Self-crosslinkable polymer and composition for forming resist underlayer film

By forming a photoresist underlayer film with a self-crosslinking polymer having MOM groups on nitrogen atoms and phenolic varnish resin, the problems of crosslinking agents and catalysts in the prior art are solved, and the formation of a high-quality thermosetting film at low temperature is achieved, reducing costs and improving etching resistance and coatability.

CN118974135APending Publication Date: 2024-11-15NISSAN CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031323.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the composition for forming the lower layer film of the resist requires a crosslinking agent and a crosslinking catalyst when forming a thermosetting film, which leads to high cost and may reduce etch resistance, increase sublimation content and changes in optical constants, and result in poor coatability.

Method used

A polymer resin material with MOM groups on nitrogen atoms is used to form a thermosetting film at low or high temperature through self-crosslinking polymers, avoiding the use of crosslinking agents and crosslinking catalysts, and combining phenolic varnish resin and solvent to form a photoresist lower layer film.

Benefits of technology

It forms a high-quality thermosetting film in an atmospheric or nitrogen atmosphere, reducing material costs, improving etch resistance, embedding and planarization, and improving the coating properties of substrates with high and low differences.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064172700000021
    Figure BDA0005064172700000021
  • Figure BDA0005064172700000033
    Figure BDA0005064172700000033
  • Figure BDA0005064172700000034
    Figure BDA0005064172700000034
Patent Text Reader

Abstract

Provided is a polymer resin material capable of forming a heat-cured film at a lower temperature even without a crosslinking agent or a crosslinking catalyst. A self-crosslinkable polymer containing a unit structure (A) having an aromatic ring and a unit structure (B) that is an organic group having a carbon atom attached thereto, at least one unit structure (A) is (i) a unit structure in which at least two aromatic rings are linked to an-NR-bond, (ii) a unit structure containing a heterocyclic structure having at least one-NR-bond as a ring constituent element, or (iii) a unit structure containing an aromatic ring having at least one-NR2 substituent, and R is a hydrogen atom or an alkoxymethyl group; at least a portion of R in the whole polymer is an alkoxymethyl group, the so-called linking carbon atom is a carbon atom in a unit structure B that forms a covalent bond with an aromatic ring in a unit structure A, and is a carbon atom that does not constitute an aromatic ring.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer resin suitable for photolithography in semiconductor substrate processing, a composition for forming an anti-etching underlayer film mixed with the polymer resin, a resist underlayer film obtained from the resist underlayer film forming composition, a method for forming a resist pattern using the resist underlayer film forming composition, and a method for manufacturing a semiconductor device using the composition. Background Art

[0002] In recent years, in the photolithography process for manufacturing semiconductor devices, there has been a demand for further improvement in the quality of semiconductor process materials including resist underlayer films.

[0003] For example, in the resist lower film forming composition, in order to form such a thermosetting film, in addition to the polymer resin that becomes the main component, a cross-linking compound (cross-linking agent) and a catalyst (cross-linking catalyst) for promoting the cross-linking reaction are also mixed, but if there is no such cross-linking agent or cross-linking catalyst, then generally, as long as it does not become an ultra-high temperature, a thermosetting film cannot be formed. However, if there is a polymer resin material that can form a thermosetting film at a lower temperature even without a cross-linking agent or a cross-linking catalyst, the operation can be made simpler and it is also advantageous in terms of cost. In addition, by including a cross-linking agent or a cross-linking catalyst, a reduction in etching resistance, an increase in sublimation components, a change in optical constants, a deterioration in planarization and embedding properties, etc. sometimes occur, and as a material design, it is strongly desired to form a resist lower film without including them.

[0004] In patent documents 1 and 2, polymers containing substituents having carbon-carbon triple bonds such as propargyl groups on nitrogen atoms are disclosed as polymers mixed in organic film-forming compositions. It is generally believed that such carbon-carbon triple bonds are used as intermolecular crosslinking groups, and can also form cured films in inert gases, and can show high etching resistance and good embedding and planarization properties. However, in these patent documents, polymers containing carbon-carbon triple bonds on nitrogen atoms are characterized, and polymers with self-crosslinking properties other than these are not disclosed. In addition, there is no mention of sublimation components and coating properties on high-low substrates.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-41059

[0008] Patent Document 2: Japanese Patent Application Publication No. 2019-44022 Summary of the invention

[0009] Problems to be solved by the invention

[0010] Therefore, the problem to be solved by the invention of this application is to provide a polymer resin material having an alkoxymethyl group such as a MOM group (methoxymethyl) on a nitrogen atom, which can form a thermosetting film by low-temperature sintering or high-temperature sintering in an air atmosphere or a nitrogen atmosphere even without containing a cross-linking agent or a cross-linking catalyst, and a composition for forming an anti-etching agent underlayer film mixed with the polymer resin, which is advantageous in terms of cost because the components of the constituent materials can be reduced.

[0011] In addition, it is more preferable to provide a polymer resin material that has high etching resistance, good embedding properties, and planarization properties, reduces the sublimation components generated during firing, and shows good coating properties on uneven substrates, and a composition for forming an anti-etching agent underlayer film mixed with the polymer resin.

[0012] Means for solving problems

[0013] The present invention includes the following aspects. [1]

[0015] A self-crosslinking polymer comprising:

[0016] (A) one or more unit structures A having an aromatic ring; and

[0017] (B) one or more unit structures B as organic groups having one or more connecting carbon atoms,

[0018] At least one of the unit structures A is:

[0019] (i) a unit structure comprising at least two aromatic rings connected by at least one -NR- bond,

[0020] (ii) a unit structure comprising a heterocyclic ring having at least one -NR- bond as a ring constituent, and when the heterocyclic ring is not an aromatic heterocyclic ring, the heterocyclic ring forms a condensed ring with a first aromatic ring, and / or the heterocyclic ring is substituted with a substituent comprising a second aromatic ring, or

[0021] (iii) a unit structure comprising at least one aromatic ring having at least one -NR2 substituent,

[0022] The above R is a hydrogen atom or an alkoxymethyl group, and at least a part of the R groups in all polymers are alkoxymethyl groups,

[0023] The connecting carbon atom is a carbon atom in the unit structure B that forms a covalent bond with the aromatic ring in the unit structure A and is a carbon atom that does not constitute the aromatic ring. [2]

[0025] The self-crosslinking polymer according to claim 1, which is a novolac resin. [3]

[0027] The self-crosslinking polymer according to [1] or [2], wherein the unit structure A is selected from the following unit structures (I-1) to (I-5) and positional isomers thereof,

[0028]

[0029] The above (I-1) to (I-5) may further optionally have a substituent.

[0030] In the above (I-1) to (I-5), R has the same meaning as in [1],

[0031] In the above (I-1), each Ar is the same or different and represents an aromatic ring which may have a substituent.

[0032] In the above (I-2) to (I-5),

[0033] represents an aromatic ring part in a fused ring which may have a substituent, and each of them may be the same as or different from each other,

[0034] In the above (I-4), X represents CR 1 R 2 , O, S or NR'; R' is the same as the definition of R in claim 1, and may be the same as or different from R in the above chemical formula (I-4); R 1 and R 2 are the same as or different from each other and are aromatic ring residues or aliphatic hydrocarbon groups having 1 to 3 carbon atoms,

[0035] In (I-5) above represents a heterocyclic moiety in a fused ring compound which may have a substituent,

[0036] Y is a substituent including an aromatic ring, and may be a substituent of any of the above-mentioned aromatic ring part and the above-mentioned heterocyclic part. [4]

[0038] The self-crosslinking polymer according to any one of [1] to [3] above, wherein the unit structure B is a unit structure including a structure represented by the following (II), (III) or (IV).

[0039]

[0040] (In formula (II), R and R' each independently represent a hydrogen atom, an aromatic ring residue having 6 to 30 carbon atoms which may have a substituent, a heterocyclic residue having 3 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a substituent.)

[0041]

[0042] [In formula (III),

[0043] Z is a monocyclic, bicyclic, tricyclic or tetracyclic condensed ring having 4 to 25 carbon atoms and optionally having a substituent, wherein the monocyclic ring is a non-aromatic monocyclic ring; at least one of the monocyclic rings constituting the bicyclic, tricyclic and tetracyclic rings is a non-aromatic monocyclic ring, and the remaining monocyclic rings may be either aromatic or non-aromatic. The monocyclic, bicyclic, tricyclic or tetracyclic condensed ring may further form a condensed ring with one or more aromatic rings to form a condensed ring of at least five rings,

[0044] X and Y are the same or different, indicating -CR 31 R 32 -Base, R 31 and R 32 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms,

[0045] x, y each represent the number of X, Y, and each independently represent 0 or 1,

[0046] *-X x is bonded to any carbon atom (referred to as "carbon atom 1") of the non-aromatic monocyclic ring constituting Z (when x=1), or extends from carbon atom 1 (when x=0),

[0047] Y y -* is bonded to any carbon atom (referred to as "carbon atom 2") of the above non-aromatic monocyclic ring constituting Z (when y=1), or extends from carbon atom 2 (when y=0),

[0048] The carbon atom 1 and the carbon atom 2 may be the same or different, and in different cases, may belong to the same non-aromatic monocyclic ring or different non-aromatic monocyclic rings.

[0049] * indicates a bonding bond. ]

[0050] -J 1 -Z 0 -J 2 - (IV)

[0051] [In formula (IV), Z 0represents an aromatic ring residue or an aliphatic ring residue having 6 to 30 carbon atoms which may have a substituent, or an organic group in which two aromatic ring residues or aliphatic ring residues are linked by a single bond, J 1 and J 2 Each independently represents a divalent organic group which is directly bonded or may have a substituent.] [5]

[0053] According to the resist underlayer film forming composition described in the above [4], the formula (III) is the following formula (III-1).

[0054]

[0055] [In formula (III-1),

[0056] Z is a 4- to 17-membered monocyclic, bicyclic, tricyclic or tetracyclic organic group which may have a substituent, wherein the monocyclic ring is a non-aromatic monocyclic ring; at least one of the monocyclic rings constituting the bicyclic, tricyclic and tetracyclic rings is a non-aromatic monocyclic ring, and the remaining monocyclic rings may be either aromatic or non-aromatic.

[0057] One or more aromatic rings may be further fused or fused with the above-mentioned monocyclic, bicyclic, tricyclic and tetracyclic organic groups to form pentacyclic or more rings.

[0058] C and C' each represent a carbon atom in the group of atoms constituting the cyclic portion of any non-aromatic monocyclic ring of the above Z, and the non-aromatic monocyclic rings to which C and C' belong may be the same or different,

[0059] n is the number of carbon atoms C', which is an integer from 0 to 2.

[0060] p, q, p', q' represent the number of bonding bonds, and each independently represents 0 or 1.

[0061] When n is 0, p and q are 1,

[0062] When n is 1 or 2, at least one of p and q is 1, and at least one of p' and q' of each C' is 1,

[0063] When n is 2, the non-aromatic monocyclic rings to which the two C's belong may be the same or different. If they are the same, the two C's may be directly bonded or not.

[0064] X, Y, X', Y' are the same or different, indicating -CR 1 R 2 -Base, R 1 and R 2are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms. When n is 2, the two X's may be the same or different, and the two Y's may be the same or different.

[0065] x, y, x', y' each represent the number of X, Y, X', Y', and each independently represent 0 or 1.] [6]

[0067] The self-crosslinking polymer according to any one of [1] to [5] above, wherein the terminal group of the self-crosslinking polymer is an aromatic ring residue having 6 to 30 carbon atoms which may have a substituent, an unsaturated hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, a hydroxyl group or a hydrogen atom. [7]

[0069] A resist underlayer film-forming composition comprising a thermal acid generator, the self-crosslinking polymer according to any one of [1] to [6] above, and a solvent. [8]

[0071] The resist underlayer film forming composition according to the above [7], further comprising a cross-linking agent. [9]

[0073] In the resist underlayer film forming composition described in the above [8], the crosslinking agent is an aminoplast crosslinking agent or a phenoplast crosslinking agent.

[10]

[0075] In the resist underlayer film forming composition described in the above [9], the aminoplast crosslinking agent is highly alkylated, alkoxylated, or alkoxyalkylated melamine, benzoguanamine, glycoluril, urea, or a polymer thereof.

[11]

[0077] In the resist underlayer film forming composition described in the above [9], the phenolic plastic crosslinking agent is a highly alkylated, alkoxylated, or alkoxyalkylated aromatic compound, or a polymer thereof.

[12]

[0079] In the resist underlayer film forming composition according to any one of [7] to

[11] above, the solvent is a compound having an alcoholic hydroxyl group or a compound having a group capable of forming an alcoholic hydroxyl group.

[13]

[0081] According to the resist underlayer film forming composition described in the above

[12] , the compound having an alcoholic hydroxyl group or the compound having a group capable of forming an alcoholic hydroxyl group is a propylene glycol-based solvent, an oxyisobutyrate-based solvent, or a butanediol-based solvent.

[14]

[0083] According to the resist underlayer film forming composition described in the above

[12] , the compound having an alcoholic hydroxyl group or the compound having a group capable of forming an alcoholic hydroxyl group is propylene glycol monomethyl ether, cyclohexanone, propylene glycol monomethyl ether acetate, ethyl lactate, or methyl 2-hydroxy-2-methylpropionate.

[15]

[0085] The resist underlayer film forming composition according to any one of [7] to

[14] , further comprising a surfactant.

[16]

[0087] A resist underlayer film which is a fired product of a coating film formed from the resist underlayer film-forming composition according to any one of [7] to

[15] above on a semiconductor substrate.

[17]

[0089] A method for forming a resist pattern for producing a semiconductor, comprising the step of applying the resist underlayer film-forming composition according to any one of [7] to

[15] above onto a semiconductor substrate and firing the composition to form a resist underlayer film.

[18]

[0091] A method for manufacturing a semiconductor device comprises the following steps:

[0092] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition described in any one of [7] to

[15] above;

[0093] forming a resist film on the resist underlayer film;

[0094] A process of forming a resist pattern by irradiation with light or electron beams and development;

[0095] a step of etching the resist underlayer film using the formed resist pattern; and

[0096] A step of processing a semiconductor substrate using a patterned resist underlayer film.

[19]

[0098] A method for manufacturing a semiconductor device comprises the following steps:

[0099] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition described in any one of [7] to

[15] above;

[0100] forming a hard mask on the resist underlayer film;

[0101] A step of further forming a resist film on the hard mask;

[0102] A process of forming a resist pattern by irradiation with light or electron beams and development;

[0103] A process of etching the hard mask using the formed resist pattern;

[0104] A step of etching the resist underlayer film using the patterned hard mask; and

[0105] A step of processing a semiconductor substrate using a patterned resist underlayer film.

[20]

[0107] A method for manufacturing a semiconductor device comprises the following steps:

[0108] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition described in any one of [7] to

[15] above;

[0109] forming a hard mask on the resist underlayer film;

[0110] A step of further forming a resist film on the hard mask;

[0111] A process of forming a resist pattern by irradiation with light or electron beams and development;

[0112] A process of etching the hard mask using the formed resist pattern;

[0113] A step of etching the resist underlayer film using the patterned hard mask;

[0114] A process of removing the hard mask; and

[0115] A step of processing a semiconductor substrate using a patterned resist underlayer film. [twenty one]

[0117] A method for manufacturing a semiconductor device comprises the following steps:

[0118] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition described in any one of [7] to

[15] above;

[0119] forming a hard mask on the resist underlayer film;

[0120] A step of further forming a resist film on the hard mask;

[0121] A process of forming a resist pattern by irradiation with light or electron beams and development;

[0122] A process of etching the hard mask using the formed resist pattern;

[0123] A step of etching the resist underlayer film using the patterned hard mask;

[0124] A process of removing the hard mask; and

[0125] A step of forming a vapor-deposited film (spacer) on the resist underlayer film after the hard mask is removed;

[0126] A process of processing the vapor-deposited film (spacer) by etching;

[0127] A step of removing the patterned resist underlayer film to leave the patterned vapor-deposited film (spacer); and

[0128] A step of processing a semiconductor substrate via a patterned vapor-deposited film (spacer). [twenty two]

[0130] According to the manufacturing method described in any one of

[19] to

[21] above, the hard mask is formed by coating or vapor deposition of an inorganic material. [twenty three]

[0132] According to the production method described in any one of

[18] to

[21] , the resist film is patterned by nanoimprinting or self-assembled film. [twenty four]

[0134] According to the method for manufacturing a semiconductor device described in

[20] or

[21] above, the hard mask is removed by either etching or an alkaline chemical solution.

[0135] Effects of the Invention

[0136] The self-crosslinking polymer as one embodiment of the present invention can form a thermosetting film by low-temperature or high-temperature calcination in air or nitrogen atmosphere even without containing a crosslinking agent or a crosslinking catalyst, and can reduce the components of the constituent materials, which is also cost-effective.

[0137] Furthermore, in a more preferred embodiment, a polymer resin material mixed with a self-crosslinking polymer as one embodiment of the present invention and a composition for forming an anti-etching agent underlayer film mixed with the polymer resin have, in addition to high etching resistance, good embedding property and flattening property, reduced sublimation components produced during firing, and exhibit good coating properties on height difference substrates. DETAILED DESCRIPTION

[0138] [1. Definition of terms]

[0139] In this specification, the definitions of main terms related to the novolac resin as one embodiment of the present invention are described below. Unless otherwise specified, the definitions of the following terms apply to the novolac resin.

[0140] (1-1) “Novolac resin”

[0141] The term "novolak resin" is used in a broad sense to include not only phenol / formaldehyde resins (so-called novolac-type phenolic resins) and aniline / formaldehyde resins (so-called novolac-type aniline resins) in a narrow sense, but also a polymer formed by covalent bond formation (substitution reaction, addition reaction, condensation reaction, or addition condensation reaction, etc.) between an organic compound having a functional group capable of covalently bonding to an aromatic ring [for example, an aldehyde group, a ketone group, an acetal group, a ketal group, a hydroxyl group or an alkoxy group bonded to a secondary or tertiary carbon, a hydroxyl group, an alkoxy group or a halide group bonded to an α-position carbon atom (benzyl carbon atom, etc.) of an alkylaryl group; a carbon-carbon unsaturated bond of divinylbenzene, dicyclopentadiene, etc.] and an aromatic ring in a compound having an aromatic ring (preferably having a substituent containing a heteroatom such as an oxygen atom, a nitrogen atom, a sulfur atom, etc. on the aromatic ring) in the presence of an acid catalyst or under reaction conditions equivalent thereto.

[0142] Therefore, the novolac resin referred to in the present application specification is a polymer formed by connecting a plurality of compounds having aromatic rings, by forming a covalent bond between an organic compound containing a carbon atom derived from the above-mentioned functional group (sometimes referred to as a "connecting carbon atom") and an aromatic ring in a compound having an aromatic ring via a connecting carbon atom.

[0143] In this specification, the terms unit structure A, unit structure B, and unit structure C are used as unit structures constituting the "phenolic varnish resin". Unit structure A is a unit structure derived from a compound having an aromatic ring. Unit structure B is a unit structure derived from a compound having a functional group capable of covalently bonding to the aromatic ring of unit structure A. Unit structure C is a unit structure having an equivalent bonding method to composite unit structure AB, and is a unit structure derived from a compound having an aromatic ring and having a functional group capable of covalently bonding to the aromatic ring of unit structure A. Since the bonding method is the same, unit structure C can be replaced by composite unit structure AB.

[0144] (1-2) “Residue”

[0145] The so-called "residue" refers to an organic group in which a hydrogen atom bonded to a carbon atom or a heteroatom (nitrogen atom, oxygen atom, sulfur atom, etc.) is replaced with a bond, and can be a monovalent group or a polyvalent group. For example, if one hydrogen atom is replaced with one bond, it becomes a monovalent organic group, and if two hydrogen atoms are replaced with bonds, it becomes a divalent organic group.

[0146] (1-3) “Aromatic ring” (aromatic group, aryl group, arylene group)

[0147] The term "aromatic ring" is a concept including aromatic hydrocarbon rings, aromatic heterocycles, and residues thereof [sometimes referred to as "aromatic groups", "aryl groups" (in the case of monovalent groups) or "arylene groups" (in the case of divalent groups)], and includes not only monocyclic types (aromatic monocyclic rings) but also polycyclic types (aromatic polycyclic rings). In the case of polycyclic types, at least one monocyclic ring is an aromatic monocyclic ring, and the remaining monocyclic rings forming a condensed ring with the aromatic monocyclic ring may be monocyclic heterocyclic rings (heteromonocyclic rings) or monocyclic alicyclic hydrocarbons (alicyclic monocyclic rings).

[0148] Examples of the aromatic ring include benzene, indene, naphthalene, azulene, styrene, toluene, xylene, mesitylene, cumene, anthracene, phenanthrene, benzo[9,10]phenanthrene, benzanthracene, pyrene, Fluorene, biphenyl, coronene, perylene, fluoranthene, benzo[k]fluoranthene, benzo[b]fluoranthene, benzo[ghi]perylene, coronene, dibenzo[g,p] Aromatic hydrocarbon rings such as acenaphthene, dihydroacenaphthene, tetracene, pentacene, cyclooctatetraene, more typically aromatic hydrocarbon rings such as benzene, naphthalene, anthracene, pyrene, furan, pyran, pyridine, pyrimidine, pyrazine, thiophene, pyrrole, N-alkylpyrrole, N-arylpyrrole, imidazole, pyridine, pyrimidine, pyrazine, triazine, thiazole, indole, phenylindole, bisindolefluorene, bisindolebenzofluorene, bisindoledibenzofluorene, purine, quinoline, isoquinoline, chromene, thianthrene, phenothiazine, phenanthrene, Aromatic heterocyclic rings such as oxazine, xanthene, acridine, phenazine, carbazole, and indolocarbazole, more typically furan, thiophene, pyrrole, indole, phenylindole, bisindolefluorene, phenothiazine, carbazole, and indolocarbazole, but are not limited thereto.

[0149] The aromatic ring (e.g., benzene ring, naphthalene ring, etc.) may optionally have a substituent, and examples of such a substituent include a halogen atom, a saturated or unsaturated straight chain, branched chain or cyclic hydrocarbon group (-R) (which may be interrupted once or more by an oxygen atom in the middle of the hydrocarbon chain. It includes alkyl, alkenyl, alkynyl, propargyl, etc.), an alkoxy or aryloxy group (-OR, where R represents the above hydrocarbon group -R), an alkylamino group [-NHR or -NR2 (the two Rs may be the same or different, where R represents the above hydrocarbon group -R, it includes alkyl, alkenyl, alkynyl, propargyl, etc. which may be interrupted once or more by an oxygen atom in the middle of the hydrocarbon chain. ], hydroxyl, amino (-NH2), carboxyl, cyano, nitro, ester group (-CO2R or -OCOR, where R represents the above hydrocarbon group -R), amide group (-NHCOR, -CONHR, -NRCOR (the two Rs may be the same or different) or -CONR2 (the two Rs may be the same or different), where R represents the above hydrocarbon group -R), sulfonyl group-containing group (-SO2R, where R represents the above hydrocarbon group -R or hydroxyl -OH), thiol group (-SH), thioether group (-SR, where R represents the above hydrocarbon group -R); organic group containing ether bond [R 11 -OR 11 (R 11 Each independently represents an alkyl group having 1 to 6 carbon atoms such as methyl and ethyl, an aryl group such as phenyl, naphthyl, o-aminobenzoyl, and pyrenyl. ) is a residue of an ether compound represented by; for example, an organic group containing an ether bond such as methoxy, ethoxy, and phenoxy], and a substituent such as an aryl group.

[0150] Furthermore, organic groups having one or more aromatic rings (benzene, naphthalene, anthracene, pyrene, etc.) and one or more aliphatic rings or heterocyclic condensed rings are also included. Further, examples of the aliphatic rings here include cyclobutane, cyclobutene, cyclopentane, cyclopentene, cyclohexane, cyclohexene, methylcyclohexane, methylcyclohexene, cycloheptane, and cycloheptene, and examples of the heterocyclic rings include furan, thiophene, pyrrole, imidazole, pyran, pyridine, pyrimidine, pyrazine, pyrrolidine, piperidine, piperazine, and morpholine.

[0151] It may be an organic group having a structure in which two or more aromatic rings are connected via a divalent connecting group such as an alkylene group.

[0152] (1-4) “Heterocyclic”

[0153] "Heterocycle" includes both aliphatic heterocycles and aromatic heterocycles, and is a concept that includes not only monocyclic (heteromonocyclic) but also polycyclic (heteropolycyclic). In the case of a polycyclic, at least one monocyclic ring is a heteromonocyclic ring, and the remaining monocyclic rings may be aromatic hydrocarbon monocyclic rings or alicyclic monocyclic rings. As aromatic heterocycles, the examples in (1-3) above may be referred to. As with the aromatic ring in (1-3) above, it may have a substituent.

[0154] (1-5) “Non-aromatic ring” (aliphatic ring)

[0155] The so-called "non-aromatic monocyclic ring" is a monocyclic hydrocarbon that is not aromatic, typically a monocyclic ring of an alicyclic compound. It can be called an aliphatic monocyclic ring (it can include an aliphatic heteromonocyclic ring, and it can include an unsaturated bond as long as it is not an aromatic compound). Like the aromatic ring in (1-3) above, it can have a substituent.

[0156] Examples of the non-aromatic monocyclic ring (aliphatic ring, aliphatic monocyclic ring) include cyclopropane, cyclobutane, cyclobutene, cyclopentane, cyclopentene, cyclohexane, methylcyclohexane, cyclohexene, methylcyclohexene, cycloheptane, and cycloheptene.

[0157] The so-called "non-aromatic polycyclic" is a polycyclic hydrocarbon that is not aromatic, typically a polycyclic alicyclic compound. It can be called an aliphatic polycyclic [which may include an aliphatic heteropolycyclic (at least one of the monocyclics constituting the polycyclic is an aliphatic heterocyclic), and may include an unsaturated bond as long as it is not an aromatic compound]. It includes a non-aromatic bicyclic, a non-aromatic tricyclic, and a non-aromatic tetracyclic.

[0158] The so-called "non-aromatic bicyclic ring" is a condensed ring composed of two monocyclic hydrocarbons that are not aromatic, and is typically a condensed ring of two alicyclic compounds. In this specification, it is sometimes referred to as an aliphatic bicyclic ring (which may include an aliphatic heterobicyclic ring and may include an unsaturated bond as long as it is not an aromatic compound). Examples of the non-aromatic bicyclic ring include dicyclopentane, dicyclooctane, and dicycloheptene.

[0159] The so-called "non-aromatic tricyclic ring" is a condensed ring composed of three monocyclic hydrocarbons that are not aromatic, and is typically a condensed ring of three alicyclic compounds (each of which may be a heterocyclic ring and may contain an unsaturated bond as long as it is not an aromatic compound). Examples of the non-aromatic tricyclic ring include tricyclooctane, tricyclononane, and tricyclodecane.

[0160] The so-called "non-aromatic tetracyclic ring" is a condensed ring composed of four monocyclic hydrocarbons that are not aromatic, and is typically a condensed ring of four alicyclic compounds (each of which may be a heterocyclic ring and may contain an unsaturated bond as long as it is not an aromatic compound). Examples of the non-aromatic tetracyclic ring include hexahydropyrene and the like.

[0161] (1-6)

[0162] The "carbon atoms constituting the ring (part)" refers to the carbon atoms constituting the hydrocarbon ring (which may be any of an aromatic ring, an aliphatic ring, and a heterocyclic ring) in a state without a substituent.

[0163] (1-7)

[0164] The term "hydrocarbon group" refers to a group formed by removing one or more hydrogen atoms from a hydrocarbon, and such hydrocarbons include saturated or unsaturated aliphatic hydrocarbons, saturated or unsaturated alicyclic hydrocarbons, and aromatic hydrocarbons.

[0165] (1-8)

[0166] In the chemical structural formula representing the unit structure of the phenolic varnish resin in the present application specification, a bond (indicated by *) is sometimes recorded for convenience, but such a bond can adopt any bonding position in the unit structure that can be bonded unless otherwise specified, and there is no limitation on the bonding position in the unit structure.

[0167] [2. Self-crosslinking polymer [1]]

[0168] (2-1)

[0169] A self-crosslinking polymer as one embodiment of the present invention includes:

[0170] (A) one or more unit structures A having an aromatic ring; and

[0171] (B) One or more unit structures B as organic groups having one or more connecting carbon atoms.

[0172] Furthermore, at least one of the unit structures A is:

[0173] (i) a unit structure comprising at least two aromatic rings connected by at least one -NR- bond,

[0174] (ii) a unit structure comprising a heterocyclic ring having at least one -NR- bond as a ring constituent, and when the heterocyclic ring is not an aromatic heterocyclic ring, the heterocyclic ring forms a condensed ring with a first aromatic ring, and / or the heterocyclic ring is substituted with a substituent comprising a second aromatic ring, or

[0175] (iii) A unit structure comprising at least one aromatic ring having at least one -NR2 substituent.

[0176] Here, the above R is a hydrogen atom or an alkoxymethyl group, and at least a part of the R groups in the entire polymer are alkoxymethyl groups, which can impart self-crosslinking properties. The alkoxy group in the alkoxymethyl group is preferably a hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrocarbon group having 1 to 3 carbon atoms, and most preferably a methoxymethyl group.

[0177] At least a part of R in all polymers is an alkoxymethyl group, and the proportion of the alkoxymethyl group is adjusted from the viewpoint of imparting desired self-crosslinking properties.

[0178] One connecting carbon atom in unit structure B [see (1-1) above] (i) may form a covalent bond with each of the aromatic rings of two unit structures A, or (ii) may form a covalent bond with an aromatic ring of one unit structure A and a polymer terminal group. In the latter case (ii), unit structure B contains at least 2, more preferably 2 connecting carbon atoms.

[0179] The connecting carbon atom is a carbon atom in unit structure B that forms a covalent bond between unit structure A and unit structure B by forming a covalent bond with the aromatic ring in unit structure A, and is a carbon atom that does not constitute an aromatic ring.

[0180] It should be noted that the covalent bonding to the aromatic ring of the unit structure A also includes the covalent bonding to the aromatic ring of the unit structure C equivalent to the composite unit structure AB in which one unit structure A and one unit structure B are combined, as described later [(2-4-3-3), (2-4-5-3) and (2-4-6)].

[0181] (2-2)

[0182] The self-crosslinking polymer as one embodiment of the present invention is preferably a novolac resin [see (1-1) above].

[0183] Therefore, the novolac resin referred to in the present application specification is a polymer formed by connecting multiple compounds having aromatic rings by forming a covalent bond between an organic compound (unit structure B) containing a carbon atom derived from a functional group (corresponding to a "connecting carbon atom") and an aromatic ring (unit structure A) in a compound having an aromatic ring.

[0184] (2-3; unit structure A)

[0185] (2-3-1)

[0186] The unit structure A of the self-crosslinking polymer as one embodiment of the present invention is one or more unit structures having an aromatic ring, and

[0187] At least one of the unit structures A is:

[0188] (i) a unit structure comprising at least two aromatic rings connected by at least one -NR- bond,

[0189] (ii) a unit structure comprising a heterocyclic ring having at least one -NR- bond as a ring constituent, and when the heterocyclic ring is not an aromatic heterocyclic ring, the heterocyclic ring forms a condensed ring with a first aromatic ring, and / or the heterocyclic ring is substituted with a substituent comprising a second aromatic ring, or

[0190] (iii) A unit structure comprising at least one aromatic ring having at least one -NR2 substituent.

[0191] Here, R is a hydrogen atom or an alkoxymethyl group, and at least a part of R in all polymers is an alkoxymethyl group.

[0192] The connection of the aromatic rings by the -NR- bond in (i) above does not necessarily require that the -NR- bond is directly covalently bonded to the aromatic ring, and also includes an embodiment in which the -NR- bond is indirectly covalently bonded via a divalent organic group (e.g., a divalent hydrocarbon chain). In addition, it also includes an embodiment in which a plurality of -NR- bonds are connected to each other via a divalent organic group (e.g., a divalent hydrocarbon chain), and two aromatic rings are connected via such a plurality of connected -NR- bonds.

[0193] In addition, the so-called unit structure containing a heterocycle in (ii) above also includes a scheme in which the heterocycle and one or more first aromatic rings are fused, or the heterocycle or the fused ring is substituted with a substituent containing a second aromatic ring. Furthermore, the substitution of the fused ring by the substituent may be a substitution of the heterocycle portion or a substitution of the first aromatic ring portion. However, in the case where the heterocycle is not an aromatic heterocycle, the heterocycle forms a fused ring with the first aromatic ring and / or the heterocycle is substituted with a substituent containing a second aromatic ring. This is because the unit structure A is a unit structure having an aromatic ring. Here, as a specific example in which the -NR- bond is contained in an aromatic ring, aromatic rings such as pyrrole rings and fused aromatic rings such as carbazole can be cited.

[0194] In addition, the unit structure containing an aromatic ring having an -NR2 substituent in the above (iii) is a scheme having an aromatic ring (including not only an aromatic hydrocarbon ring but also an aromatic heterocycle) having an -NR2 substituent as a substituent containing a heteroatom, and it is preferred that at least one of the two Rs of the -NR2 substituent is an alkoxymethyl group, and more preferably one is an alkoxymethyl group. In addition, as the aromatic ring, a condensed ring composed of a plurality of aromatic monocyclic rings is preferred.

[0195] (2-3-2)

[0196] (2-3-2-1)

[0197] Among the unit structures A, (i) a unit structure comprising at least two aromatic rings connected by at least one -NR- bond, the unit structure of the following formula (I-1) is typical, but it also includes a scheme in which multiple aromatic rings connected by -NR- bonds are separately bonded by single bonds to form a ring, such as the unit structures of the following formulas (I-2) and (I-3) and positional isomers thereof.

[0198]

[0199] [Here, Ar is the same or different and represents an aromatic ring, and R represents a hydrogen atom or an alkoxymethyl group.]

[0200]

[0201] represents an aromatic ring part in a fused ring which may have a substituent, and each of them may be the same as or different from each other,

[0202] R represents a hydrogen atom or an alkoxymethyl group.]

[0203]

[0204] represents an aromatic ring part in a fused ring which may have a substituent, and each of them may be the same as or different from each other,

[0205] R represents a hydrogen atom or an alkoxymethyl group.]

[0206] (2-3-2-2)

[0207] In addition, examples of the unit structure A (ii) containing a heterocyclic ring having at least one -NR- bond as a ring constituent include unit structures of formulae (I-4) and (I-5).

[0208]

[0209] represents an aromatic ring part in a fused ring which may have a substituent, and each of them may be the same as or different from each other,

[0210] R represents a hydrogen atom or an alkoxymethyl group,

[0211] X represents C(R 1 )(R 2 ), O, S, or NR'; R' is the same as that of R and may be the same as or different from R; R 1 and R 2 are the same or different from each other and represent an aliphatic hydrocarbon group having 1 to 3 carbon atoms.]

[0212]

[0213] represents an aromatic ring part in a fused ring which may have a substituent, and each of them may be the same as or different from each other,

[0214] represents a heterocyclic moiety in a fused ring compound which may have a substituent,

[0215] R represents a hydrogen atom or an alkoxymethyl group,

[0216] Y is a substituent containing an aromatic ring, and may be a substituent of any of the above aromatic ring moiety and the above heterocyclic moiety.]

[0217] The aromatic ring possessed by Y can be directly bonded to the condensed ring of formula (I-5), or it can be bonded to the condensed ring of formula (I-5) via a divalent organic group. In addition, the aromatic ring possessed by Y can be directly bonded to the condensed ring of formula (I-5), or it can be indirectly bonded via a divalent linking group (e.g., a divalent hydrocarbon group).

[0218] Furthermore, the bond from Y to other unit structure preferably extends from Y's aromatic ring.

[0219] (2-3-3)

[0220] It is preferred that the unit structure A including a -NR- bond is at least one selected from the following.

[0221]

[0222] (2-3-4)

[0223] Regarding the "aromatic ring" in the unit structure A of the self-crosslinkable polymer which is one embodiment of the present invention, the above-mentioned (1-3) can be referred to.

[0224] It is preferred that the "aromatic ring" in the unit structure A of the self-crosslinkable polymer which is one embodiment of the present invention has 6 to 30, or 6 to 24 carbon atoms.

[0225] The "aromatic ring" in the unit structure A of the self-crosslinkable polymer as one embodiment of the present invention is preferably one or more benzene rings, naphthalene rings, anthracene rings, pyrene rings; or a condensed ring of a benzene ring, naphthalene ring, anthracene ring, pyrene ring and a heterocyclic ring or an aliphatic ring.

[0226] (2-3-5)

[0227] The aromatic ring in the unit structure A of the self-crosslinkable polymer as one embodiment of the present invention may further have a substituent unless the effects of the present invention are impaired. As such a substituent, see (1-3) above.

[0228] (2-3-6)

[0229] It is preferred that the unit structure A having a -NR- bond or an NR2 substituent is at least one selected from the following.

[0230]

[0231]

[0232]

[0233] Among the above-mentioned skeletons, the following are mentioned as more preferable skeletons.

[0234]

[0235] (2-3-7)

[0236] The unit structure A may optionally include a unit structure having no -NR- bond or NR2 substituent (here, R is a hydrogen atom or an alkoxymethyl group), and the following unit structures can be exemplified.

[0237] (Example of amine skeleton)

[0238]

[0239] (Example of phenol skeleton)

[0240]

[0241]

[0242]

[0243] In particular, although it is a unit structure A other than the unit structure A having a -NR- bond or an NR2 substituent, as a preferred unit structure A having a phenol skeleton, for example, the following unit structures can be included.

[0244]

[0245] (2-3-8)

[0246] In addition, at least one of the H of NH in the amine skeleton when R=H in the NR of the unit structure A skeleton in the above (2-3-6), the H of NH in the amine skeleton, the H of NH2 in the NR2 substituent when R=H, and the H of OH in the phenol skeleton in the above (2-3-7) can be replaced by the substituents described below.

[0247]

[0248]

[0249] (2-3-9)

[0250] As described in (2-4-3-3), (2-4-5-3), (2-4-6) and the like described later, although it has a structure that can also function as the unit structure B, since the structure has an aromatic ring,

[0251] in a unit structure A; or

[0252] When it functions as one unit structure C equivalent to the composite unit structure AB in which one unit structure A and one unit structure B are combined, it may be optionally contained.

[0253] (2-4; unit structure B)

[0254] (2-4-1)

[0255] The unit structure B of the self-crosslinkable polymer as one embodiment of the present invention is one or more unit structures as organic groups having one or more connecting carbon atoms.

[0256] The connecting carbon atom is as described in the above (1-1).

[0257] The unit structure B of the polymer preferably has a unit structure containing an organic group, wherein the organic group is a 4-17-membered monocyclic, bicyclic, tricyclic or tetracyclic organic group which may have a substituent, and the monocyclic ring is a non-aromatic monocyclic ring; at least one of the monocyclic rings constituting the bicyclic, tricyclic and tetracyclic rings is a non-aromatic monocyclic ring, and the remaining monocyclic rings may be aromatic monocyclic rings or non-aromatic monocyclic rings. In addition, one or more aromatic rings may be further fused or fused with the monocyclic, bicyclic, tricyclic or tetracyclic organic group to form a pentacyclic or higher ring. Furthermore, one or more connecting carbon atoms are not carbon atoms constituting the aromatic monocyclic ring, and the unit structure A [or unit structure C] is bonded to the unit structure B by covalently bonding with the aromatic ring of the unit structure A [or unit structure C].

[0258] (2-4-2)

[0259] The unit structure B preferably represents one or two or more unit structures including a structure represented by the following formula (II), (III) or (IV).

[0260] Such a unit structure also includes a unit structure in which two or three identical or different structures represented by these formulae are linked via a divalent or trivalent linking group [see (2-4-4-3) described later].

[0261] Furthermore, unit structure B is covalently bonded to a carbon atom on the aromatic ring of unit structure A via a bond in the following formula (II), (III) or (IV), so that unit structure A [or unit structure C] is bonded to unit structure B.

[0262]

[0263] [In formula (II), R and R' each independently represent a hydrogen atom, an aromatic ring residue having 6 to 30 carbon atoms which may have a substituent, a heterocyclic residue having 3 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a substituent.]

[0264]

[0265] [In formula (III),

[0266] Z is a monocyclic, bicyclic, tricyclic or tetracyclic condensed ring having 4 to 25 carbon atoms and optionally having a substituent, wherein the monocyclic ring is a non-aromatic monocyclic ring; at least one of the monocyclic rings constituting the bicyclic, tricyclic and tetracyclic rings is a non-aromatic monocyclic ring, and the remaining monocyclic rings may be either aromatic or non-aromatic. The monocyclic, bicyclic, tricyclic or tetracyclic condensed ring may further form a condensed ring with one or more aromatic rings to form a condensed ring of at least five rings,

[0267] X and Y are the same or different, indicating -CR 31 R 32 -Base, R 31 and R 32 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms,

[0268] x and y each represent the number of X and Y, and each independently represents 0 or 1.

[0269] *-X x is bonded to any carbon atom (referred to as "carbon atom 1") of the non-aromatic monocyclic ring constituting Z (when x=1), or extends from carbon atom 1 (when x=0),

[0270] Y y -* is bonded to any carbon atom (referred to as "carbon atom 2") of the above non-aromatic monocyclic ring constituting Z (when y=1), or extends from carbon atom 2 (when y=0),

[0271] The carbon atom 1 and the carbon atom 2 may be the same or different, and in different cases, may belong to the same non-aromatic monocyclic ring or different non-aromatic monocyclic rings.

[0272] * indicates a bonding bond. ]

[0273] -J 1 -Z 0 -J 2 - (IV)

[0274] [In formula (IV), Z 0represents an aromatic ring residue or an aliphatic ring residue having 6 to 30 carbon atoms which may have a substituent, or an organic group in which two aromatic ring residues or aliphatic ring residues are linked by a single bond, J 1 and J 2 Each independently represents a divalent organic group which is directly bonded or may have a substituent.]

[0275] (2-4-3)

[0276] (2-4-3-1)

[0277] When the unit structure B includes the formula (II), the definitions of R and R' in the formula (II) are the same as those described in (1-3) and (1-4) above regarding "substituent", "aromatic ring" and "heterocycle".

[0278]

[0279] Furthermore, in the definitions of R and R' in formula (II), examples of "alkyl" include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, 1-methyl-cyclopropyl, 2-methyl-cyclopropyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, cyclopentyl, 1-methyl-cyclobutyl 1,2-dimethyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl -n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2 ,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-isopropyl-cyclopropyl, 2-isopropyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl, and 2-ethyl-3-methyl-cyclopropyl, n-heptyl, n-octyl, n-nonyl, and n-decyl.

[0280] Preferably, R and R' are each independently phenyl, naphthyl, anthracenyl, phenanthryl, naphthacene or pyrene.

[0281] (2-4-3-2)

[0282] The two bonds in formula (II) are generally bonded to the aromatic ring of another structure having an aromatic ring (corresponding to unit structure A or C), but are bonded to the polymer terminal group (see (2-4-7) described later) at the polymer terminal.

[0283] In addition, in the unit structure of the structure shown in the formula (II), for example, the structures of two or three of the above-mentioned formulas (II) that are identical or different from each other can be combined with a divalent or trivalent linking group to form a dimer or trimer structure. In this case, one of the two bonds in the structure of each of the above-mentioned formulas (II) is combined with the above-mentioned linking group. As such a linking group, for example, a linking group (equivalent to unit structure A) with two or three aromatic rings can be cited. As the example of a specific divalent or trivalent linking group, it can be referred to (2-4-4-3) described later.

[0284] (2-4-3-3)

[0285] It should be noted that, when at least one of R and R' in formula (II) is an aromatic ring, if such an aromatic ring is combined with another unit structure B and combined with the aromatic ring of the unit structure A through a bonding bond of formula (II), then a unit structure C equivalent to the composite unit structure AB can be replaced by at least a part of the composite unit structure AB.

[0286] Therefore, such a unit structure C may be included in the unit structure including the structure represented by formula (II). In this case, it is considered that another bond of formula (II) is bonded to, for example, a polymer terminal group or an aromatic ring in another polymer chain to form a crosslink.

[0287] Such a mode of the unit structure C is described more specifically in the formula (V) in (2-4-6) described later.

[0288] It should be noted that, in this specification, when referring to the combination with the unit structure A, even if it is not explicitly stated, it can be interpreted as including the combination with the aromatic ring in the unit structure C. In addition, in this specification, when referring to the combination with the unit structure B, even if it is not explicitly stated, it can be interpreted as including the combination with the connecting carbon atom in the unit structure C.

[0289] (2-4-3-4)

[0290] Some specific examples of the organic group including the structure represented by formula (II) are as follows: * represents a bonding site with the unit structure A. Of course, the structure may include the exemplified structure as a part of the whole.

[0291]

[0292] (2-4-4)

[0293] (2-4-4-1)

[0294] In the case where the unit structure B comprises formula (III),

[0295]

[0296] In formula (III),

[0297] Z is a monocyclic ring or a bicyclic, tricyclic or tetracyclic condensed ring which may have a substituent and has 4 to 25 carbon atoms. Furthermore, the number of carbon atoms here refers to the number of carbon atoms constituting only the ring skeleton of the monocyclic ring or the bicyclic, tricyclic or tetracyclic condensed ring excluding the substituent, and does not include the number of heteroatoms constituting the heterocyclic ring when the monocyclic or condensed ring is a heterocyclic ring.

[0298] The monocyclic ring is a non-aromatic monocyclic ring; at least one of the monocyclic rings constituting the bicyclic, tricyclic and tetracyclic rings is a non-aromatic monocyclic ring, and the remaining monocyclic rings may be either an aromatic monocyclic ring or a non-aromatic monocyclic ring.

[0299] The above-mentioned monocyclic, bicyclic, tricyclic or tetracyclic condensed ring may further form a condensed ring with one or more aromatic rings to form a pentacyclic or higher condensed ring, and the number of carbon atoms in the pentacyclic or higher condensed ring is preferably 40 or less. The number of carbon atoms here refers to the number of carbon atoms constituting only the ring skeleton of the above-mentioned pentacyclic or higher condensed ring excluding substituents, and does not include the number of heteroatoms constituting the heterocycle when the above-mentioned pentacyclic or higher condensed ring is a heterocycle.

[0300] X and Y are the same or different, indicating -CR 31 R 32 -Base, R 31 and R 32 Each of them is the same or different and represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms.

[0301] x and y each represent the number of X and Y, and each independently represents 0 or 1.

[0302] *-X x is bonded to any carbon atom (referred to as "carbon atom 1") of the non-aromatic monocyclic ring constituting Z (when x=1) or extends from carbon atom 1 (when x=0),

[0303] Y y -* is bonded to any carbon atom (referred to as "carbon atom 2") of the above-mentioned non-aromatic monocyclic ring constituting Z (when y=1) or extends from carbon atom 2 (when y=0), and carbon atom 1 and carbon atom 2 may be the same or different, and in different cases, may belong to the same non-aromatic monocyclic ring or different non-aromatic monocyclic rings.

[0304] In formula (III), a connecting carbon atom other than carbon atom 1 and carbon atom 2 may be optionally included [see (2-4-4-4) described later].

[0305] It should be noted that, when Z is a condensed ring of tricyclic or higher types, the serial positional relationship between the one or two non-aromatic monocyclic rings to which carbon atoms 1 and 2 in formula (III) respectively belong and the remaining monocyclic rings in the condensed ring is arbitrary. When carbon atom 1 and carbon atom 2 belong to different non-aromatic monocyclic rings (referred to as "non-aromatic monocyclic ring 1" and "non-aromatic monocyclic ring 2", respectively), the serial positional relationship between the non-aromatic monocyclic ring 1 and the non-aromatic monocyclic ring 2 in the condensed ring is also arbitrary.

[0306] (2-4-4-2)

[0307] As a unit structure that is one embodiment of the formula (III), the following formula (III-1) can be mentioned.

[0308]

[0309] In formula (III-1),

[0310] Z is a 4- to 17-membered monocyclic, bicyclic, tricyclic or tetracyclic organic group which may have a substituent, at least one of the one or more monocyclic rings constituting the organic group is a non-aromatic monocyclic ring, and the number of non-aromatic monocyclic rings is 4 at most. The other monocyclic rings are aromatic rings, and may further form a condensed ring with an additional aromatic monocyclic ring to form a polycyclic organic group of pentacyclic or higher rings.

[0311] Here, the non-aromatic monocyclic ring is a monocyclic ring that is not aromatic, and is typically an aliphatic monocyclic ring (which may include an aliphatic heteromonocyclic ring). As the non-aromatic monocyclic ring, the above-mentioned (1-5) can be referred to.

[0312] In addition, as the aromatic monocyclic ring or aromatic ring, for example, as exemplified in the above (1-3), a benzene ring, a naphthalene ring, an anthracene ring, a pyrene ring, etc. which may have a substituent can be cited as preferred examples, and as the substituent, the examples exemplified in the above (1-3) can be cited.

[0313] In the non-aromatic monocyclic ring, there may be C and C' in formula (III) respectively representing one carbon atom in the group of atoms constituting the cyclic part [the so-called connecting carbon atom in (1-1) above]. Among them, the connecting carbon atom C must exist, but the connecting carbon atom C' is arbitrary, and n in formula (III) representing the number of C' is 0 to 2, and preferably n is 0.

[0314] X, Y, X', Y' are the same or different, indicating -CR 1 R 2 -Base, R 1 and R 2They are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms. However, since they are just arbitrary linking groups, x, y, x', and y' representing the number (0 or 1) of X, Y, X', and Y' may all be 0.

[0315] p, q, p', and q' represent the number of bonds and each independently represents 0 or 1. When p is 0, it means that it is replaced by a hydrogen atom.

[0316] In principle, these bonds are bonded to the aromatic ring of another structure (corresponding to the unit structure A or C) having an aromatic ring, but are bonded to the polymer terminal group at the polymer terminal [see (2-4-7) described later].

[0317] In order to form a polymer chain, at least 2 bonds are required, so when n is 0, p and q are 1; when n is 1, at least one of p and q is 1, and at least one of p' and q' is 1, provided that there is at least one bond extending from C and C' (the so-called connecting carbon atoms); similarly, when n is 2, at least one of p and q is 1, and at least one of p' and q' of each C' is 1.

[0318] When there are two or more bonds, it is considered that these extra bonds are bonded to, for example, a polymer terminal group or an aromatic ring in another polymer chain to form a crosslink.

[0319] (2-4-4-3)

[0320] Two or three structures of the above formula (III) which are the same or different from each other may be combined with a divalent or trivalent linking group to form a dimer or trimer structure.

[0321] In this case, one of p or q as a bond in each structure of the above formula (III) is bonded to the above linking group. Furthermore, n is not 0, one bond is provided from the connecting carbon atom C, and at least one bond is provided from the connecting carbon atom C'.

[0322] Examples of such a linking group include a linking group having two or three aromatic rings in the unit structure that can be used as the unit structure A, and examples thereof include a divalent or trivalent linking group of the following formula.

[0323]

[0324] [X 1 represents a single bond, a methylene group, an oxygen atom, a sulfur atom, -N(R 1 )-, R 1represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms (including chain hydrocarbons and cyclic hydrocarbons (which may be aromatic or non-aromatic)).]

[0325]

[0326] [X 2 represents a methylene group, an oxygen atom, -N(R 2 )-, R 2 It represents a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, or an aromatic hydrocarbon group having 5 to 20 carbon atoms.

[0327]

[0328] Alternatively, a divalent linking group such as the following formula which can form a covalent bond to a carbon atom by an addition reaction of an acetylide with a ketone can also be exemplified.

[0329]

[0330] (2-4-4-4)

[0331] Some specific examples of the organic group including the structure represented by formula (III) are as follows: Of course, the structure described above may be included as a part of the whole.

[0332]

[0333]

[0334] (2-4-5)

[0335] (2-4-5-1)

[0336] In the case where the unit structure B comprises formula (IV),

[0337] -J 1 -Z 0 -J 2 - (IV)

[0338] In formula (IV), Z 0 In the definition of , the "aromatic ring", "substituent" and "aliphatic ring" are the same as those described in the above (1-3) and (1-5).

[0339] Examples of the organic group in which two aromatic ring residues or aliphatic ring residues are linked via a single bond include divalent residues such as a biphenyl group, a cyclohexylphenyl group, and a dicyclohexyl group.

[0340] In J 1 and J 2In the definition of , the "divalent organic group" is preferably a linear or branched alkylene group having 1 to 6 carbon atoms which may have a hydroxyl group or a halogenated group (e.g., fluorine) as a substituent. Examples of the linear alkylene group include methylene, ethylene, propylene, butylene, pentylene, and hexylene.

[0341] (2-4-5-2)

[0342] Two or three structures of the above formula (IV) which are the same or different from each other may be combined with a divalent or trivalent linking group to form a dimer or trimer structure.

[0343] In this case, one of the two bonds in each structure of the above formula (IV) is bonded to the above linking group.

[0344] Examples of such a linking group include a linking group having two or three aromatic rings in the unit structure that can be used as the unit structure A.

[0345] As specific examples of the divalent or trivalent linking group, reference can be made to the above (2-4-4-3).

[0346] (2-4-5-3)

[0347] It should be noted that since formula (IV) includes a scheme containing an aromatic ring, in the case of such a scheme, if the aromatic ring of formula (IV) is combined with another unit structure B and is combined with the aromatic ring of unit structure A through a bond of formula (IV), then a unit structure C equivalent to the composite unit structure AB can be replaced with at least one composite unit structure AB.

[0348] Therefore, such a unit structure C may be included in the unit structure including the structure represented by formula (IV). In this case, it is considered that another bond of formula (IV) is bonded to, for example, a polymer terminal group or an aromatic ring in another polymer chain to form a crosslink.

[0349] Such a mode of the unit structure C is described more specifically in the formula (V) in (2-4-6) described later.

[0350] (2-4-5-4)

[0351] Some specific examples of the unit structure including the structure represented by formula (IV) are as follows: * represents a bonding site with the unit structure A. Of course, the unit structure may include the exemplified structure as a part of the whole.

[0352]

[0353] (2-4-6)

[0354] (2-4-6-1)

[0355] As in the above embodiments (2-4-3-3) and (2-4-5-3), Z in the above formula (III) contains an aromatic ring Ar 1 In the case of, as a unit structure C that can be derived from such formula (III) and replace at least a part of the composite unit structure AB and is equivalent to the composite unit structure AB, a unit structure including a structure of the following formula (V) can be mentioned.

[0356]

[0357] In formula (V),

[0358] Z 1 represents at least one non-aromatic monocyclic ring, Ar 1 Represents Z 1 The non-aromatic monocyclic ring of the present invention forms at least one aromatic monocyclic ring of the fused ring, as Z and Ar 1 As a whole, it constitutes a bicyclic, tricyclic, tetracyclic or pentacyclic condensed ring which may have a substituent and has a carbon number of 8 to 25. Furthermore, the carbon number here refers to the number of carbon atoms constituting only the ring skeleton of the bicyclic, tricyclic or tetracyclic condensed ring excluding the substituent, and does not include the number of heteroatoms constituting the heterocyclic ring when the bicyclic, tricyclic or tetracyclic condensed ring is a heterocyclic ring.

[0359] One or more aromatic rings may further form a condensed ring with the above-mentioned bicyclic, tricyclic, tetracyclic or pentacyclic organic group to form a hexacyclic or higher ring. The number of carbon atoms in the hexacyclic or higher ring condensed ring is preferably 40 or less. The number of carbon atoms referred to herein refers to the number of carbon atoms constituting only the ring skeleton of the above-mentioned pentacyclic or higher ring condensed ring excluding substituents, and does not include the number of heteroatoms constituting the heterocyclic ring when the above-mentioned hexacyclic or higher ring condensed ring is a heterocyclic ring.

[0360] In addition, among the cyclic organic groups, Z 1 One or more non-aromatic monocyclic rings and Ar 1 The sequential position relationship of one or more aromatic monocyclic rings of Z includes any relationship. 1 There are two or more non-aromatic monocyclic rings belonging to Ar 1 When there are two or more aromatic monocyclic rings, Z 1 The non-aromatic monocyclic ring and the Ar 1 The aromatic monocyclic rings may be arranged alternately to form a condensed ring.

[0361] In addition, X, Y, x, and y are the same as defined in formula (III).

[0362] As one embodiment of the formula (V), the following formula (V-1) can be mentioned.

[0363]

[0364] [In formula (V-1),

[0365] Z 1 ,Ar 1 , X, Y, x and y are the same as defined in formula (V),

[0366] T represents the polymer terminus.]

[0367] When a bond connecting a carbon atom in formula (V-1) is connected to a polymer terminal T (hydrogen atom; various functional groups such as hydroxyl group and unsaturated aliphatic hydrocarbon group, terminal unit structure A, unit structure A in other polymer chains, etc.), a unit structure C equivalent to the composite unit structure AB may be substituted with at least one composite unit structure AB. That is, the aromatic ring in formula (V-1) [Ar in formula (V-1)] 1 ] is combined with other unit structures B, and is combined with the aromatic ring of unit structure A using the bond from the remaining connecting carbon atom shown in formula (V-1), thereby extending the polymer chain.

[0368] Alternatively, as one embodiment of the formula (V), another unit structure C equivalent to the composite unit structure AB may include a unit structure including the structure of the following formula (V-2).

[0369]

[0370] Here, in formula (V-2),

[0371] Z 1 represents at least one non-aromatic monocyclic ring, Ar 1 represents at least one aromatic monocyclic ring as Z and Ar 1 As a whole, a cyclic organic group is formed as a bicyclic or higher condensed ring of 8 to 17 members which may have a substituent. The arrangement and order of each aromatic monocyclic ring and non-aromatic monocyclic ring in the cyclic organic group may be arbitrary.

[0372] Here, the "non-aromatic monocyclic ring", "aromatic monocyclic ring" or "aromatic ring" are as described in the above (1-3) and (1-5).

[0373] In the non-aromatic monocyclic ring, C in the formula (V-2) which represents one carbon atom in the group of atoms constituting the cyclic part [the so-called connecting carbon atom in the above (1-1)] may exist.

[0374] X and Y are the same or different, indicating -CR 1 R 2 -Base, R 1 and R 2 They are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms. However, since they are merely arbitrary linking groups, x and y representing the number of X and Y (0 or 1) may all be 0.

[0375] T represents a polymer terminal group or an aromatic ring residue Ar 2 , regarding the aromatic ring residue, it is the same as the above (2-4-4-1).

[0376] p represents one bond for covalent bonding with the aromatic ring of the unit structure A (which may include the aromatic ring in the unit structure C).

[0377] On the other hand, k and m represent the number of bonds used for covalent bonding with unit structure B (which may include unit structure C), and k independently represents 0 to 2, m represents 0 or 1, and at least one of k and m is not 0 (when k and m are 0, it means that the bond is replaced by a hydrogen atom).

[0378] Therefore, regarding the formula (V-2), one unit structure C equivalent to the composite unit structure AB may be substituted with at least a part of the composite unit structure AB.

[0379] It should be noted that, when k is 2, or when k is 1 and m is 1, the extra bonds form crosslinks with polymer terminal groups or other polymer chains.

[0380] (2-4-6-2)

[0381] The unit structure C including the structure of formula (V), particularly (V-1) or (V-2), is illustrated by a more specific structure.

[0382] For example, in the following structure, T is a hydrogen atom as a terminal group, and p and k1, or p and k2, can form a unit structure C equivalent to the composite unit structure AB.

[0383] It should be noted that k1 and k2 can also function as a unit structure A.

[0384]

[0385] The following structural example shows an example where T is a phenyl group. In this example, p and k1, p and k2, or p and m can form a unit structure C equivalent to the composite unit structure AB.

[0386] It should be noted that the unit structure A can also be functioned by k1 and k2, k1 and m, or k2 and m.

[0387]

[0388] (2-4-6-3)

[0389] Some specific examples of the unit structure C (one unit structure equivalent to the composite unit structure AB) of the formula (V) are as follows: * represents a bonding site with the unit structure A.

[0390] In the unit structure C, the bond to the unit structure B extends from the aromatic ring in these structures, but in the specific examples below, such a bond is omitted. It goes without saying that the unit structure may include the exemplified structure as a part of the whole.

[0391]

[0392] In addition, in the above-mentioned specific examples, when the bond does not extend from the aromatic ring, it is a specific example of a polymer terminal.

[0393] (2-4-7)

[0394] At the polymer terminal, the unit structure B forms a covalent bond with the polymer terminal group. Such a polymer terminal group may be an aromatic ring derived from the unit structure A, or may not be such.

[0395] Examples of the polymer terminal group include an aromatic ring residue having 6 to 30 carbon atoms which may have a substituent, an unsaturated hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, a hydroxyl group, and a hydrogen atom.

[0396] (2-5: Synthesis method of phenolic varnish resin)

[0397] The novolac resin which is one embodiment of the present invention can be prepared by a known method.

[0398] For example, it can be prepared by condensing an aromatic ring-containing compound represented by HAH with an oxygen-containing compound represented by OHC-B, O=CB, HO-B-OH, RO-B-OR, etc. Here, in the formula, -A- corresponds to the unit structure A, and -C(B)- or -B- corresponds to the unit structure B. R represents an alkyl group having about 1 to 3 carbon atoms. Either one of the aromatic ring-containing compound and the oxygen-containing compound can be used, or two or more of them can be used in combination. In the condensation reaction, the oxygen-containing compound can be used in a ratio of 0.1 to 10 moles, preferably 0.1 to 2 moles, relative to 1 mole of the aromatic ring-containing compound.

[0399] As the catalyst used in the condensation reaction, inorganic acids such as sulfuric acid, phosphoric acid, and perchloric acid, organic sulfonic acids such as p-toluenesulfonic acid, p-toluenesulfonic acid monohydrate, methanesulfonic acid, and trifluoromethanesulfonic acid, and carboxylic acids such as formic acid and oxalic acid can be used. The amount of the catalyst used varies depending on the type of the catalyst used, but is generally 0.001 to 10,000 parts by mass, preferably 0.01 to 1,000 parts by mass, and more preferably 0.05 to 100 parts by mass, relative to 100 parts by mass of the aromatic ring-containing compound (in many cases, the total of these).

[0400] The condensation reaction can be carried out without a solvent, but is usually carried out using a solvent. The solvent is not particularly limited as long as it can dissolve the reaction substrate and does not hinder the reaction. Examples thereof include 1,2-dimethoxyethane, diethylene glycol dimethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, tetrahydrofuran, tetrahydropyran, 4-methyltetrahydropyran, diethylene glycol di ... The condensation reaction temperature is usually 40°C to 200°C, preferably 100°C to 180°C. The reaction time varies depending on the reaction temperature, but is usually 5 minutes to 50 hours, preferably 5 minutes to 24 hours.

[0401] The weight average molecular weight of the novolac resin according to one embodiment of the present invention is usually 500 to 100,000, preferably 600 to 50,000, 700 to 10,000, or 800 to 8,000.

[0402] [3. Resist underlayer film-forming composition [7]]

[0403] (3-1)

[0404] The resist underlayer film-forming composition according to one embodiment of the present invention comprises a thermal acid generator, a self-crosslinking polymer [1], and a solvent, and may further optionally comprise a crosslinking agent and a surfactant.

[0405] The self-crosslinking polymer [1] has been described in the above-mentioned [2. Self-crosslinking polymer [1]].

[0406] (3-2: Thermal Acid Generator)

[0407] (3-2-1)

[0408] Any thermal acid generator may be used within a range not impairing the effects of the present invention, but a thermal acid generator represented by the following formula (1) can be preferably used.

[0409] [A 1 (SO3) n ] n-(B 1 H) n+ (one)

[0410] Here, in formula (1),

[0411] A 1 It is an optionally substituted linear, branched, or cyclic saturated or unsaturated aliphatic hydrocarbon group, or an optionally substituted aromatic ring residue, and is preferably a methyl group, a trifluoromethyl group, a naphthyl group, a norbornylmethyl group, a dimethylphenyl group, or a tolyl group.

[0412] Here, regarding the "aromatic ring" and the "residue", refer to the above-mentioned (1-3) and (1-2), respectively.

[0413] In formula (1), n ​​represents the number of sulfonic acid anion groups, which is 1 or 2, preferably 1.

[0414] In formula (1), B 1 is one or more counterbases, is a monobasic base, or represents the monobasic part of a dibasic base or a tribasic base. 1 In the case of a dibasic or tribasic base, it is equivalent to B 1 There are two or three of them, which are covalently bonded to each other.

[0415] Furthermore, A 1 With B 1 It can be connected by a single bond or a linker. 1 Preferably, at least one of the bases has a pKa greater than that of pyridine.

[0416] In the present invention, specific examples of the base having a pKa greater than that of pyridine, preferably a base having a pKa of 6.5 or greater, include N-methylmorpholine, N,N-diethylaniline, N-isobutylmorpholine, and N-allylmorpholine.

[0417] In the determination of pKa, for example, the pKa value in water, preferably the pKa value in water at 25° C., can be measured by potentiometric titration [see, for example, S. Xu et al., “Dissociation constants of alkanolamines”, Can. J. Chem. 71, 1048 (1993)] for comparison. References may also be made to R. Linnell, J. Org. Chem. 1960, 25, 2, 290-290; Kotake Mujio, ed.: “Dayoujikagakubejuan 2, yojinkakendenkan”, p. 584 (1963), (Asakura Bookstore); HK Hall Jr. et al., Tetrahedron Letters 53 (2012) 1830-1832, etc.

[0418] (3-2-2)

[0419] Preferably, the counter base B in the formula (1) of the above (3-2-1) is 1 For R I R II R III N.

[0420] [Wherein,

[0421] R I and R II Each independently represents a hydrogen atom, a linear or branched saturated or unsaturated aliphatic hydrocarbon group which may be substituted,

[0422] R I With R II The ring may be formed via a hetero atom or not via a hetero atom, or may be formed via an aromatic ring, and the hetero atom is preferably an oxygen atom, a nitrogen atom or a sulfur atom.

[0423] R III represents a hydrogen atom, an aromatic ring residue which may be substituted, or a straight-chain or branched saturated or unsaturated aliphatic hydrocarbon group which may be substituted,

[0424] In R I With R II When no ring is formed, R III is a hydrogen atom or an aromatic ring residue which may be substituted].

[0425] More preferably, the counter base B in the formula (I) of component (a) is 1 It is a base represented by a cyclic amine compound of the following formula (II) or (III).

[0426] R 1 R 2 R3 N (II)

[0427] [In formula (2),

[0428] R 1 and R 2 Each independently represents a linear or branched saturated or unsaturated aliphatic hydrocarbon group which may be substituted,

[0429] R 3 represents a hydrogen atom, an aromatic group which may be substituted, preferably a phenyl group, a naphthyl group, an anthracenyl group, a pyrenyl group, or a phenanthryl group which may be substituted.],

[0430]

[0431] [In formula (3),

[0432] R is

[0433] Hydrogen atom;

[0434] an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, a hydroxyl group having 1 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, an organic group containing an ether bond, an organic group containing a keto bond, or an organic group containing an ester bond, which may be substituted with a nitro group, a cyano group, an amino group, a carboxyl group, a hydroxyl group, an amide group, an aldehyde group, a (meth)acryloyl group, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom), or an alkoxy group having 1 to 10 carbon atoms; or

[0435] The groups obtained by combining them are

[0436] R' is an aromatic ring and is an aromatic ring condensed with the ring of the cyclic amine in formula (III), or -(R a ) n -X-(R b ) m -,

[0437] R a and R b Each independently represents an alkylene group which may be substituted,

[0438] X is O, S, SO2, CO, CONH, COO, or NH,

[0439] n and m are each independently 2, 3, 4, 5, or 6.]

[0440] Preferably, R in formula (III) is a hydrogen atom, a methyl group, an ethyl group, an isobutyl group, an allyl group, or a cyanomethyl group.

[0441] In addition, it is preferred that R' in formula (II) is -(CH2) n-O-(CH2) m - means that n and m are each independently 2, 3, 4, 5, or 6.

[0442] (3-2-3)

[0443] As A of the formula (1) in the above (3-2-1) 1 In the definition of or R in (3-2-2) above I R II R III R in N I , R II , R III In the definition of R 1 R 2 R 3 R in N 1 , R 2 In the definition of "straight-chain or branched saturated aliphatic hydrocarbon group", for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl -n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, etc.

[0444] In addition, as A in the formula (1) of the above (3-2-1), 1The “cyclic saturated aliphatic hydrocarbon group” in the present invention includes, for example, cyclopropyl, cyclobutyl, 1-methyl-cyclopropyl, 2-methyl-cyclopropyl, cyclopentyl, 1-methyl-cyclobutyl, 2-methyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3- Dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-isopropyl-cyclopropyl, 2-isopropyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,3-trimethyl-cyclopropyl, 1-ethyl-2-methyl-cyclopropyl, 2-ethyl-1-methyl-cyclopropyl, 2-ethyl-2-methyl-cyclopropyl and 2-ethyl-3-methyl-cyclopropyl, etc.

[0445] In addition, as A in the formula (1) of the above (3-2-1), 1 In the definition of or R in (3-2-2) above I R II R III R in N I , R II , R III In the definition of or in formula (II) R 1 , R 2In the definition of "straight-chain or branched unsaturated aliphatic hydrocarbon group", for example, vinyl, 1-propenyl, 2-propenyl, 1-methyl-1-vinyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylvinyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylvinyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-ethyl-2-propenyl, 2-methyl-1-butenyl, 2-methyl-2-butenyl, 2-methyl-3-butenyl, 3-methyl-1- butenyl, 3-methyl-2-butenyl, 3-methyl-3-butenyl, 1,1-dimethyl-2-propenyl, 1-isopropylvinyl, 1,2-dimethyl-1-propenyl, 1,2-dimethyl-2-propenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 4-hexenyl, 5-hexenyl, 1-methyl-1-pentenyl, 1-methyl-2-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-n-butylvinyl, 2-methyl-1-pentenyl, 2-methyl-2-pentenyl, 2-methyl-3-pentenyl, 2-methyl-4-pentenyl, 2-n-propyl-2-propenyl, 3-methyl-1-pentenyl, 3-methyl-2-pentenyl, 3-methyl-3 4-Methyl-3-pentenyl, 4-methyl-1-pentenyl, 4-methyl-2-pentenyl, 4-methyl-3-pentenyl, 4-methyl-4-pentenyl, 1,1-dimethyl-2-butenyl, 1,1-dimethyl-3-butenyl, 1,2-dimethyl-1-butenyl, 1,2-dimethyl-2-butenyl, 1,2-dimethyl-3-butenyl, 1-methyl-2-ethyl-2-propenyl, 1-sec-butylvinyl, 1,3-dimethyl-1-butenyl, 1,3-dimethyl-2-butenyl, 1,3-dimethyl-3-butenyl, 1-isobutylvinyl, 2,2-dimethyl-3-butenyl, 2,3-dimethyl-1-butenyl 1-ethyl-1-butenyl, 1-ethyl-2-butenyl, 1-ethyl-3-butenyl, 1-n-propyl-1-propenyl, 1-n-propyl-2-propenyl, 2-ethyl-1-butenyl, 2-ethyl-2-butenyl, 2-ethyl-3-butenyl, 1,1,2-trimethyl-2-propenyl, 1-tert-butylvinyl, 1-methyl-1-ethyl-2-propenyl, 1-ethyl-2-methyl-1-propenyl, 1-ethyl-2-methyl-2-propenyl, 1-isopropyl-1-propenyl, 1-isopropyl-2-propenyl and the like.

[0446] In addition, as A in the formula (1) of the above (3-2-1), 1 In the definition of "cyclic unsaturated aliphatic hydrocarbon group", for example, 1-cyclopentenyl, 2-cyclopentenyl, 3-cyclopentenyl, 1-methyl-2-cyclopentenyl, 1-methyl-3-cyclopentenyl, 2-methyl-1-cyclopentenyl, 2-methyl-2-cyclopentenyl, 2-methyl-3-cyclopentenyl, 2-methyl-4-cyclopentenyl, 2-methyl-5-cyclopentenyl, 2-methylene-cyclopentyl, 3-methyl-1-cyclopentenyl, 3-methyl-2-cyclopentenyl, 3-methyl-3-cyclopentenyl, 3-methyl-4-cyclopentenyl, 3-methyl-5-cyclopentenyl, 3-methylene-cyclopentyl, 1-cyclohexenyl, 2-cyclohexenyl and 3-cyclohexenyl can be mentioned.

[0447] In addition, as A in the formula (1) of the above (3-2-1), 1 The aromatic hydrocarbon group in the definition of or the definition of R in the formula (III) of the above (3-2-2) among the “aromatic ring residues” includes, for example, phenyl, o-methylphenyl, m-methylphenyl, p-methylphenyl, 2,3-dimethylphenyl, 2,4-dimethylphenyl, 2,5-dimethylphenyl, 2,6-dimethylphenyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, o-chlorophenyl, m-chlorophenyl, p-chlorophenyl, o-fluorophenyl, p-fluorophenyl, o-methoxyphenyl, p-methoxyphenyl, p-nitrophenyl, p-cyanophenyl, α-naphthyl, β-naphthyl, o-biphenyl, m-biphenyl, p-biphenyl, 1-anthryl, 2-anthryl, 9-anthryl, 1-phenanthryl, 2-phenanthryl, 3-phenanthryl, 4-phenanthryl, 9-phenanthryl, 1-pyrenyl, 2-pyrenyl and 3-pyrenyl.

[0448] In addition, as A in the formula (1) of the above (3-2-1), 1 The aromatic heterocyclic residue among the "aromatic ring residue" in the definition of "aromatic heterocyclic residue" includes, for example, furanyl, thienyl, pyrrolyl, imidazolyl, pyranyl, pyridyl, pyrimidinyl, pyrazinyl, pyrrolidinyl, piperidinyl, piperazinyl, morpholinyl, quinuclidine, indolyl, purinyl, quinolyl, isoquinolyl, chromenyl, thianthrenyl, phenothiazinyl, phenanthracene ... acridine, phenazine, carbazolyl, etc.

[0449] R I R II R III R in N III In the definition of R 1 R 2 R 3 R in N 3 In the definition of , the “aromatic ring” or “aromatic ring” is the same as exemplified above.

[0450] In addition, in the above formula (1) (3-2-1), A 1 In the definition of or R in (3-2-2) above I R II R III R in N I , R II , R III In the definition of, or in the formula (II) of (3-2-2) above, R 1 , R 2 , R 3 In the definition of or R in (3-2-2) above a , R b In the definition of , examples of the substituent corresponding to “which may be substituted” include a nitro group, an amino group, a cyano group, a sulfo group, a hydroxyl group, a carboxyl group, an aldehyde group, a propargylamino group, a propargyloxy group, a halogen atom, an alkoxy group having 1 to 10 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, an alkynyl group having 2 to 10 carbon atoms, an aryl group having 6 to 40 carbon atoms, an organic group containing an ether bond, an organic group containing a keto bond, an organic group containing an ester bond, or a combination thereof.

[0451] In addition, about the organic group containing an ether bond, the organic group containing a ketone bond, and the organic group containing an ester bond, the examples in (3-2-4) described later can be referred to.

[0452] Examples of the "alkoxy" in the definition of R in the formula (III) of the above (3-2-2) include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, n-pentyloxy, 1-methyl-n-butoxy, 2-methyl-n-butoxy, 3-methyl-n-butoxy, 1,1-dimethyl-n-propoxy, 1,2-dimethyl-n-propoxy, 2,2-dimethyl-n-propoxy, 1-ethyl-n-propoxy, n-hexyloxy, 1-methyl-n-pentyloxy, 2-methyl-n-pentyloxy, 1-ethyl-n-butoxy, 2-ethyl-n-butoxy, 1,1,2-trimethyl-n-propoxy, 1,2,2-trimethyl-n-propoxy, 1-ethyl-1-methyl-n-propoxy, and 1-ethyl-2-methyl-n-propoxy.

[0453] Regarding the definition of R in the formula (III) of the above (3-2-2), or R a , R bThe “alkylene group” in the definition of can be exemplified by an alkylene group obtained by replacing the hydrogen atoms of the alkyl groups exemplified in the above “straight-chain or branched saturated aliphatic hydrocarbon group” and “cyclic saturated aliphatic hydrocarbon group” in this item (3-2-3) with additional bonding bonds.

[0454] In addition, regarding the "alkenyl group" in the definition of R in the formula (III) of the above (3-2-2), reference can be made to the examples of the above-mentioned "straight-chain or branched unsaturated aliphatic hydrocarbon group" and "cyclic unsaturated aliphatic hydrocarbon group" in this item (3-2-3).

[0455] In addition, regarding the "hydroxyalkyl group" in the definition of R in the formula (III) of the above (3-2-2), the following organic groups can be exemplified: In the formula, * represents a carbon atom to which a bond extends.

[0456]

[0457] In addition, regarding the "alkynyl group" in the definition of R in formula (II) of the above (3-2-2), the scheme of being bonded to an aliphatic hydrocarbon chain (bonded to the end of the chain, or inserted into the middle of the chain), the scheme of further containing a heteroatom (oxygen atom, nitrogen atom, etc.) in the above scheme, or the scheme of connecting multiple alkynyl groups, etc., can be exemplified by the following organic groups. The * in the formula represents the carbon atom to which the bond extends.

[0458]

[0459] The following example is a scheme in which the heteroatom is bonded to the middle part of the chain of R.

[0460]

[0461] (3-2-4)

[0462] In the definition of R in formula (III) of the above (3-2-2), the "organic group containing an ether bond" may be R 11 -OR 11 (R 11 Each independently represents an alkyl group having 1 to 6 carbon atoms such as methyl and ethyl, an alkylene group, phenyl, phenylene, naphthyl, naphthylene, o-aminobenzoyl, or pyrenyl. The residue of the ether compound represented by ) includes, for example, an organic group containing an ether bond such as a methoxy group, an ethoxy group, or a phenoxy group.

[0463] In the definition of R in formula (III) of the above (3-2-2), the "organic group containing a ketone bond" may be R 21 -C(=O)-R 21 (R 21Each independently represents an alkyl group having 1 to 6 carbon atoms such as methyl and ethyl, an alkylene group, phenyl, phenylene, naphthyl, naphthylene, o-aminobenzoyl, or pyrenyl. The residue of the ketone compound represented by ) includes, for example, an organic group containing a keto bond including an acetoxy group and a benzoyl group.

[0464] In the definition of R in formula (III) of the above (3-2-2), the "organic group containing an ester bond" may be R 31 -C(=O)OR 31 (R 31 Each independently represents an alkyl group having 1 to 6 carbon atoms such as methyl and ethyl, an alkylene group, phenyl, phenylene, naphthyl, naphthylene, o-aminobenzoyl, or pyrenyl. The residue of the ester compound represented by ) includes organic groups containing an ester bond such as methyl ester, ethyl ester, and phenyl ester.

[0465] (3-2-5)

[0466] Examples of the thermal acid generator represented by formula (1) include, but are not limited to, any combination of at least one of the examples of counterbase cations and sulfonic acid anions shown below so that the charge becomes neutral.

[0467] (3-2-5-1: Examples of counter base cations)

[0468]

[0469]

[0470]

[0471] (3-2-5-2: Examples of sulfonic acid anions)

[0472]

[0473]

[0474] (3-2-6)

[0475] More specifically, the following examples of thermal acid generators which are combinations of counter base cations and sulfonic acid anions can be cited, but the examples are not limited to these.

[0476]

[0477]

[0478]

[0479] (3-2-7)

[0480] The amount of the thermal acid generator is 0.0001 to 20 mass %, preferably 0.0005 to 10 mass %, and more preferably 0.01 to 3 mass % based on the total solid content in the resist underlayer film-forming composition.

[0481] The thermal decomposition starting temperature of the thermal acid generator according to one embodiment of the present invention, i.e., the thermal acid generation temperature, is preferably 50° C. or higher, more preferably 100° C. or higher, further preferably 150° C. or higher, and is preferably 400° C. or lower.

[0482] (3-3: Solvent)

[0483] (3-3-1)

[0484] The resist underlayer film forming composition as one embodiment of the present invention contains a solvent.

[0485] The solvent is not particularly limited as long as it can dissolve the thermal acid generator, the self-crosslinking polymer [1], and any components added as needed. In particular, when the uniform solution is used for nanoimprinting, it is recommended to use a solvent generally used in the photolithography process in combination if coating performance is taken into consideration.

[0486] Examples of such solvents include methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, methyl isobutyl carbinol, propylene glycol monobutyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, propylene glycol monobutyl ether acetate, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxylate, ethyl hydroxylate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, Methyl propionate, methyl pyruvate, ethyl pyruvate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monopropyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, propylene glycol dipropyl ether, propylene glycol dibutyl ether, ethyl lactate, propyl lactate, isopropyl lactate, butyl lactate, isobutyl lactate, methyl formate, ethyl formate Esters, propyl formate, isopropyl formate, butyl formate, isobutyl formate, pentyl formate, isoamyl formate, methyl acetate, ethyl acetate, pentyl acetate, isoamyl acetate, hexyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, butyl propionate, isobutyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, isopropyl butyrate, butyl butyrate, isobutyl butyrate, ethyl hydroxyacetate, methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxy-2-methylpropionate, methyl 2-hydroxy-3-methylbutyrate, ethyl methoxyacetate, ethyl ethoxyacetate, 3-methyl The solvents include methyl 3-ethoxypropionate, ethyl 3-methoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl acetate, 3-methoxypropyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl propionate, 3-methyl-3-methoxybutyl butyrate, methyl acetoacetate, toluene, xylene, methyl ethyl ketone, methyl propyl ketone, methyl butyl ketone, 2-heptanone, 3-heptanone, 4-heptanone, cyclopentanone, cyclohexanone, N,N-dimethylformamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpyrrolidone, 4-methyl-2-pentanol, and γ-butyrolactone. These solvents may be used alone or in combination of two or more.

[0487] (3-3-2)

[0488] In addition, from the viewpoint of uniform solubility of the thermal acid generator, the self-crosslinking polymer [1], and further the optional components (aminoplast crosslinking agent or phenolic plastic crosslinking agent, etc.), the solvent is preferably a compound having an alcoholic hydroxyl group or a compound having a group capable of forming an alcoholic hydroxyl group. Preferred examples of such a solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, propylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monomethyl ... Glycol monomethyl ether acetate, propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, propylene glycol propyl ether acetate, cyclopentanone, cyclohexanone, ethyl 2-hydroxypropionate, methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate.

[0489] Among them, preferred are propylene glycol solvents (propylene glycol monomethyl ether, etc.), oxyisobutyrate solvents (methyl 2-hydroxy-2-methylpropionate, etc.), or butanediol solvents. Among them, further preferred are propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monopropyl ether acetate, methyl 2-hydroxy-2-methylpropionate, ethyl lactate, and cyclohexanone. Most preferred are propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl 2-hydroxy-2-methylpropionate, ethyl lactate, and cyclohexanone.

[0490] (3-3-3)

[0491] In addition, a solvent having a boiling point of 160° C. or higher may be contained. For example, the following compounds described in International Publication No. 2018 / 131562 (A1) can be used.

[0492]

[0493] (R in formula (i) 1 , R 2 and R 3 Each represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms which may be interrupted by an oxygen atom, a sulfur atom or an amide bond, and may be the same or different from each other and may be bonded to each other to form a ring structure.

[0494] Alternatively, 1,6-diacetoxyhexane (boiling point 260° C.), tripropylene glycol monomethyl ether (boiling point 242° C.) described in JP-A-2021-84974, and various high boiling point solvents described in paragraph 0082 of the publication can be preferably used.

[0495] Alternatively, dipropylene glycol monomethyl ether acetate (boiling point 213° C.), diethylene glycol monoethyl ether acetate (boiling point 217° C.), diethylene glycol monobutyl ether acetate (boiling point 247° C.), dipropylene glycol dimethyl ether (boiling point 171° C.), dipropylene glycol monomethyl ether (boiling point 187° C.), dipropylene glycol monobutyl ether (boiling point 231° C.), tripropylene glycol monomethyl ether (boiling point 231° C.) and dipropylene glycol monomethyl ether (boiling point 231° C.) can be preferably used. The present invention also includes various high boiling point solvents described in paragraphs 0023 to 0031 of the publication, such as propylene carbonate (boiling point 242°C), tetraethylene glycol dimethyl ether (boiling point 275°C), 1,6-diacetoxyhexane (boiling point 260°C), dipropylene glycol (boiling point 230°C), 1,3-butanediol diacetate (boiling point 232°C), and the like.

[0496] (3-4: other optional ingredients)

[0497] The resist underlayer film-forming composition according to the present invention may contain a crosslinking agent, a surfactant, a light absorber, a rheology regulator, an adhesion promoter, and the like in addition to the above-mentioned agents, as necessary.

[0498] (3-4-1: Aminoplast crosslinker)

[0499] As aminoplast crosslinking agents, there can be mentioned highly alkylated, alkoxylated, or alkoxyalkylated melamine, benzoguanamine, glycoluril, urea, polymers thereof, etc. Preferred crosslinking agents have at least two crosslinking-forming substituents, such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea, or methoxymethylated thiourea. In addition, condensates of these compounds can also be used.

[0500] As the crosslinking agent, a crosslinking agent with high heat resistance can be used. As the crosslinking agent with high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (for example, a benzene ring or a naphthalene ring) in the molecule can be preferably used.

[0501] It is preferably at least one selected from tetramethoxymethyl glycoluril and hexamethoxymethylmelamine.

[0502] The aminoplast crosslinking agent may be used alone or in combination of two or more. The aminoplast crosslinking agent may be produced by a known method or a method in accordance therewith, or a commercially available product may be used.

[0503] The amount of the aminoplast crosslinking agent used varies depending on the coating solvent used, the base substrate used, the required solution viscosity, the required film shape, etc., but is 0.001 mass % or more, 0.01 mass % or more, 0.05 mass % or more, 0.5 mass % or more, or 1.0 mass % or more, and 80 mass % or less, 50 mass % or less, 40 mass % or less, 20 mass % or less, or 10 mass % or less relative to the total solid content of the resist underlayer film forming composition as one embodiment of the present invention.

[0504] Some specific examples are as follows.

[0505]

[0506] (3-4-2: Phenolic plastic crosslinker)

[0507] Examples of the phenolic plastic crosslinking agent include highly alkylated, alkoxylated, or alkoxyalkylated aromatic compounds, and polymers thereof. Preferred crosslinking agents are those having at least two crosslinking substituents in one molecule, such as 2,6-dihydroxymethyl-4-methylphenol, 2,4-dihydroxymethyl-6-methylphenol, bis(2-hydroxy-3-hydroxymethyl-5-methylphenyl)methane, bis(4-hydroxy-3-hydroxymethyl-5-methylphenyl)methane, 2,2-bis(4-hydroxy-3,5-dihydroxymethylphenyl)propane, bis(3-formyl-4-hydroxyphenyl)methane, bis(4-hydroxy-2,5-dimethylphenyl)formylmethane, and α,α-bis(4-hydroxy-2,5-dimethylphenyl)-4-formyltoluene. Condensates of these compounds may also be used.

[0508] As the crosslinking agent, a crosslinking agent with high heat resistance can be used. As the crosslinking agent with high heat resistance, a compound containing a crosslinking-forming substituent having an aromatic ring (for example, a benzene ring or a naphthalene ring) in the molecule can be preferably used.

[0509] The phenolic plastic crosslinking agent may be used alone or in combination of two or more. The phenolic plastic crosslinking agent may be produced by a known method or a method in accordance therewith, or a commercially available product may be used.

[0510] The amount of the phenolic plastic crosslinking agent used varies depending on the coating solvent used, the base substrate used, the required solution viscosity, the required film shape, etc., but is 0.001 mass% or more, 0.01 mass% or more, 0.05 mass% or more, 0.5 mass% or more, or 1.0 mass% or more, and 80 mass% or less, 50 mass% or less, 40 mass% or less, 20 mass% or less, or 10 mass% or less relative to the total solid content of the resist underlayer film forming composition as one embodiment of the present invention.

[0511] Examples of such a compound include, in addition to the above, a compound having a partial structure of the following formula (4) and a polymer or oligomer having a repeating unit of the following formula (5).

[0512]

[0513] The above R 11 , R 12 , R 13 , and R 14 It is a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and the alkyl groups exemplified above can be used. n1 is an integer of 1 to 4, n2 is an integer of 1 to (5-n1), and (n1+n2) represents an integer of 2 to 5. n3 is an integer of 1 to 4, n4 is 0 to (4-n3), and (n3+n4) represents an integer of 1 to 4. The oligomer and polymer can be used in the range of 2 to 100 or 2 to 50 repeating unit structures.

[0514] Some specific examples are as follows.

[0515]

[0516] (3-4-3: Surfactants)

[0517] The resist underlayer film-forming composition as one embodiment of the present invention may contain a surfactant in order to prevent pinholes, streaks, and the like from being generated and to further improve coating properties on uneven surfaces.

[0518] Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkyl aryl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether, polyoxyethylene / polyoxypropylene block copolymers, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, and sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate. Non-ionic surfactants such as sugar alcohol tristearate, polyoxyethylene sorbitan fatty acid esters, etc., Etotron EF301, EF303, EF352 (Todo Co., Ltd. Manufactured by プロダクツ, trade name), メガファック F171, F173, R-30, R-40 (made by Dainippon Technology Co., Ltd., trade name), フロラード FC430, Fluorine-based surfactants such as FC431 (manufactured by Sumitomo Soft Arm (Co., Ltd.), Asahigard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (manufactured by Asahi Glass (Co., Ltd.), and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The amount of these surfactants mixed is usually 2.0% by mass or less, preferably 1.0% by mass or less, relative to the total solid content of the resist underlayer film-forming composition as one embodiment of the present invention. These surfactants may be added alone or in combination of two or more.

[0519] (3-4-4: Other additives)

[0520] In the resist underlayer film forming composition as one embodiment of the present invention, as a catalyst for promoting the crosslinking reaction, in addition to the crosslinking catalyst as the thermal acid generator of formula (1), an acidic compound such as citric acid, a thermal acid generator such as 2,4,4,6-tetrabromocyclohexadienonone, benzoin toluenesulfonate, 2-nitrobenzyl toluenesulfonate, other organic sulfonic acid alkyl esters, bis(4-tert-butylphenyl)iodide, etc. may be mixed. Trifluoromethanesulfonate, triphenylsulfonium trifluoromethanesulfonate, etc. Salt-based photoacid generators, halogen-containing compound-based photoacid generators such as phenyl-bis(trichloromethyl)-s-triazine, and sulfonic acid-based photoacid generators such as benzoin tosylate and N-hydroxysuccinimide trifluoromethanesulfonate.

[0521] As the light absorber, for example, commercially available light absorbers described in "Industrial Colorant Technology and Market" (published by CMC) and "Dye Handbook" (edited by the Society of Synthetic Organic Chemistry) can be suitably used, for example, CI Disperse Yellow 1, 3, 4, 5, 7, 8, 13, 23, 31, 49, 50, 51, 54, 60, 64, 66, 68, 79, 82, 88, 90, 93, 102, 114 and 124; CI Disperse Orange 1, 5, 13, 25, 29, 30, 31, 44, 57, 72 and 73; CI Disperse Red 1, 5, 7, 13, 17, 19, 43, 50, 54, 58, 65, 72, 73, 88, 117, 137, 143, 199 and 210; CI Disperse Violet 43; CI Disperse Blue 96; CI Fluorescent Brightener 112, 135 and 163; CI Solvent Orange 2 and 45; CI Solvent Red 1, 3, 8, 23, 24, 25, 27 and 49; CI Pigment Green 10; CI Pigment Brown 2, etc. The light absorber is usually blended in a ratio of 10% by mass or less, preferably 5% by mass or less, based on the total solid content of the resist underlayer film-forming composition according to the present invention.

[0522] The rheology modifier is mainly added for the purpose of improving the fluidity of the resist underlayer film-forming composition, especially in the baking process, to improve the uniformity of the film thickness of the resist underlayer film and to improve the filling property of the resist underlayer film-forming composition into the inside of the hole. As specific examples, phthalic acid derivatives such as dimethyl phthalate, diethyl phthalate, diisobutyl phthalate, dihexyl phthalate, butyl isodecyl phthalate, adipic acid derivatives such as di-n-butyl adipate, diisobutyl adipate, diisooctyl adipate, octyldecyl adipate, maleic acid derivatives such as di-n-butyl maleate, diethyl maleate, dinonyl maleate, oleic acid derivatives such as methyl oleate, butyl oleate, tetrahydrofurfuryl oleate, or stearic acid derivatives such as n-butyl stearate and glyceryl stearate can be cited. These rheology control agents are usually blended in a ratio of less than 30 mass % based on the total solid content of the resist underlayer film-forming composition according to the present invention.

[0523] The adhesion aid is mainly added for the purpose of improving the adhesion between the substrate or the resist and the resist underlayer film-forming composition, and particularly for the purpose of preventing the resist from peeling off during development. Specific examples include chlorosilanes such as trimethylchlorosilane, dimethylvinylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane; alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylvinylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole; silanes such as vinyltrichlorosilane, γ-chloropropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and γ-glycidoxypropyltrimethoxysilane; benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, and 2-mercaptobenzothiazole. Heterocyclic compounds such as azole, urea, thiouracil, mercaptoimidazole, and mercaptopyrimidine, ureas such as 1,1-dimethylurea and 1,3-dimethylurea, or thiourea compounds. These adhesion promoters are usually mixed in a ratio of less than 5% by mass, preferably less than 2% by mass, relative to the total solid content of the resist underlayer film forming composition of the present invention.

[0524] The solid content of the resist underlayer film forming composition as one embodiment of the present invention is 0.1 to 70 mass %, or 0.1 to 60 mass %. The solid content is the content ratio of all components after removing the solvent from the resist underlayer film forming composition. The crosslinkable resin can be contained in the solid content at a ratio of 1 to 99.9 mass %, or 50 to 99.9 mass %, or 50 to 95 mass %, or 50 to 90 mass %.

[0525] [4: Resist underlayer film

[16] ]

[0526] The resist underlayer film can be formed as follows using the resist underlayer film-forming composition [7] which is one embodiment of the present invention.

[0527] The resist underlayer film forming composition [7] as one embodiment of the present invention is applied to a substrate used in the manufacture of a semiconductor device (e.g., a silicon wafer substrate, a silicon dioxide coated substrate (SiO2 substrate), a silicon nitride substrate (SiN substrate), a silicon oxide nitride substrate (SiON substrate), a titanium nitride substrate (TiN substrate), a tungsten substrate (W substrate), a glass substrate, an ITO substrate, a polyimide substrate, and a low dielectric constant material (low-k material) coated substrate) by an appropriate coating method such as a spin coater or a coater, and then fired using a heating means such as a hot plate to form a resist underlayer film. The firing conditions are appropriately selected from a firing temperature of 80°C to 600°C and a firing time of 0.3 to 60 minutes. Preferably, the firing temperature is 150°C to 400°C, more preferably 150°C to 350°C, and the firing time is 0.5 to 2 minutes. As the atmosphere gas during firing, air can be used, or an inert gas such as nitrogen or argon can be used. In one embodiment, the oxygen concentration is preferably 1% or less. Here, the thickness of the formed lower film is, for example, 10 to 1000 nm, or 20 to 500 nm, or 30 to 400 nm, or 50 to 300 nm. In addition, if a quartz substrate is used as the substrate, a replica of the quartz imprint mold (mold replica) can be made.

[0528] In addition, a close-fitting layer and / or an organosilicon layer containing less than 99% by mass or less than 50% by mass of Si can also be formed by coating or vapor deposition on the resist underlayer film as one embodiment of the present invention. For example, in addition to the close-fitting layer described in Japanese Unexamined Patent Publication No. 2013-202982, Japanese Patent No. 5827180, and the resist underlayer film (inorganic resist underlayer film) containing silicon described in International Publication No. 2009 / 104552 (A1) being formed by spin coating with a composition, an inorganic material film of Si system can also be formed by CVD method etc.

[0529] In addition, by applying the composition for forming an anti-etching underlayer film [7] which is one embodiment of the present invention onto a semiconductor substrate having a portion with a height difference and a portion without a height difference (so-called height difference substrate) and firing it, the height difference between the portion with a height difference and the portion without a height difference can be reduced.

[0530] [5: Method for manufacturing a semiconductor device

[18] to

[21] ]

[0531] (5-1)

[0532] (i) A method for manufacturing a semiconductor device as one embodiment of the present invention includes the following steps:

[0533] A step of forming a resist underlayer film using the resist underlayer film-forming composition [7] which is one embodiment of the present invention;

[0534] a step of forming a resist film on the formed resist underlayer film;

[0535] A step of forming a resist pattern by irradiating the formed resist film with light or electron beams and developing the film;

[0536] A step of etching the resist underlayer film through the formed resist pattern to perform patterning; and

[0537] A step of processing a semiconductor substrate through a patterned resist underlayer film.

[0538] (ii) In addition, a method for manufacturing a semiconductor device as one embodiment of the present invention includes the following steps:

[0539] A step of forming a resist underlayer film using the resist underlayer film-forming composition [7] which is one embodiment of the present invention;

[0540] forming a hard mask on the formed resist underlayer film;

[0541] forming a resist film on the formed hard mask;

[0542] a step of forming a resist pattern by irradiating the formed resist film with light or electron beams and developing the film, and a step of etching the hard mask through the formed resist pattern to perform patterning; and

[0543] A step of etching the resist underlayer film through the patterned hard mask to perform patterning; and

[0544] A step of processing a semiconductor substrate through a patterned resist underlayer film.

[0545] (iii) In addition, a method for manufacturing a semiconductor device as one embodiment of the present invention includes the following steps:

[0546] A step of forming a resist underlayer film using the resist underlayer film-forming composition [7] which is one embodiment of the present invention;

[0547] forming a hard mask on the resist underlayer film;

[0548] A step of further forming a resist film on the hard mask;

[0549] A process of forming a resist pattern by irradiation with light or electron beams and development;

[0550] A process of etching the hard mask using the formed resist pattern;

[0551] A step of etching the resist underlayer film using the patterned hard mask;

[0552] A process of removing the hard mask; and

[0553] A step of processing a semiconductor substrate using a patterned resist underlayer film.

[0554] (iv) In addition, a method for manufacturing a semiconductor device as one embodiment of the present invention includes the following steps:

[0555] A step of forming a resist underlayer film using the resist underlayer film-forming composition [7] which is one embodiment of the present invention;

[0556] forming a hard mask on the resist underlayer film;

[0557] A step of further forming a resist film on the hard mask;

[0558] A process of forming a resist pattern by irradiation with light or electron beams and development;

[0559] A process of etching the hard mask using the formed resist pattern;

[0560] A step of etching the resist underlayer film using the patterned hard mask;

[0561] A process of removing the hard mask; and

[0562] A step of forming a vapor-deposited film (spacer) on the resist underlayer film after the hard mask is removed;

[0563] A process of processing the vapor-deposited film (spacer) by etching;

[0564] A step of removing the patterned resist underlayer film to leave the patterned vapor-deposited film (spacer); and

[0565] A step of processing a semiconductor substrate via a patterned vapor-deposited film (spacer).

[0566] (5-2)

[0567] The step of forming a resist underlayer film using the resist underlayer film-forming composition which is one embodiment of the present invention is as described in the above-mentioned [4: Resist underlayer film

[16] ].

[0568] A hard mask such as a film containing silicon can be formed on the resist underlayer film formed by the above-mentioned process as a second resist underlayer film, and a resist pattern can be formed thereon. The second resist underlayer film can be a coating film, or a SiON film, a SiN film, or a SiO2 film formed by a vapor deposition method such as CVD or PVD. Further, an anti-reflection film (BARC) can be formed on the second resist underlayer film as a third resist underlayer film, and the third resist underlayer film can be a resist shape correction film without anti-reflection capability.

[0569] In the above-mentioned process of forming the resist pattern, exposure is carried out by being used to form a mask (photomask) of a prescribed pattern or by directly describing. For exposure source, for example, g-rays, i-rays, KrF excimer lasers, ArF excimer lasers, EUV, electron beams can be used. After exposure, post-exposure heating (Post Exposure Bake) is carried out as required. Then, development is carried out by developer (for example 2.38% by mass tetramethylammonium hydroxide aqueous solution, butyl acetate), further washed with rinse solution or pure water, and the developer used is removed. Then, post-baking is carried out for the drying of the resist pattern and the adhesion with substrate of improvement.

[0570] The etching process performed after the formation of the above-mentioned resist pattern is performed by dry etching. As the etching gas used for dry etching, for the second resist underlayer film (organopolysiloxane film), CHF3, CF4, C2F6 can be mentioned, for example, O2, N2O, NO2 can be mentioned for the first resist underlayer film formed by the resist underlayer film forming composition of the present invention, and for the surface having a height difference or concave and / or convex portion, CHF3, CF4, C2F6 can be mentioned. Furthermore, argon gas, nitrogen gas or carbon dioxide can be mixed in these gases and used.

[0571] (5-3)

[0572] The resist film may be patterned by a nanoimprint method or a self-assembled film method.

[0573] For the nanoimprint method, the resist composition is molded using a mold (mold) that is transparent and patterned relative to the irradiated light. In addition, for the self-assembled film method, a self-assembled film of a regular structure of nanometer level is naturally formed using diblock polymers (polystyrene-polymethyl methacrylate, etc.) and the like to carry out patterning.

[0574] In the nanoimprint method, before applying the curable composition that becomes the resist film, a silicon layer (hard mask layer) can be optionally formed on the resist underlayer film by coating or vapor deposition, and further a bonding layer can be formed on the resist underlayer film or on the silicon layer (hard mask layer) by coating or vapor deposition, and the curable composition that becomes the resist film is applied on the bonding layer.

[0575] (5-4)

[0576] It should be noted that wet etching is sometimes performed for the purpose of simplifying the process and reducing damage to the processed substrate. This results in suppressing the change in processing dimensions and reducing pattern roughness, and the substrate can be processed with a good yield. Therefore, in the above (5-1)(iii)(iv), the hard mask can also be removed by either etching or alkaline liquid. In particular, when using an alkaline liquid, although there is no restriction on the components, it is preferred that the following be included as the alkaline component.

[0577] Examples of the alkali component include tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, methyltripropylammonium hydroxide, methyltributylammonium hydroxide, ethyltrimethylammonium hydroxide, dimethyldiethylammonium hydroxide, benzyltrimethylammonium hydroxide, hexadecyltrimethylammonium hydroxide, (2-hydroxyethyl)trimethylammonium hydroxide, monoethanolamine, diethanolamine, triethanolamine, 2-(2-aminoethoxy)ethanol, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-dibutylethanolamine, N -methylethanolamine, N-ethylethanolamine, N-butylethanolamine, N-methyldiethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, tetrahydrofurfurylamine, N-(2-aminoethyl)piperazine, 1,8-diazabicyclo[5.4.0]undecene-7, 1,4-diazabicyclo[2.2.2]octane, hydroxyethylpiperazine, piperazine, 2-methylpiperazine, trans-2,5-dimethylpiperazine, cis-2,6-dimethylpiperazine, 2-piperidinol, cyclohexylamine, 1,5-diazabicyclo[4,3,0]nonene-5, etc. In addition, from the viewpoint of handling, tetramethylammonium hydroxide and tetraethylammonium hydroxide are particularly preferred, and an inorganic base can be used in combination with a quaternary ammonium hydroxide. As the inorganic base, an alkali metal hydroxide such as potassium hydroxide, sodium hydroxide, and rubidium hydroxide is preferred, and potassium hydroxide is more preferred.

[0578] Example

[0579] [Synthesis of polymer]

[0580] The following compound group A, compound group B, catalyst group C, solvent group D, and reprecipitation solvent group E were used to synthesize the structural formulas (S1) to (S12) of the polymers before introduction of alkoxymethyl groups such as MOM groups (methoxymethyl groups).

[0581] ○Compound Group A~B

[0582]

[0583] ○Catalyst group C, solvent group D, reprecipitation solvent group E

[0584] Methanesulfonic acid: C1

[0585] 3-Mercaptopropionic acid: C2

[0586] 1,4-di Alkane: D1

[0587] 4-Methyltetrahydrofuran (MTHP): D2

[0588] Propylene glycol monomethyl ether acetate (=PGMEA): D3

[0589] Methanol: E1

[0590] Water: E2

[0591] [Synthesis example 1]

[0592] In a flask, 18.0 g of carbazole, 16.8 g of 1-naphthaldehyde, 8.28 g of methanesulfonic acid, 0.9 g of 3-mercaptopropionic acid, and 1,4-dihydro- 100.5 g of alkane was added. Then, the mixture was reacted for about 2 hours under reflux in a nitrogen atmosphere. After the reaction was stopped, the mixture was reprecipitated with methanol and dried to obtain a resin (S1). The weight average molecular weight Mw measured by GPC in terms of polystyrene was about 3,170.

[0593]

[0594] [Synthesis Examples 1 to 12]

[0595] Polymers before introduction of MOM groups were synthesized by variously changing compound group A, compound group B, catalyst group C, solvent group D, and reprecipitation solvent group E. It should be noted that the experimental operation was the same as that of Synthesis Example 1. Polymers (S1) to (S12) were synthesized under the following conditions.

[0596] [Table 1]

[0597]

[0598]

[0599] [Synthesis of MOM group-introduced polymer]

[0600] The synthesis of the MOM group-introduced polymers of the structural formulas (SM1) to (SM11) used as the resist underlayer film was carried out by utilizing the introduction reaction of the MOM group into the polymers (S1) to (S11).

[0601] [Synthesis Example 13]

[0602] Add 5.0 g of polymer (S1) and 20.0 g of N,N-dimethylformamide to a flask and cool it to 0°C with an ice bath. Next, add 0.7 g of sodium hydride (55%) and 1.3 g of chloromethyl methyl ether, and stir for about 30 minutes. Then, take it out of the ice bath, slowly heat it to room temperature while aging for 22 hours. After the reaction stops, reprecipitate it with methanol and dry it to obtain a resin (SM1). The weight average molecular weight Mw measured by GPC in terms of polystyrene is about 3,572. The obtained resin is dissolved in PGMEA or cyclohexanone (CYH), and ion exchange is performed for 4 hours using a cation exchange resin and an anion exchange resin to obtain the target compound solution.

[0603]

[0604] [Synthesis Examples 13 to 23]

[0605] The amount of solvent and the amount of alkali were variously changed to synthesize a MOM group-introduced polymer used for the resist underlayer film. It should be noted that the experimental operation was the same as that of Synthesis Example 12. The MOM group-introduced polymers (SM1) to (SM11) were synthesized under the following conditions.

[0606] [Table 2]

[0607]

[0608]

[0609] [Preparation of Resist Underlayer Film]

[0610] Polymers (SM1) to (SM11) or polymers (S1) to (S12), solvents (propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone (CYH), crosslinking agents (CR1 to CR2), acid generators (Ad1), and Megaff R-30NML (manufactured by DIC Corporation, F1) as a surfactant are mixed in the weight proportions shown in the following table (for components other than the solvent, the relative weight is the polymer when it is set to 100 g; for the solvent, the relative weight of each solvent when the total amount of the solvent is set to 100 g), and filtered using a 0.1 μm polytetrafluoroethylene microfilter to prepare anti-etching agent underlayer film materials (M1 to M13, comparison M1 to comparison M14).

[0611]

[0612] [Table 3-1]

[0613]

[0614] [Table 3-2]

[0615]

[0616] [Dissolution test into resist solvent]

[0617] The resist lower film material of the embodiment was coated on a silicon wafer using a spin coater, and fired for 60 seconds to form a resist lower film in a manner that the film thickness became 65nm. After the formed resist lower film was immersed in PGME (propylene glycol monomethyl ether) / PGMEA=7 / 3 as a general diluent for 60 seconds, it was fired for 30 seconds at 100°C. By comparing the film thickness before and after the diluent immersion, the firing temperature that exhibits resistance to solvents was confirmed. The comparative example was fired for 60 seconds at a firing temperature that exhibits solvent resistance and a resist lower film was formed in a manner that the film thickness became 65nm, and the operation was performed in the same manner as the above method, thereby confirming resistance to solvents. In the case where self-crosslinking is imparted to the polymer by introducing the MOM group, compared with the polymer into which the MOM group is not introduced, resistance to solvents is exhibited at low temperatures. The firing temperature when the reduction rate of the film thickness before and after the diluent immersion becomes less than 1% is judged to be 0 compared to the comparative example for a low temperature.

[0618] In addition, the above-mentioned lower film material was coated on a silicon wafer using ACT-8 manufactured by Tokyo Elektronik Co., Ltd., and fired at the specified temperature / prescribed time recorded in the table under nitrogen to form a 65nm resist lower film. After immersion in PGME / PGMEA=7 / 3 for 60 seconds as described above, it was fired at 100°C for 30 seconds. By comparing the film thickness before and after diluent immersion, resistance to solvents was confirmed. The reduction rate of the film thickness before and after diluent immersion was judged to be smaller than that of the comparative example as 0 (Table 1).

[0619] [Table 4]

[0620] (Table 1)

[0621]

[0622] By confirming above that self-crosslinking can be given by introducing MOM group to the polymer that does not have self-crosslinking.It should be noted that, when fired under the atmosphere as general firing conditions, the sample (Comparative Examples 1-10) with large dissolution to the resist solvent cannot be used as the resist lower layer film.Therefore, in the evaluation later as comparative examples, comparative examples 11-13 were used.

[0623] [Measurement of optical constants]

[0624] The solution of the resist underlayer film forming composition prepared in the comparative example and the embodiment was coated on a silicon wafer using a spin coater. The prescribed temperature / prescribed time recorded in the table was fired on a hot plate to form a resist underlayer film with a film thickness of 50 nm. The refractive index (n value) and optical absorption coefficient (also referred to as k value, attenuation coefficient) of these resist underlayer films at a wavelength of 193 nm were measured using a spectroscopic ellipsometer (Table 2).

[0625] [Table 5]

[0626] (Table 2)

[0627]

[0628] [Measurement of etching rate]

[0629] The resist lower film material of the comparative example and the embodiment was coated on a silicon wafer using a spin coater. The prescribed temperature / prescribed time recorded in the table was fired on a hot plate to form a 65nm resist lower film. The dry etching rate was measured using O2 / N2 gas or CF4 gas as the etching gas (Table 3). The situation where the etching rate was slow relative to the comparative example was judged as 0, and the situation where it was fast was judged as ×.

[0630] The etcher and etching gas used in the etching measurement were as follows.

[0631] RIE-200NL (manufactured by SAMU): CF4 50sccm

[0632] RIE-200NL (manufactured by SAMU): O2 / N2 10sccm / 200sccm

[0633] [Table 6]

[0634] (Table 3)

[0635]

[0636] [Coating and Coverage Test on Height Difference Substrates]

[0637] As a coating test to a high-low substrate, a SiO2 substrate with a film thickness of 100nm was used. In the case of a high-low substrate, the coating property of the resist lower film sometimes deteriorates depending on the type of substrate. Therefore, a test was conducted on whether the high-low substrate can be coated without uneven coating. The situation where the coating can be coated without uneven coating was judged to be 0. The groove area (dense pattern area) with a groove width of 50nm and a spacing of 100nm in the above-mentioned substrate was evaluated for flattening. The coating thickness of the dense area and the area (open area) where no pattern is formed was compared. After the resist lower film forming composition modulated in the comparative example and the embodiment was applied to the above-mentioned substrate, the prescribed temperature / prescribed time recorded in the table was fired on a hot plate to form a 65nm resist lower film. The flattening property of the substrate was observed using a scanning electron microscope (S-4800) manufactured by Hitachi HiTech Nologiz (KK), and the film thickness difference between the groove area (pattern part) and the open area (no pattern part) of the height difference substrate was measured (the coating height difference between the groove area and the open area is called deviation) to evaluate the flattening property. Here, the so-called flattening property means that the film thickness difference (Iso-dense deviation) of the coated coating existing on the upper part of the part with pattern (groove area (pattern part)) and the part without pattern (open area (no pattern part)) is small. The case where the deviation is improved relative to the comparative example is judged as ○ (Table 4).

[0638] [Table 7]

[0639] (Table 4)

[0640] Examples / Comparative Examples Composition Film thickness Firing temperature Substrate Type Coating properties Planarization Example 2 M3 65nm 350℃ / 60sec <![CDATA[SiO2]]> ○ ○ Example 3 M5 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ ○ Example 5 M4 65nm 350℃ / 60sec <![CDATA[SiO2]]> ○ ○ Example 7 M8 65nm 400℃ / 60sec <![CDATA[SiO2]]> ○ ○ Example 8 M10 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ ○ Example 9 M9 65nm 400℃ / 60sec <![CDATA[SiO2]]> ○ ○ Example 10 M11 65nm 24℃ / 60sec <![CDATA[SiO2]]> ○ ○ Embodiment 11 M12 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ ○ Example 12 M13 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ ○ Comparative Example 11 Compare M12 65nm 400℃ / 60sec <![CDATA[SiO2]]> ○ × Comparative Example 12 Compare M13 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ × Comparative Example 13 Compare M14 65nm 400℃ / 60sec <![CDATA[SiO2]]> ○ ×

[0641] [Test of embedding properties into uneven substrates]

[0642] As a coating test on a high-low substrate, a SiO2 substrate with a film thickness of 100nm was used. The embedding property was evaluated for the groove area (dense pattern area) with a groove width of 50nm and a spacing of 100nm in the above-mentioned substrate. After the resist lower film forming composition prepared in the comparative example and the embodiment was applied to the above-mentioned substrate, it was sintered at the specified temperature / specified time recorded in the table on a hot plate to form a 65nm resist lower film. The embedding property of the substrate was observed using a scanning electron microscope (S-4800) manufactured by Hitachi High-Tech Nologis Co., Ltd. The situation where the resist lower film was filled to the bottom of the groove was judged to be embedding property ○ (Table 5).

[0643] [Table 8]

[0644] (Table 5)

[0645] Examples / Comparative Examples Composition Film thickness Firing temperature Substrate Type Embedment Example 1 M1 65nm 350℃ / 60sec <![CDATA[SiO2]]> ○ Example 2 M3 65nm 350℃ / 60sec <![CDATA[SiO2]]> ○ Example 3 M5 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ Example 4 M2 65nm 350℃ / 60sec <![CDATA[SiO2]]> ○ Example 5 M4 65nm 350℃ / 60sec <![CDATA[SiO2]]> ○ Example 7 M8 65nm 400℃ / 60sec <![CDATA[SiO2]]> ○ Example 8 M10 65nm 940℃ / 60sec <![CDATA[SiO2]]> ○ Example 9 M9 65nm 400℃ / 60sec <![CDATA[SiO2]]> ○ Example 10 M11 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ Embodiment 11 M12 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ Example 12 M13 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ Comparative Example 11 Compare M12 65nm 400℃ / 60sec <![CDATA[SiO2]]> ○ Comparative Example 12 Compare M13 65nm 240℃ / 60sec <![CDATA[SiO2]]> ○ Comparative Example 13 Compare M14 65mm 400℃ / 60sec <![CDATA[SiO2]]> ○

[0646] [Sublimation amount measurement]

[0647] The amount of sublimation was measured using a sublimation amount measuring device described in International Publication No. 2007 / 111147. The resist underlayer film-forming compositions prepared in the comparative examples and the examples were applied to silicon wafers, and the amount of sublimation when the film thickness reached 65 nm after firing at 300° C. for 60 seconds was measured. When the amount of sublimation was less than that of the comparative example, it was judged as ○ (Table 6).

[0648] [Table 9]

[0649] (Table 6)

[0650] Examples / Comparative Examples Composition Firing temperature Sublimation amount Example 1 M1 300℃ / 60sec ○ Example 2 M3 300℃ / 60sec ○ Example 3 M5 300℃ / 60sec ○ Example 4 M2 300℃ / 60sec ○ Example 5 M4 300℃ / 60sec ○ Example 6 M6 300℃ / 60sec ○ Example 7 M8 300℃ / 60sec ○ Example 8 M10 300℃ / 60sec ○ Example 9 M9 300℃ / 60sec ○ Example 10 M11 300℃ / 60sec ○ Embodiment 11 M12 300℃ / 60sec ○ Example 12 M13 300℃ / 60sec ○ Comparative Example 13 Compare M14 300℃ / 60sec ×

[0651] As mentioned above, the material of the embodiment is different from the previous material, and even if it does not contain a cross-linking agent or a curing catalyst, it also shows curability in the atmosphere and in nitrogen, so it can be judged to have self-cross-linking property. Of course, it can also be used by containing a cross-linking agent and a curing catalyst in the same way as before. In addition, this material can freely change the optical constants and etching resistance by changing the polymer species skeleton, and can suppress reflection during exposure, so a good resist pattern can be formed. In addition, the fluorine or oxygen gas as the main etching gas shows better etching resistance than the comparative example. Further, even on various vapor-deposited films, it also shows good coating properties, and the embedding and flattening properties to fine height difference substrates are also good. In addition, since the amount of sublimation is also small, it is a material with less device pollution. Therefore, it is expected to become a material that can be widely used in diversified semiconductor manufacturing processes.

Claims

1. A self-crosslinking polymer comprising: (A) one or more unit structures A having an aromatic ring; and (B) one or more unit structures B as organic groups having one or more connecting carbon atoms, At least one of the unit structures A is: (i) a unit structure comprising at least two aromatic rings connected by at least one -NR- bond, (ii) a unit structure comprising a heterocyclic ring having at least one -NR- bond as a ring constituent, and when the heterocyclic ring is not an aromatic heterocyclic ring, the heterocyclic ring forms a condensed ring with a first aromatic ring and / or the heterocyclic ring is substituted with a substituent comprising a second aromatic ring, or (iii) a unit structure comprising at least one aromatic ring having at least one -NR2 substituent, The R is a hydrogen atom or an alkoxymethyl group, and at least a portion of the R groups in all polymers are alkoxymethyl groups. The connecting carbon atom is a carbon atom in the unit structure B that forms a covalent bond with the aromatic ring in the unit structure A and is a carbon atom that does not constitute the aromatic ring. 2 . The self-crosslinking polymer according to claim 1 , which is a novolac resin.

3. The self-crosslinkable polymer according to claim 1, wherein the unit structure A is selected from the following unit structures (I-1) to (I-5) and positional isomers thereof, The above (I-1) to (I-5) may further optionally have a substituent. In (I-1) to (I-5), R is the same as defined in [1], In the above (I-1), each Ar is the same or different and represents an aromatic ring which may have a substituent. In (I-2) to (I-5), represents an aromatic ring part in a fused ring which may have a substituent, and each of them may be the same as or different from each other, In (I-4), X represents CR 1 R 2 , O, S or NR'; R' is the same as the definition of R in claim 1, and may be the same as or different from R in the chemical formula (I-4); R 1 and R 2 are the same as or different from each other and are aromatic ring residues or aliphatic hydrocarbon groups having 1 to 3 carbon atoms, In (I-5) represents a heterocyclic moiety in a fused ring compound which may have a substituent, Y is a substituent including an aromatic ring, and may be a substituent of any of the aromatic ring part and the heterocyclic part.

4. The self-crosslinking polymer according to claim 1, wherein the unit structure B is a unit structure comprising a structure represented by (II), (III) or (IV) below, In formula (II), R and R' each independently represent a hydrogen atom, an aromatic ring residue having 6 to 30 carbon atoms which may have a substituent, a heterocyclic residue having 3 to 30 carbon atoms which may have a substituent, or a linear, branched or cyclic alkyl group having 10 or less carbon atoms which may have a substituent; In formula (III), Z is a monocyclic, bicyclic, tricyclic or tetracyclic condensed ring having 4 to 25 carbon atoms and optionally having a substituent, wherein the monocyclic ring is a non-aromatic monocyclic ring; at least one of the monocyclic rings constituting the bicyclic, tricyclic and tetracyclic rings is a non-aromatic monocyclic ring, and the remaining monocyclic rings may be either aromatic or non-aromatic, and the monocyclic, bicyclic, tricyclic or tetracyclic condensed ring may further form a condensed ring with one or more aromatic rings to form a condensed ring of at least five rings, X and Y are the same or different, indicating -CR 31 R 32 -Base, R 31 and R 32 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, x and y each represent the number of X and Y, and each independently represents 0 or 1. *-X x is bonded to any carbon atom of the non-aromatic monocyclic ring constituting Z, that is, "carbon atom 1", that is, when x=1, or extends from carbon atom 1, that is, when x=0, Y y -* is bonded to any carbon atom of the non-aromatic monocyclic ring constituting Z, i.e., "carbon atom 2", i.e., y=1, or extends from carbon atom 2, i.e., y=0, The carbon atom 1 and the carbon atom 2 may be the same or different, and in different cases, may belong to the same non-aromatic monocyclic ring or to different non-aromatic monocyclic rings. * indicates a bonding bond; -J 1 -Z 0 -J 2 - (IV) In formula (IV), Z 0 represents an aromatic ring residue or an aliphatic ring residue having 6 to 30 carbon atoms which may have a substituent, or an organic group in which two aromatic ring residues or aliphatic ring residues are linked by a single bond, J 1 and J 2 Each independently represents a divalent organic group which is directly bonded or may have a substituent.

5. The resist underlayer film forming composition according to claim 4, wherein the formula (III) is the following formula (III-1): In formula (III-1), Z is a 4-17 membered monocyclic, bicyclic, tricyclic or tetracyclic organic group which may have a substituent, wherein the monocyclic ring is a non-aromatic monocyclic ring; at least one of the monocyclic rings constituting the bicyclic, tricyclic and tetracyclic rings is a non-aromatic monocyclic ring, and the remaining monocyclic rings may be either aromatic or non-aromatic. One or more aromatic rings may be further fused or fused with the monocyclic, bicyclic, tricyclic and tetracyclic organic groups to form a pentacyclic or higher ring. C and C' each represent a carbon atom in the group of atoms constituting the cyclic portion of any non-aromatic monocyclic ring of Z, and the non-aromatic monocyclic rings to which C and C' belong may be the same or different, n is the number of carbon atoms C', representing an integer from 0 to 2, p, q, p', q' represent the number of bonding bonds, and each independently represents 0 or 1. When n is 0, p and q are 1, When n is 1 or 2, at least one of p and q is 1, and at least one of p' and q' of each C' is 1, When n is 2, the non-aromatic monocyclic rings to which the two C's belong may be the same or different. If they are the same, the two C's may be directly bonded or not. X, Y, X', Y' are the same or different, indicating -CR 1 R 2 -Base, R 1 and R 2 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 3 carbon atoms. When n is 2, the two X's may be the same or different, and the two Y's may be the same or different. x, y, x', and y' each represent the number of X, Y, X', and Y', and each independently represents 0 or 1.

6. The self-crosslinking polymer according to claim 1, wherein the terminal group of the self-crosslinking polymer is an aromatic ring residue having 6 to 30 carbon atoms which may have a substituent, an unsaturated hydrocarbon group having 1 to 10 carbon atoms which may have a substituent, a hydroxyl group or a hydrogen atom. 7 . A resist underlayer film-forming composition comprising a thermal acid generator, the self-crosslinking polymer according to claim 1 , and a solvent. 8 . The resist underlayer film-forming composition according to claim 7 , further comprising a cross-linking agent. 9 . The resist underlayer film-forming composition according to claim 8 , wherein the crosslinking agent is an aminoplast crosslinking agent or a phenoplast crosslinking agent.

10. The resist underlayer film-forming composition according to claim 9, wherein the aminoplast crosslinking agent is highly alkylated, alkoxylated or alkoxyalkylated melamine, benzoguanamine, glycoluril, urea, or a polymer thereof.

11. The resist underlayer film-forming composition according to claim 9, wherein the phenolic plastic crosslinking agent is a highly alkylated, alkoxylated or alkoxyalkylated aromatic compound, or a polymer thereof. 12 . The resist underlayer film-forming composition according to claim 7 , wherein the solvent is a compound having an alcoholic hydroxyl group or a compound having a group capable of forming an alcoholic hydroxyl group. 13 . The resist underlayer film-forming composition according to claim 12 , wherein the compound having an alcoholic hydroxyl group or the compound having a group capable of forming an alcoholic hydroxyl group is a propylene glycol-based solvent, an oxyisobutyrate-based solvent, or a butanediol-based solvent.

14. The resist underlayer film-forming composition according to claim 12, wherein the compound having an alcoholic hydroxyl group or the compound having a group capable of forming an alcoholic hydroxyl group is propylene glycol monomethyl ether, cyclohexanone, propylene glycol monomethyl ether acetate, ethyl lactate or methyl 2-hydroxy-2-methylpropionate. 15 . The resist underlayer film forming composition according to claim 7 , further comprising a surfactant. 16 . A resist underlayer film which is a fired product of a coating film formed from the resist underlayer film-forming composition according to claim 7 on a semiconductor substrate. 17 . A method for forming a resist pattern for producing a semiconductor, comprising the step of applying the resist underlayer film-forming composition according to claim 7 on a semiconductor substrate and firing the composition to form a resist underlayer film.

18. A method for manufacturing a semiconductor device, comprising the following steps: A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition according to any one of claims 7 to 15; forming a resist film on the resist underlayer film; A process of forming a resist pattern by irradiation with light or electron beams and development; a step of etching the resist underlayer film using the formed resist pattern; and A step of processing a semiconductor substrate using a patterned resist underlayer film.

19. A method for manufacturing a semiconductor device, comprising the following steps: A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition according to any one of claims 7 to 15; forming a hard mask on the resist underlayer film; A step of further forming a resist film on the hard mask; A process of forming a resist pattern by irradiation with light or electron beams and development; A process of etching the hard mask using the formed resist pattern; A step of etching the resist underlayer film using the patterned hard mask; as well as A step of processing a semiconductor substrate using a patterned resist underlayer film.

20. A method for manufacturing a semiconductor device, comprising the following steps: A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition according to any one of claims 7 to 15; forming a hard mask on the resist underlayer film; A step of further forming a resist film on the hard mask; A process of forming a resist pattern by irradiation with light or electron beams and development; A process of etching the hard mask using the formed resist pattern; A step of etching the resist underlayer film using the patterned hard mask; A process of removing the hard mask; as well as A step of processing a semiconductor substrate using a patterned resist underlayer film.

21. A method for manufacturing a semiconductor device, comprising the following steps: A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition according to any one of claims 7 to 15; forming a hard mask on the resist underlayer film; A step of further forming a resist film on the hard mask; A process of forming a resist pattern by irradiation with light or electron beams and development; A process of etching the hard mask using the formed resist pattern; A step of etching the resist underlayer film using the patterned hard mask; A process of removing the hard mask; A step of forming a vapor-deposited film, i.e., a spacer, on the resist underlayer film after the hard mask is removed; A process of processing the vapor deposited film, i.e., the spacer, by etching; A step of removing the patterned resist underlayer film to leave the patterned vapor-deposited film, i.e., the spacer; and A process of processing a semiconductor substrate via a patterned vapor-deposited film, i.e., a spacer. 22 . The manufacturing method according to claim 19 , wherein the hard mask is formed by coating or vapor deposition of an inorganic material. 23 . The production method according to claim 18 , wherein the resist film is patterned by a nanoimprint method or a self-assembled film.

24. The method for manufacturing a semiconductor device according to claim 20 or 21, wherein the hard mask is removed by either etching or an alkaline chemical solution.