Perovskite absorption layer and preparation method and application thereof
By evaporateing inorganic salts and passivating agents into perovskite solar cells to form an inorganic frame layer and adding organic salt solution, the problem of insufficient organic solvent reaction in the perovskite absorption layer is solved, and the perovskite solar cell is improved performance.
Patent Information
- Application Number
- CN202411022593.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
During the preparation of the existing perovskite absorption layer, due to the thick thickness of the inorganic frame layer, the organic solvent cannot fully react with the underlying inorganic salts, affecting the performance of perovskite solar cells.
By co-evaporating the inorganic salt and passivating agent on the surface of the substrate, and adding organic salt solution to the side of the inorganic frame layer away from the substrate, react and annealing to form a perovskite absorption layer, optimizing the passivating agent ratio and annealing conditions To promote the reaction between organic salts and inorganic salts.
The performance of perovskite solar cells is improved, and the photovoltaic performance of the cells is improved by uniformly distributing the reaction of passivator and organic salts.
Smart Images

Figure CN118973356A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and to a perovskite absorption layer and a preparation method and application thereof, and in particular to a perovskite absorption layer and a preparation method thereof, a perovskite solar cell comprising the perovskite absorption layer and a preparation method thereof, a photovoltaic module and a photovoltaic system. Background Art
[0002] In the photovoltaic power generation technology route, titanium ore cells have low cost, can form stacked cells, and have higher ultimate efficiency. The perovskite absorber layer is the core component of perovskite solar cells. The absorption band gap, grain size, crystal composition, structure, uniformity of the film, and coverage of the substrate of the perovskite absorber layer will directly affect the photovoltaic performance of perovskite solar cells.
[0003] At present, there are many methods for preparing perovskite absorption layers, such as vacuum evaporation, spin coating, magnetron sputtering, atomic deposition, electrochemical deposition, etc. Among them, in the process involving evaporation + solution preparation, the passivator is added to the organic solvent. However, the thickness of the evaporated inorganic framework layer in the suede stack is relatively thick, which will cause the organic solvent to be unable to fully react with the underlying inorganic salt, thereby affecting the performance of the perovskite solar cell.
[0004] In view of the problems existing in the existing technology, it is very necessary to develop a new type of perovskite absorption layer to improve the performance of perovskite solar cells. Summary of the invention
[0005] The embodiments of the present application provide a perovskite absorption layer and a preparation method and application thereof, in particular, a perovskite absorption layer and a preparation method thereof, a perovskite solar cell comprising the perovskite absorption layer and a preparation method thereof, a photovoltaic module and a photovoltaic system, so as to solve or alleviate the technical problems raised above.
[0006] In a first aspect, an embodiment of the present application provides a method for preparing a perovskite absorption layer, the preparation method comprising:
[0007] (1) forming an inorganic framework layer by co-evaporating an inorganic salt and a passivating agent on a surface of one side of the substrate;
[0008] (2) Adding an organic salt solution to the surface of the inorganic framework layer away from the substrate, reacting, and annealing to form a perovskite absorption layer.
[0009] Optionally, the inorganic salt in step (1) includes any one of PbI2, CsBr, PbBr or CsI, or a combination of at least two of them.
[0010] Optionally, the passivating agent in step (1) includes any one of PEAI, CF3-PACl, PDADI, OAI or TEACL, or a combination of at least two thereof.
[0011] Optionally, the co-evaporation ratio of the inorganic salt and the passivating agent in step (1) is [1-1.5]:[0.01-0.1].
[0012] Optionally, when the inorganic salt in step (1) is a combination of PbI2 and CsBr, and the passivating agent is PDADI, the co-evaporation ratio of PbI2, CsBr and PDADI is 1:[0.1-0.3]:[0.01-0.05].
[0013] Optionally, the co-evaporation in step (1) comprises: melting the inorganic salt and the passivating agent separately under vacuum conditions, evaporating the molten substances and depositing them on the substrate.
[0014] Optionally, the vacuum degree of the vacuum condition is ≤5E -6 torr.
[0015] Optionally, the melting and evaporation temperature is lower than the decomposition temperature of the organic compound and the lithium-containing metal compound.
[0016] Optionally, the evaporation method includes heating evaporation or electron beam evaporation.
[0017] Optionally, the deposition thickness is 600-800 nm.
[0018] Optionally, the solute of the organic salt solution in step (2) is any one of FAI, FABr, MACl or MASCN or a combination of at least two thereof, and the solvent is any one of ethanol, isopropanol or N,N-dimethylformamide or a combination of at least two thereof.
[0019] Optionally, the molar concentration of the organic salt solution in step (2) is 1.4-2.5 mol / L.
[0020] Optionally, before adding the organic salt solution to the inorganic framework layer in step (2), the inorganic framework layer is pre-annealed, wherein the pre-annealing is performed in a nitrogen environment, the pre-annealing temperature is 120-200° C., and the pre-annealing time is 0.5-2 min.
[0021] Optionally, the annealing in step (2) includes primary annealing and secondary annealing;
[0022] The primary annealing is performed in a nitrogen environment at a temperature of 80-120° C. and a time of 1-5 min.
[0023] The secondary annealing is carried out in air, the temperature of the secondary annealing is 120-200° C., and the time of the secondary annealing is 10-30 minutes.
[0024] In a second aspect, an embodiment of the present application provides a perovskite absorption layer, which is prepared by the above-mentioned preparation method.
[0025] In a third aspect, the present application provides a laminated perovskite solar cell, comprising:
[0026] Basal layer;
[0027] A hole transport layer, a perovskite absorption layer, an electron transport layer and a first electrode layer are sequentially stacked on a surface of one side of the substrate layer, wherein the perovskite absorption layer is the above-mentioned perovskite absorption layer;
[0028] And a second electrode layer is arranged on the other side surface of the substrate layer.
[0029] In a fourth aspect, an embodiment of the present application provides a photovoltaic module, comprising a plurality of perovskite solar cells connected in series and / or in parallel; wherein at least one perovskite solar cell is the stacked perovskite solar cell described in the first aspect.
[0030] In a fifth aspect, an embodiment of the present application provides a photovoltaic system, wherein the photovoltaic system includes the photovoltaic component described in the third aspect.
[0031] The above technical solution adopted in the embodiment of the present application may have the following advantages:
[0032] When preparing the perovskite absorption layer, the inorganic salt and the passivator are evaporated together so that the low-doped passivator is evenly distributed in the inorganic layer. After the organic salt solution is added, the passivator can leave some vacancies, allowing the excess organic salt to penetrate and react with the inorganic salt at the bottom layer, thereby improving the performance of the perovskite solar cell. In addition, the selection of some passivators can not only leave vacancies, allowing the excess organic salt to penetrate and react with the inorganic salt at the bottom layer, but also promote the reaction between the organic salt and the inorganic salt, thereby improving the reaction efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0034] Figure 1 Schematic diagram of the materials used for the inorganic framework layer in the embodiment.
[0035] Figure 2Schematic diagram of the formation of the perovskite absorption layer in the embodiment.
[0036] Figure 3 This is the structure of the stacked perovskite solar cell provided in the embodiment of the present application.
[0037] Description of reference numerals:
[0038] 010 is the second electrode layer; 020 is the base layer; 030 is the hole transport layer; 040 is the perovskite absorption layer; 050 is the electron transport layer; and 060 is the first electrode layer. DETAILED DESCRIPTION
[0039] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.
[0040] The present application embodiment provides a method for preparing a perovskite absorption layer, comprising:
[0041] (1) forming an inorganic framework layer by co-evaporating an inorganic salt and a passivating agent on a surface of one side of the substrate;
[0042] (2) Adding an organic salt solution to the surface of the inorganic framework layer away from the substrate, reacting, and annealing to form a perovskite absorption layer.
[0043] When forming the perovskite absorption layer, the inorganic salt includes any one of PbI2, CsBr, PbBr or CsI, or a combination of at least two of them; the passivator includes any one of PEAI (phenylethylammonium iodide), CF3-PACl (4-aminobenzotrifluoride hydrochloric acid), PDADI (1,4-phenylenediamine hydroiodide), OAI (octylamine iodide) or TEACL (thiopheneethylamine hydrochloride), or a combination of at least two of them; the co-evaporation ratio of the inorganic salt and the passivator is [1-1.5]:[0.01-0.1], and exemplarily, the co-evaporation ratio of the inorganic salt and the passivator is 1:0.01, 1:0.03, 1:0.05, 1:0.08 or 1:0.1.
[0044] When forming the inorganic framework layer, the inorganic salt and the passivator are co-evaporated in a specific ratio, so that the low-doped passivator can be evenly distributed in the inorganic framework layer, so that after the organic salt solution is added, the inorganic salt can fully react with the organic salt.
[0045] When forming the perovskite absorption layer, choosing a specific type of passivator can not only leave vacancies to allow excess organic salts to penetrate and react with the underlying inorganic salts, but also promote the reaction between organic and inorganic salts and improve reaction efficiency.
[0046] In some embodiments, Figure 1 As shown, the inorganic salt is a combination of PbI2 and CsBr, and the passivating agent is PDADI (1,4-phenylenediamine hydroiodide). When this combination is used, the co-evaporation ratio of PbI2, CsBr and PDADI is 1:[0.1-0.3]:[0.01-0.05].
[0047] In some embodiments, the co-evaporation comprises: melting the inorganic salt and the passivating agent separately under vacuum conditions, evaporating the molten substances and depositing them on the substrate;
[0048] In some embodiments, the vacuum degree of the vacuum condition is ≤5E -6 torr; when the vacuum is too high, the pressure is smaller and the evaporation effect is worse.
[0049] In some embodiments, the melting and evaporation temperatures are lower than the decomposition temperatures of the inorganic salt and the passivator; wherein the melting and evaporation temperatures are both lower than the decomposition temperatures of the inorganic salt and the passivator, ensuring that the inorganic salt and the passivator will not decompose during the evaporation process.
[0050] In some embodiments, the evaporation method includes thermal evaporation or electron beam evaporation.
[0051] In some embodiments, when the inorganic salt is a combination of PbI2 and CsBr, the passivating agent is PDADI (1,4-phenylenediamine hydroiodide), and preferably the deposition rate ratio of PbI2, CsBr and PDADI is 1:0.1:0.01.
[0052] In some embodiments, the deposited thickness is 600-1000 nm, and illustratively, the deposited thickness is 600 nm, 650 nm, 700 nm, 750 nm, 800 nm, 850 nm, 900 nm, 950 nm, or 1000 nm.
[0053] In some embodiments, the solute of the organic salt solution is any one of FAI (methylguanidine lead iodate), FABr (formamidine bromide), MACl (methylammonium chloride) or MASCN (methylammonium thiocyanate) or a combination of at least two thereof, and the solvent is any one of ethanol, isopropanol or N,N-dimethylformamide or a combination of at least two thereof; wherein the molar concentration of the organic salt solution is 1.4-2.5 mol / L, exemplarily, the molar concentration of the organic salt solution is 1.4 mol / L, 1.5 mol / L, 2 mol / L or 2.5 mol / L.
[0054] In some embodiments, before adding the organic salt solution to the inorganic framework layer, the inorganic framework layer is pre-annealed, and the pre-annealing is carried out in a nitrogen environment. The pre-annealing temperature is 120-200°C (exemplarily, the pre-annealing temperature is 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C), and the pre-annealing time is 0.5-2min. Exemplarily, the pre-annealing time is 0.5min, 0.8min, 1min, 1.2min, 1.5min, 1.7min or 2min.
[0055] In some embodiments, the annealing in step (2) includes primary annealing and secondary annealing;
[0056] The primary annealing is carried out in a nitrogen environment, the primary annealing temperature is 80-120°C (exemplarily, the primary annealing temperature is 80°C, 90°C, 100°C, 110°C or 120°C), the primary annealing time is 1-5min, exemplary, the primary annealing time is 1min, 2min, 3min, 4min or 5min.
[0057] The secondary annealing is carried out in air, the temperature of the secondary annealing is 120-200°C (exemplarily, the temperature of the primary annealing is 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C), and the time of the secondary annealing is 10-30min, and exemplary, the time of the secondary annealing is 10min, 15min, 20min, 25min or 30min.
[0058] When preparing the perovskite absorber layer, Figure 2 As shown, an organic salt solution is added to the surface of the inorganic framework layer, and some vacancies left by the passivator during the formation of the inorganic layer are utilized to allow the organic salt to penetrate and fully react with the inorganic salt, thereby improving the performance of the perovskite solar cell.
[0059] The embodiment of the present application also provides a perovskite absorption layer, which is prepared by the above-mentioned preparation method.
[0060] An embodiment of the present application also provides a perovskite solar cell, comprising the above-mentioned perovskite absorption layer.
[0061] The perovskite solar cell may be a single-layer perovskite solar cell or a stacked perovskite solar cell.
[0062] like Figure 3 As shown, the embodiment of the present application provides a stacked perovskite solar cell, comprising:
[0063] Base layer 020;
[0064] A hole transport layer 030, a perovskite absorption layer 040, an electron transport layer 050 and a first electrode layer 060 are sequentially stacked on a surface of one side of the substrate layer, wherein the perovskite absorption layer is the above-mentioned perovskite absorption layer;
[0065] And a second electrode layer 010 is arranged on the other side surface of the substrate layer.
[0066] In some embodiments, the base layer is a silicon-based solar cell. Before use, the base layer is subjected to UV-zone treatment for 10-20 minutes. Exemplarily, the treatment time is 10 minutes, 12 minutes, 15 minutes, 18 minutes or 20 minutes.
[0067] In some embodiments, the materials of the first electrode layer and the second electrode layer are independently selected from any one or a combination of at least two of indium tin oxide, indium zinc oxide, zinc aluminum oxide, silver nanowires, gold, silver, copper, aluminum or carbon. Based on the deposition thickness of the perovskite absorption layer being 600-1000nm, the first electrode layer and the second electrode layer are independently selected from 100-500nm, and exemplary, the first electrode layer and the second electrode layer are independently selected from 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm or 500nm.
[0068] In some embodiments, the hole transport layer material is a SAM or a metal-containing semiconductor; wherein the SAM can be [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-diphenyl-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid, [4-(3,6-dimethoxy-9H Any one or a combination of at least two of [4-(2,7-dibromo-9,9-dimethylacridine-10(9H)-yl)butyl]phosphonic acid, [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid or (4-(2,7-dibromo-9,9-dimethylacridine-10(9H)-yl)butyl)phosphonic acid; the metal-containing semiconductor may be any one or a combination of at least two of nickel oxide, aluminum copper oxide, iron copper oxide, copper oxide, copper iodide, tungsten oxide, molybdenum oxide, copper sulfide, ferrous sulfide and cuprous thiocyanate. Calculated based on the thickness of the perovskite absorption layer being 600-1000nm, the thickness of the hole transport layer is 5-20nm, and exemplary, the thickness of the hole transport layer is 5nm, 8nm, 10nm, 12nm, 15nm, 18nm or 20nm.
[0069] In some embodiments, the electron transport layer material is selected from tin dioxide, titanium dioxide, [6,6]-phenyl-C71-butyric acid isomethyl ester, C60 or C 60 Any one or a combination of at least two of the derivatives; calculated based on the thickness of the perovskite absorption layer being 600-1000nm, the thickness of the electron transport layer being 25-30nm, and illustratively, the thickness of the electron transport layer being 25nm, 26nm, 27nm, 28nm, 29nm or 30nm.
[0070] In some embodiments, an electron extraction layer is further disposed between the electron transport layer and the first electrode layer.
[0071] In some embodiments, a transmittance-enhancing layer is further provided on the surface of the first electrode layer, and the material of the transmittance-enhancing layer is usually MgF2.
[0072] In some embodiments, the specific preparation method of the tandem perovskite solar cell includes:
[0073] S1, forming a hole transport layer, a perovskite absorption layer, and an electron transport layer in sequence on a surface of one side of the substrate layer to form a stacked structure;
[0074] S2. A first electrode layer is formed on the surface of the stacked structure formed in S1 on a side away from the hole transport layer, and a second electrode layer is formed on the surface of the stacked structure formed in S1 on a side away from the electron transport layer.
[0075] In some embodiments, the specific preparation method of the tandem perovskite solar cell includes:
[0076] S100: Provide a silicon-based cell substrate layer and perform UVO treatment for 10-20 minutes;
[0077] S200: In a PVD (physical vapor deposition) coating device, 20 nm of NiO is deposited on one side of the treated substrate layer, and then a SAM solution is spin-coated, and annealing is performed at 80-120° C. for 10-20 minutes to form a hole transport layer;
[0078] S300: co-evaporating an inorganic salt and a passivating agent on the upper surface of the hole transport layer to form an inorganic framework layer, and then annealing the inorganic framework layer at 80-120° C. for 0.5-2 min in a nitrogen environment; then adding an organic salt solution to the surface of one side of the inorganic framework layer to react, annealing once at 80-120° C. for 1-5 min in a nitrogen environment, and annealing twice at 120-200° C. for 10-30 min in air to form a perovskite absorption layer;
[0079] S400: On the upper surface of the perovskite absorber layer The deposition rate of C 60 forming an electron transport layer;
[0080] S500: vapor-depositing a second electrode layer on a side of the stacked structure formed above that is away from the electron transport layer, and vapor-depositing a first electrode layer on a side that is away from the base layer.
[0081] In some embodiments, the method further includes evaporating an electron extraction layer on the surface of the electron transport layer after forming the electron transport layer and before forming the first and second electrode layers.
[0082] In an optional embodiment, the preparation of the electron extraction layer includes: evaporating 10-20 nm SnO2 on the upper surface of the electron transport layer by ALD (atomic deposition), and then sputtering 50 nm IZO by PVD (physical vapor deposition) to form the electron extraction layer.
[0083] In some embodiments, the method further includes evaporating an anti-reflection layer on the surface of the first electrode layer.
[0084] In an optional embodiment, the preparation of the anti-reflection layer includes: evaporating a MgF2 layer on the surface of the first electrode layer.
[0085] The following specific examples further illustrate the present application, but should not be construed as limiting the present application. Without departing from the spirit and substance of the present application, modifications or replacements made to the methods, steps or conditions of the present application are within the scope of the present application.
[0086] [Example 1]
[0087] This embodiment provides a method for preparing a perovskite absorption layer, comprising:
[0088] A1: When the vacuum degree is lower than 5E -6 In the vacuum equipment of torr, and Co-evaporation of PbI2, CsBr and PDADI on the surface of the hole transport layer at a speed of 600 nm to form an inorganic framework layer;
[0089] A2: In a nitrogen environment, the inorganic framework layer is annealed at 100°C for 1 min;
[0090] An organic salt solution with a concentration of 1.7 mol / L was prepared from FAI, MACl, FABr, MASCN and isopropanol, and spin-coated at a spin-coating rate of 4000 rpm for 60 s. Next, the solution was annealed at 90°C for 3 min in a nitrogen environment, and then transferred to air and annealed at 150°C for 20 min to form a perovskite absorption layer.
[0091] [Example 2]
[0092] This embodiment provides a method for preparing a perovskite absorption layer, comprising:
[0093] A1: When the vacuum degree is lower than 5E-6 In the vacuum equipment of torr, and Co-evaporation of PbI2, CsBr and PDADI on the surface of the hole transport layer at a speed of 600 nm to form an inorganic framework layer;
[0094] A2: In a nitrogen environment, the inorganic framework layer was annealed at 120°C for 0.5 min;
[0095] An organic salt solution with a concentration of 1.4 mol / L was prepared from FAI, MACl, FABr, MASCN and isopropanol, and spin-coated at a spin-coating rate of 4000 rpm for 60 s. Next, the solution was annealed at 120°C for 1 min in a nitrogen environment, and then transferred to air and annealed at 200°C for 10 min to form a perovskite absorption layer.
[0096] [Example 3]
[0097] This embodiment provides a method for preparing a perovskite absorption layer, comprising:
[0098] A1: When the vacuum degree is lower than 5E -6 In the vacuum equipment of torr, and Co-evaporation of PbI2, CsBr and PDADI on the surface of the hole transport layer at a speed of 600 nm to form an inorganic framework layer;
[0099] A2: In a nitrogen environment, the inorganic framework layer is annealed at 80°C for 2 minutes;
[0100] An organic salt solution with a concentration of 2.5 mol / L was prepared from FAI, MACl, FABr, MASCN and isopropanol, and spin-coated at a spin-coating rate of 4000 rpm for 60 s. Next, the solution was annealed at 80°C for 5 min in a nitrogen environment, and then transferred to air and annealed at 120°C for 30 min to form a perovskite absorption layer.
[0101] [Example 4]
[0102] The only difference from Example 1 is that the passivation material PDADI is replaced by PEAI.
[0103] [Example 5]
[0104] The only difference from Example 1 is that the passivation material PDADI is replaced by CF3-PACl.
[0105] [Comparative Example 1]
[0106] This comparative example provides a method for preparing a perovskite absorption layer, comprising:
[0107] A1: When the vacuum degree is lower than 5E -6 In the vacuum equipment of torr, and PbI2 and CsBr were co-evaporated on the surface of the hole transport layer at a speed of 600 nm, and then annealed at 150 ° C for 1 min to form an inorganic framework layer;
[0108] A2: Prepare an organic salt solution with a concentration of 1.7 M composed of FAI, MACl, FABr, MASCN, PDADI and isopropanol, spin coat at a spin coating rate of 4000 rpm for 60 seconds, then anneal at 90°C for 3 minutes, and then transfer to air and anneal at 150°C for 20 minutes to form a perovskite absorption layer.
[0109] [Comparative Example 2]
[0110] The only difference from Example 1 is that the passivating agent PDADI is not added.
[0111]
Application examples
[0112] The perovskite absorption layer prepared in Examples 1-5 and Comparative Examples 1-2 is applied to the preparation of a laminated perovskite cell, including:
[0113] S10: firstly perform UVO treatment on the silicon bottom cell for 15 minutes;
[0114] Then, 20 nm of NiO is deposited in a PVD device to form the first electrode layer;
[0115] S20: In a PVD coating device, 20 nm of NiO is deposited on one surface of the treated substrate layer, and then a SAM solution is spin-coated at 4000 rpm for 10 seconds and annealed at 100° C. for 10 minutes to form a hole transport layer;
[0116] S30: forming a perovskite absorption layer by using the preparation methods of the perovskite absorption layer provided in Examples 1-5 and Comparative Examples 1-2 respectively;
[0117] S40: When the vacuum degree is lower than 5E -6 Torr conditions, Evaporating C60 to deposit it on the upper surface of the perovskite absorption layer to form an electron transport layer with a thickness of 30 nm;
[0118] S50: On the upper surface of the electron transport layer, 15 nm of SnO2 is deposited by ALD and 50 nm of IZO is sputtered by PVD to form an electron extraction layer;
[0119] S60: After forming the electron extraction layer, 400 nm of Ag is evaporated on the side of the stacked structure away from the electron extraction layer to form a second electrode layer, and 400 nm of Ag is evaporated on the side away from the base layer to form a first electrode layer;
[0120] S70: vapor-deposit a 90nm thick anti-reflection layer of MgF2 on the surface of the first electrode layer to form a laminated perovskite solar cell.
[0121] The following is a performance test of the stacked perovskite solar cells finally formed by Examples 1-5 of the present application and Comparative Examples 1-2, so as to obtain the short-circuit current density Jsc, open-circuit voltage Voc, fill factor FF, and photoelectric conversion efficiency PCE of the corresponding battery devices. The test results are shown in Table 1.
[0122] Table 1 Performance test results of perovskite solar cells
[0123] Battery <![CDATA[Jsc(mA / cm 2 )]]> Voc(V) FF(%) PCE(%) Example 1 19.82 1.870 78.06 28.93 Example 2 19.74 1.857 77.52 28.42 Example 3 19.72 1.854 77.66 28.39 Example 4 19.78 1.866 78.59 29.01 Example 5 19.77 1.876 77.35 28.69 Comparative Example 1 19.73 1.839 76.14 27.63 Comparative Example 2 19.62 1.847 74.66 27.06
[0124] It can be seen from Examples 1-5 that within the scope defined in the embodiments of the present application, the obtained stacked perovskite cells all have good performance; from the comparison between Example 1 and Comparative Example 1, it can be seen that evaporating the passivator together with the inorganic salt can make the low-doped passivator evenly distributed in the inorganic layer, and the passivator can leave some vacancies, so that the excess organic salt penetrates and reacts with the inorganic salt, thereby improving the battery performance, while if the passivator is placed in the organic salt, the amount of organic salt penetration is small, that is, the amount of organic salt participating in the reaction is small, which is not conducive to the improvement of battery performance; from the comparison between Example 1 and Comparative Example 2, it can be seen that if the passivator is not added, there are not enough vacancies in the inorganic layer for the organic salt to penetrate and participate in the reaction, which is not conducive to the improvement of battery performance.
[0125] An embodiment of the present application provides a photovoltaic module (not shown), including at least one battery string, the battery string includes at least two perovskite solar cells of any embodiment, adjacent perovskite solar cells can be connected together by string welding, wherein the perovskite solar cell can be a single-layer perovskite solar cell or a stacked perovskite solar cell, preferably a stacked perovskite solar cell.
[0126] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in the above embodiment. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid and then connected to the mains network to realize solar power supply.
[0127] It should be noted that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.
[0128] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0129] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when describing a specific feature, structure or characteristic in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.
[0130] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0131] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for preparing a perovskite absorption layer, characterized in that: The preparation method comprises: (1) forming an inorganic framework layer by co-evaporating an inorganic salt and a passivating agent on a surface of one side of the substrate; (2) Adding an organic salt solution to the surface of the inorganic framework layer away from the substrate, reacting, and annealing to form a perovskite absorption layer.
2. The method for preparing a perovskite absorption layer according to claim 1, characterized in that: The inorganic salt in step (1) comprises any one or a combination of at least two of PbI2, CsBr, PbBr or CsI; The passivating agent in step (1) includes any one of PEAI, CF3-PACl, PDADI, OAI or TEACL, or a combination of at least two thereof; The co-evaporation ratio of the inorganic salt and the passivating agent in step (1) is [1-1.5]:[0.01-0.1].
3. The method for preparing a perovskite absorption layer according to claim 2, characterized in that: When the inorganic salt in step (1) is a combination of PbI2 and CsBr, and the passivating agent is PDADI, the co-evaporation ratio of PbI2, CsBr and PDADI is 1:[0.1-0.3]:[0.01-0.05].
4. The method for preparing a perovskite absorption layer according to claim 1, characterized in that: The co-evaporation in step (1) comprises: melting the inorganic salt and the passivating agent separately under vacuum conditions, evaporating the molten substances and depositing them on the substrate; Wherein, the preparation method meets at least one of the following characteristics: The vacuum degree of the vacuum condition is ≤5E -6 torr; The melting and evaporation temperature is lower than the decomposition temperature of the organic compound and the lithium-containing metal compound; The evaporation method includes heating evaporation or electron beam evaporation; The thickness of the deposition is 600-1000 nm.
5. The method for preparing a perovskite absorption layer according to claim 1, characterized in that: The solute of the organic salt solution in step (2) is any one of FAI, FABr, MACl or MASCN or a combination of at least two thereof, and the solvent is any one of ethanol, isopropanol or N,N-dimethylformamide or a combination of at least two thereof; The molar concentration of the organic salt solution in step (2) is 1.4-2.5 mol / L.
6. The method for preparing a perovskite absorption layer according to claim 1, characterized in that: Also includes: In step (2), before adding the organic salt solution to the inorganic framework layer, the inorganic framework layer is pre-annealed. The pre-annealing is performed in a nitrogen environment. The pre-annealing temperature is 120-200° C. and the pre-annealing time is 0.5-2 min.
7. The method for preparing a perovskite absorption layer according to claim 1, characterized in that: The annealing in step (2) includes primary annealing and secondary annealing; The primary annealing is performed in a nitrogen environment at a temperature of 80-120° C. and a time of 1-5 min. The secondary annealing is carried out in air, the temperature of the secondary annealing is 120-200° C., and the time of the secondary annealing is 10-30 minutes.
8. A perovskite absorption layer, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 7.
9. A perovskite solar cell, characterized in that: The perovskite solar cell comprises the perovskite absorption layer according to claim 8.
10. A photovoltaic module, characterized in that: The photovoltaic module comprises a plurality of perovskite solar cells connected in series and / or in parallel; wherein at least one perovskite solar cell is the stacked perovskite solar cell according to claim 9.
11. A photovoltaic system, characterized in that: The photovoltaic system comprises the photovoltaic module according to claim 10.
Citation Information
Cited By
Perovskite solar cell and preparation method thereof
CN120035355A