two end regions, and a difference between the second width and the first width ranges from 5 to 20 μm.
3. The method according to claim 1, characterized in that: The step of sequentially etching the alloy plate to be etched and removing the dry film comprises: Provide initial etching solution and dry film removal solution; Using the initial etching solution to etch the alloy plate to be etched, to obtain an initial circuit board; The desiccant solution is used to desiccant the initial circuit board, so that the dumbbell-shaped circuit is formed at the opening of the substrate in the initial circuit board after the desiccant film is removed, thereby obtaining the target circuit board.
4. The method according to claim 3, characterized in that: Before etching the alloy plate to be etched using the initial etching solution, the method further comprises: Adding a revetment agent to the initial etching solution according to a preset ratio to form a target etching solution; Correspondingly, the etching of the alloy plate to be etched by using the initial etching solution includes: The target etching solution is used to etch the alloy plate to be etched.
5. The manufacturing method according to claim 3, characterized in that: The initial etching solution is specifically an etching solution made of hydrochloric acid, cupric chloride and sodium chlorate; and / or, the dry film removing solution is specifically a strong alkaline solution.
6. The method according to claim 1, characterized in that: The method of laser processing the copper-titanium alloy substrate to obtain a pre-processed alloy plate comprises: Using a laser process, according to preset circuit design parameters, the copper-titanium alloy substrate is laser processed to form the substrate opening on the copper-titanium alloy substrate to obtain the pre-processed alloy plate; The preset line design parameters include preset line position, preset line distance and preset line width.
7. The manufacturing method according to claim 6, characterized in that: The laser processing method includes laser processing the copper-titanium alloy substrate according to preset circuit design parameters, and further includes: The laser process is adopted to perform laser processing on the copper-titanium alloy substrate according to preset alignment through-hole parameters, so as to form a plurality of exposure alignment holes in the waste area of the copper-titanium alloy substrate.
8. The manufacturing method according to claim 1, characterized in that: The size of the substrate opening is smaller than the size of the dry film opening.
9. The manufacturing method according to claim 8, characterized in that: Taking the width direction of the dumbbell-shaped circuit as the x direction and the length direction of the dumbbell-shaped circuit as the y direction, the length of the substrate opening along the x direction is less than the length of the dry film opening along the x direction, and the length of the substrate opening along the y direction is less than or equal to the length of the dry film opening along the y direction.
10. The manufacturing method according to claim 9, characterized in that: The difference between the length of the dry film opening along the x direction and the length of the substrate opening along the x direction is greater than or equal to 40 μm.
11. The manufacturing method according to claim 9, characterized in that: The length of the substrate opening along the x-direction ranges from 20 to 40 μm; and / or the length of the dry film opening along the x-direction ranges from 60 to 80 μm.
12. A flexible circuit board based on copper-titanium alloy, characterized in that: The method is as described in any one of claims 1 to 11.
Citation Information
Cited By
Flexible circuit board etching process