Hot-rolled steel sheet, method for producing same, electric-welded steel pipe, and method for producing

By controlling the microstructure and process of steel plates and steel pipes, the problem of insufficient processability and low-temperature toughness of steel pipes in the prior art is solved, and high-strength and excellent processability of mechanical structural steel pipes and steel plates are realized, suitable for automobiles, construction machinery and industry mechanical.

CN118974293APending Publication Date: 2024-11-15JFE STEEL CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202280094537.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-06
Filing Date
2022-12-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, after the strength and toughness of the steel pipes for mechanical structures have room to improve their machining properties and the machining properties of the resistance welded parts, especially when used in low temperature environments.

Method used

By controlling the microstructure of steel plates and steel pipes, ensuring that the volume ratio of bainite reaches more than 90%, limiting the ratio of Ti-based inclusions and other tissues, optimizing the cooling and hot rolling process, and preparing high yield stress and tensile strength Hot-rolled steel plates and welded steel pipes, and toughness and processability are improved through heat treatment of resistance welding parts.

Benefits of technology

It achieves high strength, excellent processability and toughness in automotive, construction machinery and industrial machinery applications, and steel pipes and steel plates that adapt to low temperature environments, improving the overall performance of the components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974293A_ABST
    Figure CN118974293A_ABST
Patent Text Reader

Abstract

Provided is a hot-rolled steel sheet which is a base material for an electric-welded steel pipe that has high strength and excellent workability and toughness, and is suitable for use as a steel pipe for a mechanical structure used in components for automobiles, construction machines, and industrial machines. The hot-rolled steel sheet has a prescribed component composition, has a steel structure in the center of the sheet thickness in which the volume fraction of bainite is 90% or more and the remainder comprises one or more of ferrite, pearlite, martensite and austenite, and has an average crystal grain size of 10.0 [mu] m or less and a grain size of 10.0 [mu] m or less in the steel structure in the center of the sheet thickness. The volume fraction of crystal grains having a grain diameter of 40.0 [mu] m or more is 40% or less, and the number density of Ti-based inclusions having a major diameter of 5.0 [mu] m or more is 20 / mm2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electric-resistance welded steel pipe suitable for use as a machine structure steel pipe for use in parts of automobiles, construction machinery, and industrial machinery, a hot-rolled steel plate as a base material thereof, and methods for producing the same. Background Art

[0002] In recent years, in automobiles, construction machinery, and industrial machinery, there has been a demand for higher strength of parts in order to improve fuel efficiency and reduce the size of equipment.

[0003] In addition, the steel pipes for machine structures used therein are subjected to bending forming, hydraulic bulging forming, pipe end flaring forming and other processing according to the application needs, and therefore high processability is also required.

[0004] Furthermore, the above-mentioned automobiles, construction machinery, and industrial machinery are sometimes used in cold regions, and therefore high low-temperature toughness is also required.

[0005] However, if the strength of the component is increased, the workability and toughness of the base material portion and the resistance welded portion will decrease, and the component cannot be used for the intended purpose.

[0006] In addition, the workability and toughness of electric resistance welded steel pipes are reduced due to work hardening during pipe making. Therefore, it is necessary to consider the reduced workability and toughness during pipe making for the hot rolled steel plate used as the base material.

[0007] In order to solve the above-mentioned problems, for example, Patent Document 1 proposes a steel plate in which bainite accounts for 90% by area or more, the average equivalent circle diameter d of the region surrounded by high-angle grain boundaries with an orientation difference of 15° or more is 4 μm or less, and further, the steel plate contains 3 to 10% by area of ​​island martensite with an average equivalent circle diameter of 0.5 to 3 μm and a Vickers hardness of Hv 700 or more.

[0008] In addition, Patent Document 2 proposes a hot-rolled steel plate, in which the total area ratio of the martensite phase and the lower bainite structure is 85% or more, the average grain size of the grains is 20 μm or less, the area ratio of the grains with an aspect ratio of 0.30 or less is 50% or less, and at the center of the plate thickness, the average value of the X-ray random intensity ratio of the {100}<011> to {211}<011> orientation group is 6.0 or less, and the maximum value is 8.0 or less.

[0009] Furthermore, Patent Document 3 proposes a rolled electric welded steel pipe for a torsion beam, wherein the area ratio of bainite is 80% or more, the average particle size of the packet grains of the bainite is 10 μm or less, the average aspect ratio of the packet grains is 2.0 or less, and the tensile strength in the pipe axis direction is 750 to 1000 MPa.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2013-057105

[0013] Patent Document 2: Japanese Patent Application Publication No. 2017-057472

[0014] Patent Document 3: International Publication No. 2019 / 220577 Summary of the invention

[0015] However, in the steel plates and electric-resistance welded steel pipes described in Patent Documents 1 to 3, the strength, toughness, workability, fatigue characteristics, etc. are improved by controlling the average crystal grain size of bainite and martensite as the main structures, but no research has been conducted from the viewpoints of the coarse grain ratio, inclusions, and workability of the electric-resistance welded portion, and there is room for further improvement in toughness and workability.

[0016] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a high-strength, excellent workability and toughness electric resistance welded steel pipe and a hot-rolled steel plate as a base material suitable for a machine structure steel pipe used as a member of an automobile, construction machinery, or industrial machinery, and a method for producing the same.

[0017] It should be noted that the "high strength" in the present invention means that in the hot-rolled steel sheet, the yield stress in the rolling direction is 650 MPa or more and the tensile strength is 750 MPa or more. In the hot-rolled steel sheet, the yield stress is preferably 700 MPa or more and the tensile strength is preferably 800 MPa or more.

[0018] On the other hand, the term "high strength" as used in the present invention means that in the electric resistance welded steel pipe, the yield stress in the pipe axial direction is 650 MPa or more, the tensile strength is 750 MPa or more, and the Vickers hardness at the center of the wall thickness of the electric resistance welded portion is 200 HV or more. In the electric resistance welded steel pipe, the yield stress is preferably 700 MPa or more, the tensile strength is 800 MPa or more, and the Vickers hardness is 220 HV or more.

[0019] The term "excellent workability" as used herein means that in a hot-rolled steel sheet, the yield ratio in the rolling direction (=yield stress / tensile strength×100) is 90.0% or less and the total elongation in the rolling direction is 15% or more. In a hot-rolled steel sheet, the yield ratio in the rolling direction is preferably 88.0% or less. It should be noted that in a hot-rolled steel sheet, the total elongation in the rolling direction is preferably 18% or more.

[0020] On the other hand, "excellent workability" as used in the present invention means that, in the electric resistance welded steel pipe, the yield ratio in the pipe axis direction (=yield stress / tensile strength×100) is 96.0% or less, the total elongation in the pipe axis direction is 15% or more, and the flattening value of the electric resistance welded portion is 0.80 or less. It should be noted that, in the electric resistance welded steel pipe, the yield ratio in the pipe axis direction is preferably 94.0% or less. In addition, in the electric resistance welded steel pipe, the total elongation in the pipe axis direction is preferably 17% or more, and the flattening value of the electric resistance welded portion is preferably 0.70 or less.

[0021] The term "excellent toughness" used in the present invention means that the Charpy impact value of the hot-rolled steel sheet at -60°C is 100 J / cm 2 In the hot-rolled steel sheet, the Charpy impact value at -60°C is preferably 140 J / cm 2 above.

[0022] On the other hand, the term "excellent toughness" as used in the present invention means that the Charpy impact value at -20°C in the electric resistance welded steel pipe is 50 J / cm 2 In the case of an electric welded steel pipe, the Charpy impact value at -20°C is preferably 60 J / cm 2 above.

[0023] The present inventors have conducted intensive studies on the above-mentioned problems and have found that if part of the grains in bainite-based steel are coarse, toughness and workability are reduced.

[0024] It was also found that the presence of a large number of coarse Ti-based inclusions reduces toughness.

[0025] If the structure is coarse on average, the proportion of high-angle grain boundaries, which are barriers to brittle fracture, decreases, so the toughness of the steel sheet decreases. In addition, even if the average grain size of the steel structure is small, if there is a certain proportion of coarse grains, this becomes the starting point of brittle fracture, so the toughness of the steel sheet still decreases.

[0026] That is, coarse grains have lower strength than their surroundings and strain is concentrated. Therefore, if there are coarse grains in a certain proportion or more in the steel structure, the steel is prone to early fracture, the total elongation is reduced, and the workability is reduced.

[0027] Therefore, by suppressing the generation of bainite existing as coarse grains, the toughness and workability can be improved.

[0028] In addition, Ti-based inclusions are polygonal and stress concentration is likely to occur near the corners, and the location where the stress concentration occurs is likely to become the starting point of brittle fracture. Therefore, if there are many coarse Ti-based inclusions, the toughness decreases.

[0029] Therefore, by suppressing the generation of such Ti-based inclusions, the toughness can be improved.

[0030] The present invention has been completed through further research based on this knowledge.

[0031] 1. A hot-rolled steel sheet having the following composition: containing, by mass%, C: 0.020% to 0.200%, Si: 0.02% to 1.00%, Mn: 0.10% to 2.50%, P: 0.050% or less, S: 0.0200% or less, Al: 0.005% to 0.100%, N: 0.0100% or less, and Ti: 0.030% to 0.200%, with the remainder being Fe and unavoidable impurities,

[0032] The steel structure having the following structure at the center of the plate thickness: the volume fraction of bainite is 90% or more, and the remainder comprises one or more of ferrite, pearlite, martensite and austenite,

[0033] Furthermore, in the steel structure at the center of the plate thickness, the average crystal grain size is 10.0 μm or less, the volume ratio of grains with a grain size of 40.0 μm or more is 40% or less, and the number density of Ti-based inclusions with a major diameter of 5.0 μm or more is 20 / mm. 2 the following.

[0034] 2. The hot-rolled steel sheet according to item 1 above, wherein the above-mentioned component composition further contains, in terms of mass %, one or more of Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less, and B: 0.0050% or less.

[0035] 3. A method for manufacturing a hot-rolled steel sheet, which is the method for manufacturing a hot-rolled steel sheet described in 1 or 2 above, comprising the following steps:

[0036] In the casting process, the molten steel is cast at an average cooling rate of 0.30°C / s or more from the solidification point of the molten steel to 1200°C to form a steel billet;

[0037] The hot rolling process is to heat the steel billet to a heating temperature in the range of 1150°C to 1300°C, and then perform hot rolling at a rough rolling end temperature of 950°C to 1180°C, a finish rolling end temperature of 850°C to 1000°C, and a total finish rolling reduction of 50% to 80%.

[0038] A cooling process, after the hot rolling process, is performed at an average cooling rate of 10°C / s to 60°C / s at the center of the plate thickness and a cooling stop temperature of 400°C to 580°C at the center of the plate thickness;

[0039] The winding step is performed at 400°C to 580°C after the cooling step.

[0040] 4. An electric welded steel pipe having a base metal portion, a weld portion and a weld heat affected zone,

[0041] The base material portion has the following composition: in mass %, C: 0.020% to 0.200%, Si: 0.02% to 1.00%, Mn: 0.10% to 2.50%, P: 0.050% or less, S: 0.0200% or less, Al: 0.005% to 0.100%, N: 0.0100% or less, and Ti: 0.030% to 0.200%, with the remainder being Fe and unavoidable impurities.

[0042] The base material portion has the following steel structure at the center of the wall thickness: the volume fraction of bainite is 90% or more, and the remainder includes one or more of ferrite, pearlite, martensite and austenite,

[0043] Furthermore, in the steel structure at the center of the wall thickness of the above-mentioned base material part, the average crystal grain size is 10.0 μm or less, the volume ratio of grains with a grain size of 40.0 μm or more is 40% or less, and the number density of Ti-based inclusions with a major diameter of 5.0 μm or more is 20 / mm. 2 the following,

[0044] The welded portion has a steel structure at the center of the wall thickness as follows: the volume fraction of ferrite is 10% or more, the volume fraction of ferrite and bainite is 60% to 98% in total, and the remainder includes one or more of pearlite, martensite and austenite.

[0045] Furthermore, the average grain size of the steel structure at the center of the wall thickness of the welded portion is 15.0 μm or less.

[0046] 5. The electric resistance welded steel pipe according to 4 above, wherein the component composition of the base material portion further contains, in mass %, one or more of Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less, and B: 0.0050% or less.

[0047] 6. A method for manufacturing an electric-welded steel pipe, which is the method for manufacturing an electric-welded steel pipe described in 4 or 5 above, comprising the following steps:

[0048] In the pipe making process, the hot-rolled steel sheet is formed into a cylindrical shape by cold rolling, and both ends of the cylindrical shape are butted and resistance welded.

[0049] The welded portion heat treatment process is to heat the position where the resistance welding is performed to 850°C to 1050°C after the pipe making process, and then to air cool it for 5s to 50s, and then to water cool it to below 200°C.

[0050] The sizing step is to adjust the outer diameter of the pipe by sizing rollers after the heat treatment step of the welded part.

[0051] The present invention can provide a high-strength, excellent workability and toughness electric resistance welded steel pipe suitable for use in machine structure steel pipes for automobiles, construction machinery, and industrial machinery parts, a hot-rolled steel plate as a base material thereof, and methods for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 This is a schematic diagram of a cross section in the pipe circumferential direction (a cross section perpendicular to the pipe axis direction) of the electric resistance welded portion of an electric-welded steel pipe. DETAILED DESCRIPTION

[0053] Hereinafter, the hot-rolled steel sheet of the present invention, the electric resistance welded steel pipe using the hot-rolled steel sheet as a base material, and the method for producing the same will be described. It should be noted that the present invention is not limited to the following embodiments.

[0054] Here, in the present invention, when the center in the pipe circumferential direction of the position where resistance welding is performed (also referred to as a resistance welded portion in the present invention) is set to 0° on a cross section perpendicular to the pipe axis of the electric resistance welded steel pipe, the component composition and steel structure of the base material portion 90° away from this position in the pipe circumferential direction are defined as the component composition of the base material portion of the electric resistance welded steel pipe of the present invention and the steel structure at the center of the wall thickness.

[0055] It should be noted that, although a position 90° away from the resistance welded portion is specified, for example, a position 180° away from the resistance welded portion also has the same component composition and steel structure.

[0056] First, the reasons for limiting the steel structure of the base material portion of the hot-rolled steel sheet and the electric resistance welded steel pipe of the present invention will be described.

[0057] In the steel structure of the hot-rolled steel plate and the electric welded steel pipe of the present invention, in the steel structure at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material part of the electric welded steel pipe, the volume fraction of bainite is 90% or more, and the remainder includes one or more of ferrite, pearlite, martensite and austenite. In addition, in the steel structure, the average crystal grain size is less than 10.0μm, and the volume fraction of grains with a grain size of 40.0μm or more is less than 40%. In addition, in the steel structure, the number density of Ti-based inclusions with a long diameter of 5.0μm or more is 20 / mm 2 the following.

[0058] It should be noted that in the present invention, the key to the above steel structure is to define at least the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-welded steel pipe. This is because in the casting process, the cooling rate is the lowest and the inclusions are the coarsest due to the final solidification position. In addition, this is because in the cooling process of hot rolling, the cooling rate is also the lowest and the grains are the coarsest.

[0059] Here, ferrite is a soft structure. In addition, bainite is a structure that is harder than ferrite and softer than pearlite, martensite, and austenite.

[0060] [Volume fraction of bainite]

[0061] If the volume fraction of bainite in the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-resistance welded steel pipe is less than 90%, the desired yield stress or tensile strength cannot be obtained. Or the desired toughness cannot be obtained. Therefore, the volume fraction of bainite in the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-resistance welded steel pipe is set to 90% or more. The volume fraction of bainite in the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-resistance welded steel pipe is preferably 93% or more, and more preferably 96% or more.

[0062] The upper limit of the volume fraction of bainite at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the base material portion of the electric resistance welded steel pipe is not particularly limited, but is preferably 99% or less from the viewpoint of ductility.

[0063] In the present invention, the volume ratio of each structure such as bainite is a value occupied in the entire steel structure in the same field of view at the target position.

[0064] [The remainder: contains one or more of austenite, ferrite, pearlite and martensite]

[0065] The remaining part of the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material part of the electric welded steel pipe contains one or more of austenite, ferrite, pearlite and martensite. These structures have a hardness difference with bainite, and stress is concentrated on the interface with bainite. If the combined volume fraction of these structures is greater than 10%, the area of ​​the interface with bainite increases, fracture is easily caused due to stress concentration, and toughness is reduced. Therefore, the combined volume fraction of these structures is set to less than 10%, preferably less than 7%, and more preferably less than 4%. It should be noted that it is difficult to completely suppress the formation of these structures in the cooling process of hot rolling, so as the lower limit of their combined volume fraction, about 1% is allowed.

[0066] In the above steel structure, various structures except austenite use austenite grain boundaries or deformation bands in austenite grains as nucleation sites. That is, in hot rolling, by increasing the reduction at a low temperature where austenite recrystallization is not easy to occur, a large number of dislocations can be introduced into austenite to refine austenite, and a large number of deformation bands can be introduced into the grains. Therefore, in the present invention, the area of ​​the nucleation site increases, the nucleation frequency becomes higher, and the steel structure can be refined.

[0067] In the present invention, observation of the steel structure can be performed by the method described below or in the later-described Examples.

[0068] That is, first, a test piece for structure observation is taken in such a manner that the observation surface is a cross section parallel to both the rolling direction and the plate thickness direction of the hot-rolled steel plate and is located at the center of the plate thickness, and in such a manner that the cross section is parallel to both the pipe axis direction and the wall thickness direction of the electric-welded steel pipe and is located at the center of the wall thickness, and the observation surface is polished and then corroded with nitric alcohol.

[0069] For the structural observation, the structure at the center of the plate thickness (or wall thickness) was observed using an optical microscope (magnification: 1000 times) or a scanning electron microscope (SEM, magnification: 1000 times) and photographed.

[0070] Next, the area ratio of bainite and the rest (ferrite, pearlite, martensite, austenite) is calculated based on the obtained optical microscope image and SEM image. The area ratio of each structure is observed in 5 or more viewing fields at the center of the plate thickness (or wall thickness), and the average value of the values ​​obtained in each viewing field is taken.

[0071] In addition, in the present invention, the area ratio obtained by tissue observation is regarded as the volume ratio of each tissue.

[0072] In addition, in the present invention, the center of the plate thickness (or wall thickness) is set as the central position in the plate thickness direction (the position of 1 / 2 of the plate thickness) or the central position in the wall thickness direction (the position of 1 / 2 of the wall thickness). If the above-mentioned steel structure exists at least within the range of ±0.20mm in the plate thickness (or wall thickness) direction centered on the plate thickness (or wall thickness), the effect of the present invention can be obtained. Therefore, in the present invention, "steel structure in the center of the plate thickness (or wall thickness)" refers to a specified area (preferably 0.10mm) existing at any point in the range of ±0.20mm in the plate thickness (or wall thickness) direction centered on the plate thickness (or wall thickness). 2 Steel structure of the above).

[0073] Ferrite is a product caused by diffusion phase transformation, with a low dislocation density and almost recovered structure. It includes polygonal ferrite and quasi-polygonal ferrite.

[0074] Bainite is a multiphase structure of lath-shaped ferrite and cementite with high dislocation density.

[0075] Pearlite is a eutectic structure of iron and iron carbide (ferrite + cementite), showing a layered structure with linear ferrite and cementite arranged alternately.

[0076] Martensite is a lath-shaped low-temperature phase transformation structure with extremely high dislocation density. In SEM images, it shows a bright contrast compared to ferrite and bainite.

[0077] It should be noted that it is difficult to distinguish martensite and austenite in the above optical microscope image and SEM image. Therefore, the total area ratio of the organization observed as martensite or austenite is calculated from the obtained SEM image, and the value obtained by subtracting the volume ratio of austenite measured by the following method from the total value is used as the volume ratio of martensite.

[0078] That is, austenite is an fcc phase, and the volume fraction of austenite is determined by X-ray diffraction. The volume fraction of austenite can be determined from the integrated intensities of the (200), (220), and (311) planes of fcc iron and the (200) and (211) planes of bcc iron obtained by X-ray diffraction.

[0079] Furthermore, in the steel structure at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-welded steel pipe, the average crystal grain size is set to 10.0 μm or less, and the volume ratio of grains with a grain size of 40.0 μm or more is set to 40% or less. In addition, in the steel structure, the number density of Ti-based inclusions with a major diameter of 5.0 μm or more is set to 20 / mm. 2 the following.

[0080] Here, in the present invention, the "average crystal grain size" refers to the average value of the equivalent circle diameters of crystal grains when a region surrounded by a boundary where the orientation difference between adjacent crystals is 15° or more is defined as a crystal grain.

[0081] In addition, the equivalent circle diameter (crystal grain size) refers to the diameter of a circle equal to the area of ​​the target crystal grain.

[0082] In addition, "Ti-based inclusions" refer to inclusions in which the proportion of Ti is 50% or more in mass %. However, since the measurement error of elements with atomic numbers 1 to 10 (H to Ne in the periodic table) is large and there is also the possibility of contamination attached to the surface, the proportion of Ti is the proportion of elements with atomic numbers after 11 (after Na in the periodic table).

[0083] [Average crystal particle size]

[0084] When the average crystal grain size of the grains in the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric welded steel pipe is greater than 10.0 μm, the yield stress or tensile strength targeted in the present invention cannot be obtained because the steel structure is not fine enough. In addition, the toughness is also reduced. Therefore, the average crystal grain size of the grains in the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric welded steel pipe is less than 10.0 μm. The average crystal grain size of the grains is preferably less than 8.0 μm. It should be noted that if the average crystal grain size is too small, the yield ratio is likely to increase, and the average crystal grain size is preferably greater than 3.0 μm.

[0085] [Grain diameter: volume ratio of grains larger than 40.0 μm]

[0086] When the volume fraction of grains with a grain size of 40.0 μm or more at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-resistance welded steel pipe is greater than 40%, the toughness and / or workability are reduced due to the high proportion of coarse grains. Therefore, the volume fraction of grains with a grain size of 40.0 μm or more at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-resistance welded steel pipe is 40% or less. The volume fraction of grains with a grain size of 40.0 μm or more at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric-resistance welded steel pipe is preferably 30% or less.

[0087] [Number density of Ti-based inclusions with a major diameter of 5.0 μm or more]

[0088] When the long diameter of the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric welded steel pipe is 5.0 μm or more, the number density of Ti-based inclusions is greater than 20 / mm 2 Therefore, the number density of Ti-based inclusions larger than 5.0 μm at the center of the thickness of the hot-rolled steel plate and the center of the thickness of the parent material of the electric welded steel pipe is 20 / mm. 2 The major diameter at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric resistance welded steel pipe is 5.0 μm or more. The number density of Ti-based inclusions is preferably 10 / mm. 2 the following.

[0089] As described in detail in the examples below, the average grain size of the steel structure, the volume fraction of grains with a grain size of 40.0 μm or more, and the number density of Ti-based inclusions with a major diameter of 5.0 μm or more can be measured by the following methods.

[0090] Regarding the measurement of the average crystal grain size, the cross sections parallel to the rolling direction and the plate thickness direction of the hot-rolled steel plate and the cross sections parallel to the pipe axis direction and the wall thickness direction of the base material portion of the electric resistance welded steel pipe were mirror-polished, and the histogram of the crystal grain size distribution at the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the base material portion of the electric resistance welded steel pipe was calculated using the SEM / EBSD method (a graph in which the horizontal axis is the crystal grain size and the vertical axis is the existence ratio of each crystal grain size), and the arithmetic mean value of the crystal grain size was calculated.

[0091] The measurement conditions are as follows: acceleration voltage: 15 kV, measurement area: 300 μm×300 μm, measurement step length (measurement resolution): 0.5 μm, and the measurement values ​​of 5 or more fields of view are averaged. It should be noted that in the analysis of crystal grain size, the results of crystal grain size less than 2.0 μm are excluded from the analysis object as measurement noise.

[0092] The volume ratio of grains having a grain size of 40.0 μm or more can be determined by calculating the total area ratio of grains having a grain size of 40.0 μm or more from the above-mentioned histogram of the grain size distribution and using the total area ratio as the above-mentioned volume ratio.

[0093] The number density of Ti-based inclusions with a major diameter of 5.0 μm or more was determined by combining the measurement of the major diameter of inclusions using SEM and elemental analysis using the SEM / EDS method in the same field of view with mirror polishing of cross sections parallel to the rolling direction and the plate thickness direction of the hot-rolled steel sheet and cross sections parallel to the pipe axis direction and the wall thickness direction of the base material portion of the electric resistance welded steel pipe.

[0094] The number density was determined by averaging the measured values ​​of five or more viewing fields at a measurement area of ​​4 mm×10 mm, with the measurement position being the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the base material portion of the electric resistance welded steel pipe.

[0095] In the steel structure at the center of the wall thickness of the electric resistance welded portion of the electric resistance welded steel pipe according to the present invention, the volume fraction of ferrite is set to 10% or more, the total volume fraction of ferrite and bainite is set to 60% to 98%, and the remainder contains one or more of pearlite, martensite and austenite, and further, the average crystal grain size is set to 15.0 μm or less.

[0096] [Volume ratio of ferrite]

[0097] If the volume fraction of ferrite in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is less than 10%, the ductility of the resistance welded portion is reduced, and the flatness value of the resistance welded portion targeted by the present invention cannot be obtained. Therefore, the volume fraction of ferrite in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is set to 10% or more. The volume fraction of ferrite in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is preferably 20% or more, and more preferably 30% or more. It should be noted that the upper limit of the volume fraction of ferrite is not particularly limited, and is preferably about 90% in industry.

[0098] [Total volume fraction of ferrite and bainite]

[0099] If the total volume fraction of ferrite and bainite in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is less than 60%, the ductility of the resistance welded portion is reduced, and the flatness value of the resistance welded portion targeted by the present invention cannot be obtained. Therefore, the total volume fraction of ferrite and bainite in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is set to 60% or more. On the other hand, if the total volume fraction of ferrite and bainite in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is greater than 98%, the strength of the resistance welded portion is reduced, and the desired Vickers hardness cannot be obtained. In addition, strain is concentrated in the resistance welded portion during the flatness test, so the desired flatness value of the resistance welded portion cannot be obtained.

[0100] Therefore, the total volume fraction of ferrite and bainite in the center of the wall thickness of the electric resistance welded portion of the electric resistance welded steel pipe is 60% to 98%. The total volume fraction of ferrite and bainite in the center of the wall thickness of the electric resistance welded portion of the electric resistance welded steel pipe is preferably 70% or more, more preferably 80% or more. On the other hand, the total volume fraction of ferrite and bainite in the center of the wall thickness of the electric resistance welded portion of the electric resistance welded steel pipe is preferably 96% or less, more preferably 94% or less.

[0101] [The remainder: contains one or more of pearlite, martensite and austenite]

[0102] The remaining part in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe contains one or more of pearlite, martensite and austenite. This is because in order to ensure the strength of the resistance welded portion, the remaining part needs to be a structure harder than ferrite and bainite. It should be noted that if the total volume ratio of these structures is greater than 40%, the desired flatness value of the resistance welded portion cannot be obtained. Therefore, the total volume ratio of these structures is set to 40% or less, preferably 30% or less, and more preferably 20% or less.

[0103] [Average crystal grain size is 15.0 μm or less]

[0104] When the average crystal grain size of the grains in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is greater than 15.0 μm, the strength of the resistance welded portion is reduced, and the desired Vickers hardness cannot be obtained. In addition, the strain is concentrated in the resistance welded portion during the flat test, so the desired flat value of the resistance welded portion cannot be obtained. Therefore, the average crystal grain size of the grains in the center of the wall thickness of the resistance welded portion of the electric-welded steel pipe is set to 15.0 μm or less. The average crystal grain size of the grains is preferably 10.0 μm or less. It should be noted that if the average crystal grain size is too small, the ductility is easily reduced, so the flat value is easily increased. Therefore, the average crystal grain size is preferably 3.0 μm or more.

[0105] [Ingredients]

[0106] Next, from the viewpoint of ensuring the above-mentioned characteristics and steel structure, the range of the composition of the electric resistance welded steel pipe of the present invention and the hot rolled steel plate as the base material thereof and the reasons for limiting the same are described. In this specification, unless otherwise specified, the "%" indicating the composition of steel (including steel plate and steel pipe) is mass %.

[0107] C: 0.020%~0.200%

[0108] C is an element that improves the strength of steel by solid solution strengthening. In order to ensure the strength targeted in the present invention, 0.020% or more of C is contained. On the other hand, if the C content is greater than 0.200%, hardenability increases, and hard pearlite, martensite, and austenite are excessively generated, so the C content is set to 0.200% or less. The C content is preferably 0.030% or more, preferably 0.180% or less. In addition, the C content is more preferably 0.040% or more, and more preferably 0.170% or less.

[0109] Si: 0.02%~1.00%

[0110] Si is an element that improves the strength of steel by solid solution strengthening. In order to obtain such an effect, 0.02% or more of Si is contained. On the other hand, if the Si content is greater than 1.00%, ductility and toughness decrease. In addition, the melting point of the oxide containing Si becomes higher, and the oxide is likely to remain in the resistance welding portion, so the ductility of the resistance welding portion decreases. Therefore, the Si content is set to 1.00% or less. The Si content is preferably 0.05% or more, preferably 0.90% or less. In addition, the Si content is more preferably 0.10% or more, and more preferably 0.80% or less.

[0111] Mn: 0.10%~2.50%

[0112] Mn is an element that utilizes solid solution strengthening to improve the strength of steel. In addition, Mn is an element that contributes to the refinement of the structure by lowering the phase transformation starting temperature. In order to ensure the strength and steel structure as the target in the present invention, more than 0.10% Mn is contained. On the other hand, if the Mn content is greater than 2.50%, the hardenability becomes high, and hard pearlite, martensite, and austenite are excessively generated, so the Mn content is set to less than 2.50%. The Mn content is preferably more than 0.40%, preferably less than 2.30%. In addition, the Mn content is more preferably more than 0.50%, more preferably less than 2.00%.

[0113] P: 0.050% or less

[0114] P segregates at the grain boundaries, causing uneven materials, so it is necessary to reduce it as much as possible, and the P content is set within the range of 0.050% or less. The P content is preferably 0.040% or less, and more preferably 0.030% or less. It should be noted that there is no particular lower limit for P, but excessive reduction will lead to increased smelting costs, so P is preferably 0.001% or more.

[0115] S: 0.0200% or less

[0116] S usually exists in steel as MnS, but MnS is stretched and thinned during the hot rolling process, which has an adverse effect on ductility and toughness. Therefore, in the present invention, it is necessary to reduce S as much as possible and set the S content to 0.0200% or less. The S content is preferably 0.0100% or less, and more preferably 0.0050% or less. It should be noted that there is no particular lower limit for S, but excessive reduction leads to an increase in smelting costs, so S is preferably 0.0001% or more.

[0117] Al: 0.005% to 0.100%

[0118] Al is an element that acts as a strong deoxidizer. In order to obtain such an effect, it is necessary to contain 0.005% or more of Al. On the other hand, if the Al content exceeds 0.100%, the weldability deteriorates, the number of alumina inclusions increases, and the surface properties deteriorate. In addition, the toughness also decreases. Therefore, the Al content is set to 0.100% or less. The Al content is preferably 0.010% or more, and preferably 0.080% or less. In addition, the Al content is more preferably 0.015% or more, and more preferably 0.070% or less.

[0119] N: 0.0100% or less

[0120] N is an impurity that is inevitably contained, and is an element that has the effect of firmly fixing the movement of dislocations to reduce ductility and toughness. In the present invention, N as an impurity is preferably reduced as much as possible, but the maximum allowable N content is 0.0100%. Therefore, the N content is set to 0.0100% or less. The N content is preferably 0.0080% or less. It should be noted that there is no lower limit for the N content, but excessive reduction leads to a rise in refining costs, so N is preferably 0.0010% or more.

[0121] Ti: 0.030%~0.200%

[0122] Ti is an element that helps to improve the strength of steel by forming fine carbides and nitrides in steel. In addition, due to its high affinity with N, it is also an element that helps to reduce the solid solution N in steel. In order to obtain the above-mentioned effect, it is necessary to contain 0.030% or more of Ti. On the other hand, if the Ti content is greater than 0.200%, coarse Ti-based inclusions are formed in the casting process, and it is difficult to ensure the number density of Ti-based inclusions with a long diameter of more than 5.0μm as the target in the present invention, and the toughness is reduced. In addition, ductility is also reduced. Therefore, the Ti content is set to less than 0.200%. The Ti content is preferably greater than 0.040%, and preferably less than 0.180%. The Ti content is more preferably greater than 0.050%, and more preferably less than 0.150%.

[0123] The above-mentioned component composition may further contain the following elements.

[0124] One or more of Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less, and B: 0.0050% or less

[0125] Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less Cu, Ni, Cr, and Mo are elements that improve the hardenability of steel and the strength of steel, and can be contained as needed. In order to obtain the above-mentioned effects, when containing Cu, Ni, Cr, and Mo, preferably Cu: 0.01% or more, Ni: 0.01% or more, Cr: 0.01% or more, and Mo: 0.01% or more are respectively contained. On the other hand, containing excessive amounts of Cu, Ni, Cr, and Mo may lead to excessive formation of hard pearlite, martensite, and austenite. In addition, defects are easily generated in the resistance welding portion, and the flatness value becomes larger (deteriorates).

[0126] Therefore, when Cu, Ni, Cr, and Mo are contained, Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, and Mo: 0.50% or less are respectively preferred.

[0127] That is, when Cu, Ni, Cr, and Mo are contained, preferably Cu: 0.01% to 0.50%, Ni: 0.01% to 0.50%, Cr: 0.01% to 0.50%, and Mo: 0.01% to 0.50%, respectively.

[0128] More preferably, Cu: 0.05% or more and Cu: 0.40% or less, Ni: 0.05% or more and Ni: 0.40% or less, Cr: 0.05% or more and Cr: 0.40% or less, and Mo: 0.05% or more and Mo: 0.40% or less. Still more preferably, Cu: 0.10% or more and Cu: 0.30% or less, Ni: 0.10% or more and Ni: 0.30% or less, Cr: 0.10% or more and Cr: 0.30% or less, and Mo: 0.10% or more and Mo: 0.30% or less.

[0129] Nb: 0.050% or less

[0130] Nb is an element that contributes to improving the strength of steel by forming fine carbides and nitrides in steel, and contributes to the refinement of the structure by inhibiting the coarsening of austenite during hot rolling. In order to obtain the above-mentioned effects, it is preferred to contain 0.002% or more of Nb. On the other hand, if the Nb content is greater than 0.050%, ductility and toughness decrease. Therefore, the Nb content is preferably less than 0.050%. The Nb content is more preferably greater than 0.005%, and more preferably less than 0.040%. In addition, the Nb content is further preferably greater than 0.010%, and further preferably less than 0.030%.

[0131] V: 0.050% or less

[0132] V is an element that contributes to improving the strength of steel by forming fine carbides and nitrides in steel. In order to obtain the above-mentioned effect, it is preferred to contain 0.002% or more of V. On the other hand, if the V content exceeds 0.050%, ductility and toughness decrease. Therefore, the V content is preferably 0.050% or less. The V content is more preferably 0.005% or more, and further preferably 0.040% or less. On the other hand, the V content is more preferably 0.010% or less, and further preferably 0.030% or less.

[0133] Ca: 0.0050% or less

[0134] Ca is an element that helps improve the toughness of steel by spheroidizing sulfides such as MnS that are stretched and thinned in the hot rolling process, and can be contained as needed. In order to obtain the above-mentioned effect, when Ca is contained, it is preferred to contain 0.0005% or more of Ca. On the other hand, if the Ca content exceeds 0.0050%, Ca oxide clusters are formed in the steel, and the toughness deteriorates. Therefore, when Ca is contained, the Ca content is preferably 0.0050% or less. The Ca content is more preferably 0.0008% or more, and more preferably 0.0045% or less. In addition, the Ca content is further preferably 0.0010% or more, and further preferably 0.0040% or less.

[0135] B: 0.0050% or less

[0136] B is an element that contributes to the refinement of the structure by lowering the phase transformation start temperature, and can be contained as needed. In order to obtain the above-mentioned effect, when B is contained, it is preferred to contain 0.0003% or more of B. On the other hand, if the B content is greater than 0.0050%, ductility and toughness deteriorate. Therefore, when B is contained, the B content is preferably 0.0050% or less. The B content is more preferably 0.0005% or more, and more preferably 0.0040% or less. In addition, the B content is further preferably 0.0008% or more, and further preferably 0.0030% or less.

[0137] In the above-mentioned component composition, the remainder is Fe and inevitable impurities. Among them, as inevitable impurities, 0.0050% or less of O (oxygen) can be contained within a range that does not impair the effects of the present invention.

[0138] The above-mentioned components are the components of the base material of the hot-rolled steel sheet and the electric-welded steel pipe in the present invention. By satisfying such components, the properties targeted by the present invention can be obtained. In addition, the components of the hot-rolled steel sheet substantially correspond to the components of the steel billet and molten steel used in its production.

[0139] In the present invention, in order to further reduce the flatness value of the electric resistance welded steel pipe, it is preferable to set the value of Mn / Si to 2.0 to 100.0.

[0140] When Mn / Si is less than 2.0 or greater than 100.0, the melting point of Si-Mn oxides becomes high, and they do not melt during resistance welding but remain as inclusions in the resistance welded portion. As a result, the flatness value may increase (deteriorate).

[0141] Mn / Si is more preferably 2.1 or more, and more preferably 90.0 or less. Also, Mn / Si is still more preferably 2.2 or more, and still more preferably 80.0 or less.

[0142] [Method for manufacturing hot-rolled steel sheet and electric-welded steel pipe]

[0143] Next, a method for producing a hot-rolled steel sheet and an electric resistance welded steel pipe according to an embodiment of the present invention will be described.

[0144] The hot rolled steel sheet of the present invention can be manufactured as follows: molten steel having the above-mentioned composition is cast at an average cooling rate of 0.30°C / s or more from the solidification point of the molten steel to 1200°C to form a steel billet (casting process), the steel billet is heated to a heating temperature of 1150°C to 1300°C, and then hot rolled at a rough rolling end temperature of 950°C to 1180°C, a finish rolling end temperature of 850°C to 1000°C, and a total finish rolling reduction of 50% to 80% (hot rolling process), then cooled at an average cooling rate of 10°C / s to 60°C / s at the center of the plate thickness and a cooling stop temperature of 400°C to 580°C at the center of the plate thickness (cooling process), and then coiled at 400°C to 580°C into a coil (coiling process).

[0145] In addition, the electric-resistance welded steel pipe of the present invention can be manufactured by forming the hot-rolled steel plate manufactured as described above into a cylindrical shape by cold rolling, butting both ends of the cylindrical shape in the circumferential direction and performing electric-resistance welding to manufacture a pipe to manufacture an electric-resistance welded steel pipe (pipe manufacturing process), then heating the position where the electric-resistance welded steel pipe is manufactured (electric-resistance welded portion) to 850° C. to 1050° C., further air cooling for 5 s to 50 s, and then water cooling to 200° C. or less (weld portion heat treatment process), and then adjusting the outer diameter of the pipe by sizing rolls (sizing process).

[0146] It should be noted that in the following description of the manufacturing method, unless otherwise specified, the expression "℃" related to temperature refers to the surface temperature of the steel billet and steel plate (hot-rolled plate). These surface temperatures can be measured using a radiation thermometer or the like. In addition, the temperature at the center of the thickness of the steel plate can be calculated by performing a heat transfer analysis on the temperature distribution in the cross section of the steel plate, and the result can be corrected according to the surface temperature of the steel plate. In addition, "hot-rolled steel plate" also includes hot-rolled plate and hot-rolled steel strip.

[0147] First, the method for producing a hot-rolled steel sheet of the present invention will be described.

[0148] In the present invention, the smelting method of the steel billet (steel billet) is not particularly limited. For example, known smelting methods such as converters, electric furnaces, and vacuum melting furnaces are all suitable. The casting method is also not particularly limited. For example, a steel billet of a desired size is produced by a known casting method such as a continuous casting method. It should be noted that there is no problem in applying the ingot casting-opening billet rolling method instead of the continuous casting method. The molten steel may also be further subjected to secondary refining such as ladle refining.

[0149] [Average cooling rate from solidification point to 1200°C in casting process: 0.30°C / s or more]

[0150] In the casting process, when the average cooling rate from the solidification point of the molten steel after the above-mentioned melting to 1200°C is less than 0.30°C / s, the Ti-based inclusions coarsen, and it is difficult to ensure the number density of Ti-based inclusions with a long diameter of 5.0μm or more as the target in the present invention, and the toughness is reduced. Therefore, the average cooling rate from the above-mentioned solidification point to 1200°C is set to be above 0.30°C / s. The average cooling rate is preferably above 0.35°C / s, and more preferably above 0.40°C / s. The upper limit of the above-mentioned average cooling rate is not specifically specified. If the average cooling rate is greater than 100°C / s, the effect of improving toughness becomes smaller relative to the increase in cooling rate, and only the equipment load is increased. Therefore, the average cooling rate from the above-mentioned solidification point to 1200°C is preferably below 100°C / s. The average cooling rate is more preferably below 80°C / s.

[0151] In addition, the above-mentioned freezing point is calculated|required by the following formula (1).

[0152] Freezing point (℃) = 1539 - (70[C] + 8[Si] + 5[Mn] + 30[P] + 25[S] + 5[Cu] + 4[Ni] + 1.5[Cr])···(1)

[0153] In the formula (1), the element symbol represents the content (mass %) of each element in the steel. It should be noted that the content of the element not contained is set to 0%.

[0154] In the present invention, the steel billet (steel ingot) obtained by the above casting is heated to a heating temperature in the range of 1150°C to 1300°C (reheating), and then the heated steel billet is hot rolled (hot rolling process) to form a hot-rolled plate, and then cooled (cooling process), and the cooled hot-rolled plate is further coiled into a coil (coiling process) to form a hot-rolled steel plate.

[0155] [Heating temperature in hot rolling process: 1150°C to 1300°C or less]

[0156] In the hot rolling process, when the heating temperature (reheating temperature) is less than 1150°C, the deformation resistance of the rolled material becomes large and rolling becomes difficult. On the other hand, if the heating temperature is greater than 1300°C, the austenite grains are coarsened, and fine austenite grains cannot be obtained in the subsequent rolling (rough rolling, finish rolling), and it is difficult to ensure the average crystal grain size as the target in the present invention. Therefore, the heating temperature in the hot rolling process is set to 1150°C to 1300°C. The heating temperature is preferably above 1170°C, and preferably below 1280°C.

[0157] It should be noted that in the present invention, in addition to the traditional method of manufacturing the steel billet (slab) and then temporarily cooling it to room temperature and then reheating it, the energy-saving direct rolling process of loading it into a heating furnace in a warm sheet state without cooling it to room temperature or immediately rolling it after a slight heat preservation can be applied without any problem.

[0158] [Rough rolling end temperature: 950℃~1180℃]

[0159] In the hot rolling process, when the rough rolling end temperature is less than 950°C, since the surface temperature of the steel sheet reaches below the ferrite transformation start temperature in the subsequent finishing rolling, a large amount of ferrite is generated, and it is difficult to ensure the volume fraction of bainite as the target of the present invention, and the yield stress or tensile strength is reduced. On the other hand, if the rough rolling end temperature is greater than 1180°C, the austenite grains are coarsened, it is difficult to ensure the average crystal grain size as the target of the present invention, and the toughness is reduced.

[0160] Therefore, the rough rolling finishing temperature in the hot rolling step is set to 950° C. to 1180° C. The rough rolling finishing temperature is more preferably 970° C. or higher, and more preferably 1150° C. or lower.

[0161] [Finish rolling end temperature: 850℃~1000℃]

[0162] In the hot rolling process, when the finishing temperature is less than 850°C, the surface temperature of the steel sheet during the finishing rolling reaches below the ferrite transformation start temperature, a large amount of ferrite is generated, and it is difficult to ensure the bainite volume fraction as the target of the present invention, and the yield stress or tensile strength is reduced. On the other hand, if the finishing temperature is greater than 1000°C, the austenite grains are coarsened, it is difficult to ensure the average crystal grain size as the target of the present invention, and the toughness is reduced.

[0163] Therefore, the finishing temperature of the hot rolling process is set to 850° C. to 1000° C. The finishing temperature of the hot rolling process is more preferably 870° C. or higher, and more preferably 980° C. or lower.

[0164] [Total reduction ratio of finishing rolling: 50% to 80%]

[0165] In the present invention, the subgrains in austenite are refined in the hot rolling process, so that the bainite and the remaining structure generated in the subsequent cooling process and coiling process are refined, and a steel structure having the yield strength targeted by the present invention is obtained. Therefore, in the hot rolling process, in order to refine the subgrains in austenite, it is necessary to increase the reduction rate in the austenite non-recrystallization temperature range and introduce sufficient processing strain. In order to achieve this purpose, in the present invention, the total reduction rate of the finish rolling is set to 50% or more.

[0166] When the total reduction rate of the finishing rolling is less than 50%, sufficient processing strain cannot be introduced in the hot rolling process. Therefore, a steel structure having the desired amount of average crystal grain size and the volume ratio of grains with a grain size of 40.0 μm or more as the target in the present invention cannot be obtained. The total reduction rate of the finishing rolling is preferably 55% or more. On the other hand, if the total reduction rate is greater than 80%, ferrite is easily generated, and it is difficult to ensure the volume ratio of bainite as the target in the present invention, and the yield stress or tensile strength is reduced. Therefore, the total reduction rate of the finishing rolling is set to less than 80%. The total reduction rate is preferably 75% or less.

[0167] It should be noted that the above-mentioned total reduction ratio of finish rolling refers to the total of the reduction ratios of the respective rolling passes in the finish rolling.

[0168] In the present invention, the upper and lower limits of the final plate thickness are not particularly specified, but from the viewpoints of ensuring the required reduction ratio and controlling the temperature of the steel plate, the final plate thickness (the thickness of the steel plate after finish rolling) is preferably in the range of 2 mm to 25 mm.

[0169] [Average cooling rate at the center of plate thickness during cooling process: 10°C / s to 60°C / s]

[0170] After the hot rolling step, a cooling step of cooling the hot rolled sheet is performed.

[0171] When the average cooling rate in the cooling process is less than 10°C / s, the ferrite volume fraction of the steel structure increases, and the steel structure having the bainite volume fraction targeted in the present invention cannot be obtained. In addition, the nucleation frequency of bainite is reduced, causing it to coarsen, so that the steel structure having the average crystal grain size targeted in the present invention cannot be obtained. On the other hand, if the above-mentioned average cooling rate is greater than 60°C / s, a large amount of martensite is generated, and the workability and toughness are reduced. Therefore, the average cooling rate of the plate thickness center of the above-mentioned hot-rolled plate is set in the range of 10°C / s to 60°C / s.

[0172] The average cooling rate is preferably 15° C. / s or more and preferably 55° C. / s or less.

[0173] In addition, in the present invention, from the viewpoint of suppressing the formation of ferrite on the surface of the steel sheet before the cooling step, it is preferred to start the cooling step immediately after the finish rolling in the hot rolling step is completed.

[0174] [Cooling stop temperature at the center of plate thickness during cooling process: 400°C to 580°C]

[0175] When the cooling stop temperature of the plate thickness center of the hot rolled plate in the cooling process is less than 400°C, a large amount of martensite is generated, so the workability and toughness are reduced. On the other hand, if the cooling stop temperature is greater than 580°C, the ferrite volume fraction increases, and the steel structure having the bainite volume fraction targeted in the present invention cannot be obtained. In addition, the nucleation frequency of bainite is reduced, making them coarse, so the structure having the average crystal grain size targeted in the present invention cannot be obtained. Therefore, the cooling stop temperature is set in the range of 400°C to 580°C.

[0176] The cooling stop temperature is preferably 420°C or higher and preferably 550°C or lower.

[0177] In the present invention, the average cooling rate refers to a value obtained by ((the plate thickness center temperature of the hot-rolled plate before cooling-the plate thickness center temperature of the hot-rolled plate after cooling) / cooling time).

[0178] The cooling method of the cooling step of the present invention may include water cooling by spraying water from a nozzle, cooling by spraying a cooling gas, etc. It should be noted that in the present invention, it is preferred to perform cooling operation (treatment) on both sides of the hot-rolled sheet so that both sides of the hot-rolled sheet are cooled under the same conditions.

[0179] [Temperature of the center of sheet thickness during the coiling process (coiling temperature): 400°C to 580°C]

[0180] After the cooling step, a coiling step of coiling the hot-rolled sheet is performed. After the coiling step, the hot-rolled sheet may be left to cool.

[0181] When the coiling temperature is less than 400°C, a large amount of martensite is generated, so the workability and toughness are reduced. On the other hand, if the coiling temperature is higher than 580°C, the ferrite volume fraction increases, and a steel structure having a bainite volume fraction as the target of the present invention cannot be obtained. In addition, the nucleation frequency of bainite decreases, and they coarsen, so a structure having an average crystal grain size as the target of the present invention cannot be obtained. Therefore, the coiling temperature is set in the range of 400°C to 580°C.

[0182] The coiling temperature is preferably 420°C or higher and preferably 550°C or lower.

[0183] Next, a method for producing an electric resistance welded steel pipe will be described.

[0184] The hot-rolled steel sheet (the hot-rolled steel sheet of the present invention) obtained by the coiling step is subjected to a pipe-making step. In the pipe-making step, the hot-rolled steel sheet is formed into a cylindrical open pipe (round steel pipe) by cold rolling, both ends (butt joints) of the cylindrical open pipe in the circumferential direction are butted and melted by high-frequency resistance heating, and pressure-bonded by upsetting with an extrusion roll, and resistance welding is performed to produce an electric-welded steel pipe.

[0185] The electric resistance welded steel pipe manufactured in this way has a base material portion as the hot-rolled steel plate, a resistance welded portion (joined portion or simply welded portion) as a location where resistance welding is performed, and a weld heat affected zone generated in the base material due to the heat during the resistance welding.

[0186] After the pipe making process, the above-mentioned electric-welded steel pipe is subjected to a weld heat treatment process. The resistance welded portion after the pipe making process is heated in the pipe making process and then rapidly cooled, so the ductility is lower than that of the base material portion. Therefore, in this weld heat treatment process, by heating the resistance welded portion and then performing appropriate cooling, the strength, workability and toughness of the resistance welded portion can be satisfied at the same time.

[0187] Here, the upset amount during resistance welding (resistance welding process) is preferably 20% or more of the plate thickness of the hot-rolled steel plate so that inclusions such as oxides and nitrides that cause a decrease in toughness are discharged together with the molten steel during welding. However, when the upset amount is greater than 100% of the plate thickness, the load on the squeeze roll becomes large. Therefore, the upset amount is preferably 20% to 100% of the plate thickness. The upset amount is more preferably 40% or more, and more preferably 80% or less.

[0188] The upset amount in the present invention can be obtained as ((circumference of the open pipe before electric resistance welding) - (circumference of the electric resistance welded steel pipe after electric resistance welding)) / (plate thickness) x 100 (%).

[0189] [Heating temperature in the weld heat treatment process: 850°C to 1050°C]

[0190] If the heating temperature in the weld heat treatment process is less than 850°C, the resistance weld is not completely austenitized, the rapid cooling structure generated in the pipe making process remains, and the ductility is reduced. Therefore, the desired flatness value of the resistance weld cannot be obtained. On the other hand, if the above heating temperature exceeds 1050°C, the austenite grains coarsen, the nucleation sites of ferrite and bainite decrease, and the volume fraction of ferrite and bainite targeted in the center of the wall thickness of the resistance weld cannot be obtained, and the desired flatness value of the resistance weld cannot be obtained. Or the average crystal grain size targeted in the present invention cannot be obtained.

[0191] [Air cooling time of weld heat treatment process: 5s to 50s]

[0192] Ferrite and bainite are generated by air cooling after heating based on the above-mentioned heating temperature. If the air cooling time is less than 5s, the desired ferrite volume fraction and the combined volume fraction of ferrite and bainite cannot be obtained in the center of the wall thickness of the resistance welding portion, and the flatness value of the resistance welding portion targeted in the present invention cannot be obtained. On the other hand, if the above-mentioned air cooling time is greater than 50s, the average crystal grain size targeted in the present invention cannot be obtained in the center of the wall thickness of the resistance welding portion. Alternatively, since it is lower than the Ms point in the air cooling, the ferrite volume fraction and the combined volume fraction of ferrite and bainite targeted in the present invention cannot be obtained, and the flatness value of the desired resistance welding portion cannot be obtained.

[0193] [Temperature after water cooling in the weld heat treatment process: 200°C or less]

[0194] The ferrite transformation and the bainite transformation are completed by the water cooling after the air cooling. If the temperature after the water cooling is higher than 200° C., the ferrite and the bainite are coarsened, and a structure having the average crystal grain size targeted by the present invention cannot be obtained.

[0195] After the weld heat treatment process, a sizing process is performed to adjust the outer diameter of the pipe using sizing rollers. In this sizing process, the outer diameter and roundness of the welded steel pipe are adjusted to desired values ​​by reducing the diameter of the welded steel pipe using rollers arranged above, below, and on the left and right sides of the welded steel pipe.

[0196] This sizing process is implemented to improve the outer diameter accuracy and roundness. In order to improve the outer diameter accuracy and roundness, it is preferred to reduce the steel pipe in a manner that the circumference of the steel pipe is reduced by a total ratio of 0.5% or more. On the other hand, if the steel pipe is reduced in a manner that the circumference of the steel pipe is reduced by a total ratio of more than 4.0%, the bending in the axial direction of the pipe when the roller passes becomes larger, and the residual stress of the steel pipe, the dislocation density on the inner surface of the pipe, and the maximum small-angle grain boundary density are all increased. As a result, the SSC resistance of the steel pipe is reduced. Therefore, it is preferred to reduce the steel pipe in a manner that the circumference of the steel pipe is reduced by a ratio of 0.5% to 4.0%. The reduction ratio of the circumference of the steel pipe is more preferably 1.0% or more, and more preferably 3.0% or less.

[0197] In the sizing process, it is preferable to perform multi-stage diameter reduction using multiple stands in order to minimize the amount of bending in the tube axis direction when the roller passes through and suppress the generation of residual stress in the tube axis direction. In addition, it is preferable to perform diameter reduction in each stand so that the tube circumference decreases at a rate of 1.0% or less.

[0198] Here, whether the steel pipe is an electric-welded steel pipe can be determined as follows: the electric-welded steel pipe is cut perpendicularly to the pipe axis, the cut surface including the welded portion (resistance welded portion) is polished and then corroded, and then observed with an optical microscope. Specifically, if the width of the joint portion of the welded portion (resistance welded portion) in the pipe circumferential direction is 1.0 μm to 1000 μm over the entire pipe thickness, it is an electric-welded steel pipe.

[0199] The etching liquid used in the above-mentioned post-polishing etching may be appropriately selected according to the steel composition and the type of steel pipe.

[0200] Figure 1 FIG. 2 schematically shows a portion of the cross section after corrosion (near the welded portion of the electric-welded steel pipe). Figure 1 As shown, the joint (weld) can be identified as a region (joint 3) having a different structure and contrast from the base material portion 1 and the weld heat affected zone 2. For example, the joint 3 of the electric resistance welded steel pipe of carbon steel and low alloy steel can be identified as a white region observed under an optical microscope in the above cross section after being corroded with nital. In addition, the joint 3 of the UOE steel pipe of carbon steel and low alloy steel can be confirmed as a region containing a honeycomb or dendrite solidification structure under an optical microscope in the above cross section corroded with nital.

[0201] It should be noted that conditions for the method of manufacturing the steel plate and the steel pipe not described above may be based on conventional methods.

[0202] Example

[0203] The present invention will be further described below based on examples. It should be noted that the present invention is not limited to the following examples.

[0204] (Manufacture of hot-rolled steel sheets)

[0205] Molten steel having the component composition shown in Table 1 was melted.

[0206]

[0207] The molten steel was subjected to a casting process under the conditions shown in Table 2 to obtain a slab (steel billet). Next, the slab was subjected to a hot rolling process, a cooling process, and a coiling process under the conditions shown in Table 2 to obtain a hot-rolled steel sheet.

[0208]

[0209] Various test specimens were taken from the hot-rolled steel sheets, and the following methods were used to carry out microstructure observation, measurement of average grain size, measurement of the volume fraction of grains with a grain size of 40.0 μm or more, measurement of the number density of Ti-based inclusions with a long diameter of 5.0 μm or more, tensile testing, and Charpy impact testing.

[0210] Various test pieces were taken from the center in the width direction of the hot-rolled steel sheet.

[0211]

[0212] (Manufacture of electric welded steel pipes)

[0213] Next, the hot-rolled steel sheet thus obtained was formed into a cylindrical open tube (round steel tube) by cold rolling, and the butted portion of the open tube was subjected to electric resistance welding to obtain a steel tube billet (pipe making process). Next, a weld heat treatment process was performed under the conditions shown in Table 4. Next, the steel tube billet after the weld heat treatment process was reduced in diameter (sizing process) by rollers arranged above, below, and on the left and right sides of the steel tube material, to obtain an electric-welded steel tube having an outer diameter D (mm) and a wall thickness t (mm) shown in Table 4.

[0214] [Table 4]

[0215]

[0216] Various test pieces were taken from the above-mentioned electric resistance welded steel pipe, and the following methods were used to carry out the structure observation, the measurement of the average crystal grain size, the measurement of the volume ratio of grains with a grain size of 40.0 μm or more, the measurement of the number density of Ti-based inclusions with a long diameter of 5.0 μm or more, the tensile test, the Charpy impact test, the Vickers hardness test, and the flat test. The various test pieces were taken from the electric resistance welded portion in the electric resistance welded steel pipe and the base material portion which was 90° away from the electric resistance welded portion in the pipe circumferential direction when the electric resistance welded portion was set to 0°. The results are shown in Table 5.

[0217]

[0218] It should be noted that specific methods of various observations, measurements, and tests are as follows.

[0219] 〔Organization Observation〕

[0220] The test pieces for microstructure observation were prepared as follows: for the hot-rolled steel plate, the observation surface was made to be a cross section parallel to both the rolling direction and the plate thickness direction of the hot-rolled steel plate; in addition, for the base material portion of the electric-resistance welded steel pipe, the observation surface was made to be a cross section parallel to both the pipe axis direction and the wall thickness direction of the electric-resistance welded steel pipe; for the electric-resistance welded portion of the electric-resistance welded steel pipe, the observation surface was made to be a cross section parallel to both the pipe circumferential direction and the wall thickness direction of the electric-resistance welded steel pipe; the test pieces were taken from the hot-rolled steel plate and the electric-resistance welded steel pipe, respectively, and mirror-polished to prepare the test pieces.

[0221] After the observation surface of the above test piece was etched with nitric alcohol, an optical microscope (magnification: 1000 times) or a scanning electron microscope (SEM, magnification: 1000 times) was used to observe and photograph the structure of the hot-rolled steel plate at the center of the plate thickness. In addition, the base material part of the electric-welded steel pipe and the resistance-welded part of the electric-welded steel pipe were observed and photographed at the center of the wall thickness. Based on the optical microscope image and SEM image obtained in this way, the area ratio of bainite and ferrite and the remaining part (pearlite, martensite, austenite) was calculated. The area ratio of each structure was set to the average value obtained by observing in 5 fields of view and averaging the values ​​obtained in each field of view. In this embodiment, the area ratio obtained by the structure observation is used as the volume ratio of each structure.

[0222] Here, ferrite is a product obtained by diffusion phase transformation, showing a low dislocation density and almost recovered structure, including polygonal ferrite and quasi-polygonal ferrite.

[0223] Bainite is a multiphase structure of lath-shaped ferrite and cementite with high dislocation density.

[0224] Pearlite is a eutectic structure of iron and iron carbide (ferrite + cementite), and presents a layered structure in which linear ferrite and cementite are alternately arranged.

[0225] Martensite is a lath-shaped low-temperature phase transformation structure with extremely high dislocation density. In SEM images, it shows bright contrast compared to ferrite and bainite.

[0226] It should be noted that it is difficult to distinguish martensite and austenite in optical microscope images and SEM images. Therefore, the area ratio of the structure observed as martensite or austenite is calculated from the obtained SEM image, and the value obtained by subtracting the volume ratio of austenite measured by the following method from the area ratio is used as the volume ratio of martensite.

[0227] The volume fraction of austenite is measured by X-ray diffraction. The test pieces for measuring the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric welded steel pipe are ground in such a way that the diffraction surface is the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric welded steel pipe, and then chemically polished to remove the surface processing layer. The measurement uses Mo's Kα rays to calculate the integrated intensity of the (200), (220), and (311) planes of fcc iron and the (200) and (211) planes of bcc iron. The normalized integrated intensity obtained by dividing each value by the theoretical intensity value is proportional to the volume fraction of each phase. The ratio of the normalized integrated intensity of austenite is calculated, and the volume fraction of austenite is calculated.

[0228] [Measurement of average crystal particle size]

[0229] In the determination of average crystal grain size, first use SEM / EBSD method to calculate the histogram of particle size distribution (set as horizontal axis: particle size, vertical axis: figure of the existence ratio of each particle size), and find the arithmetic mean of particle size. Specifically, for crystal grain size, find the orientation difference between adjacent crystal grains, take the boundary with orientation difference of more than 15 ° as crystal grain (grain boundary), measure the equivalent circle diameter of crystal grain, and use the average equivalent circle diameter as average crystal grain size. At this time, equivalent circle diameter refers to the diameter of a circle equal to the crystal grain area as the object.

[0230] [Particle size: measurement of volume fraction of grains larger than 40.0 μm]

[0231] The volume ratio of the crystal grains having a grain size of 40.0 μm or more is determined as the total area ratio of the crystal grains having a grain size of 40.0 μm or more based on the above-mentioned histogram of the crystal grain size distribution.

[0232] The measurement conditions are as follows: acceleration voltage of 15 kV, measurement area of ​​500 μm×500 μm, and measurement step length of 0.5 μm. It should be noted that in the crystal grain size analysis, the results of crystal grains with a diameter of 2.0 μm or less are excluded from the analysis object as measurement noise, and the obtained area ratio is equal to the volume ratio.

[0233] [Measurement of the number density of Ti-based inclusions with a major diameter of 5.0 μm or more]

[0234] The number density of Ti-based inclusions with a major diameter of 5.0 μm or more was determined by combining the major diameter measurement of inclusions by SEM and elemental analysis by SEM / EDS method in the same field of view on the cross section parallel to the rolling direction and the plate thickness direction of the hot-rolled steel plate and the cross section parallel to the pipe axis direction and the wall thickness direction of the parent material of the electric resistance welded steel pipe. The measurement position was set to the center of the plate thickness of the hot-rolled steel plate and the center of the wall thickness of the parent material of the electric resistance welded steel pipe, the measurement area was set to 4 mm × 10 mm, and the measurement values ​​of 5 fields of view were averaged.

[0235] 〔Tensile test〕

[0236] For the tensile test piece, a JIS No. 5 tensile test piece was taken in the hot-rolled steel plate in such a way that the tensile direction was parallel to the rolling direction. On the other hand, in the electric welded steel pipe, a JIS No. 11 tensile test piece was taken in such a way that the tensile direction was parallel to the pipe axis direction. The tensile test was carried out in accordance with the provisions of JIS Z 2241. The yield stress YS (MPa), tensile strength TS (MPa), and total elongation EL (%) were measured, and the yield ratio YR (%) defined by (YS / TS)×100 was calculated.

[0237] 〔Charpy impact test〕

[0238] For the Charpy impact test, a V-notch test piece is taken from the center of the plate thickness in a manner that the long side direction of the test piece is parallel to the rolling direction in the hot-rolled steel plate, and the test is carried out at -60°C in accordance with the provisions of JIS Z 2242 to obtain the absorbed energy. On the other hand, for electric-resistance welded steel pipes, a V-notch test piece is cut from the center of the wall thickness of the parent material portion of the obtained electric-resistance welded steel pipe in a manner that the long side direction of the test piece is parallel to the pipe axis direction, and the test is carried out at -20°C in accordance with the provisions of JIS Z 2242 to obtain the absorbed energy. The impact value is obtained by dividing the absorbed energy by the cross-sectional area of ​​the section before the test.

[0239] The number of test pieces in the Charpy impact test was set to 3 each, and the average value of the obtained impact values ​​was taken as the Charpy impact value (vE) of the hot-rolled steel sheet. -60 ) and the Charpy impact value of the parent material of the electric welded steel pipe (vE -20 ).

[0240] 〔Vickers hardness test〕

[0241] The Vickers hardness test was conducted in accordance with JIS Z 2244 by taking a test piece from the resistance welded portion of the electric resistance welded steel pipe so that the measurement plane was parallel to both the pipe circumferential direction and the wall thickness direction. The load was 0.1 kgf and the measurement position was the center of the wall thickness of the welded portion.

[0242] [Flatness test]

[0243] The flattening test was conducted by taking a 100 mm long ring-shaped test piece in the pipe axial direction from the obtained electric resistance welded steel pipe, grinding it so that the outer pipe surface of the welded portion showed metallic luster, and performing the test according to the method described in JIS G 3441. The compression speed was set to 10 mm / min, and the compression was stopped at the time when the crack occurred, and the height H of the test piece at that time was measured. The flattening value was obtained by setting the outer diameter of the steel pipe to D and using the formula H / D.

[0244] In Table 3, the hot-rolled steel sheets of Nos. 1 to 5 and the hot-rolled steel sheets of Nos. 14 and 15 are examples of the present invention, and the hot-rolled steel sheets of Nos. 6 to 13 are comparative examples.

[0245] In Table 5, electric resistance welded steel pipes Nos. 1 to 5 are examples of the present invention, and electric resistance welded steel pipes Nos. 6 to 15 are comparative examples.

[0246] Regarding the hot-rolled steel sheets of the examples of the present invention shown in Table 3, the steel structure at the center of the plate thickness is: the volume fraction of bainite is 90% or more, and the remainder contains one or more of ferrite, pearlite, martensite and austenite, the average crystal grain size is 10.0 μm or less, the volume fraction of grains with a grain size of 40.0 μm or more is 40% or less, and the number density of Ti-based inclusions with a major diameter of 5.0 μm or more is 20 pieces / mm 2the following.

[0247] On the other hand, in the case of the electric-resistance welded steel pipes of the examples of the present invention shown in Table 5, the steel structure at the center of the wall thickness of the base material portion is: the volume fraction of bainite is 90% or more, the remainder contains one or more of ferrite, pearlite, martensite and austenite, the average crystal grain size is 10.0 μm or less, the volume fraction of grains with a grain size of 40.0 μm or more is 40% or less, and the number density of Ti-based inclusions with a major diameter of 5.0 μm or more is 20 pieces / mm 2 The steel structure at the center of the wall thickness of the resistance welded portion is as follows: the volume fraction of ferrite is 10% or more, the total volume fraction of ferrite and bainite is 60% to 98% or less, the remainder includes one or more of pearlite, martensite and austenite, and the average crystal grain size is 15.0 μm or less.

[0248] In the hot-rolled steel sheets of the examples of the present invention shown in Table 3, the yield stress YS is 650 MPa or more, the tensile strength TS is 750 MPa or more, the yield ratio YR is 90.0% or less, the total elongation EL is 15% or more, and the Charpy impact value at -60°C is 100 J / cm 2 above.

[0249] On the other hand, in the electric resistance welded steel pipe of the present invention example shown in Table 5, in the base material portion, the yield stress YS is 650 MPa or more, the tensile strength TS is 750 MPa or more, the yield ratio YR is 96.0% or less, the total elongation EL is 15% or more, and the Charpy impact value at -20°C is 50 J / cm 2 As described above, in the resistance welded portion, the Vickers hardness at the center of the wall thickness is 200 HV or more, and the flattening value is 0.80 or less.

[0250] In contrast, the hot-rolled steel sheet and electric resistance welded steel pipe of Comparative Example No. 6 had a high C content, so the volume fraction of bainite was lower than the range of the present invention, and the Charpy impact value did not reach the desired value.

[0251] Since the hot-rolled steel sheet and the electric-resistance welded steel pipe of Comparative Example No. 7 had a high Si content, the total elongation, the Charpy impact value, and the flattening value of the electric-resistance welded steel pipe did not reach the desired values.

[0252] In the hot-rolled steel sheet and electric-resistance welded steel pipe of Comparative Example No. 8, since the Mn content was high, the volume fraction of bainite was lower than the range of the present invention, and the Charpy impact value did not reach the desired value.

[0253] The hot-rolled steel sheet and electric-resistance-welded steel pipe of Comparative Example No. 9 had low Ti contents, so the yield stress and tensile strength did not reach the desired values.

[0254] The hot-rolled steel sheet and electric-resistance welded steel pipe of Comparative Example No. 10 had high Ti contents, so the number density of Ti-based inclusions with a major diameter of 5.0 μm or more was higher than the range of the present invention, and the Charpy impact value did not reach the desired value.

[0255] The hot-rolled steel sheet and electric-resistance welded steel pipe of Comparative Example No. 11 had a low average cooling rate in the casting process, so the number density of Ti-based inclusions with a major diameter of 5.0 μm or more was higher than the range of the present invention, and the Charpy impact value did not reach the desired value.

[0256] The hot-rolled steel sheet and electric-welded steel pipe of Comparative Example No. 12 had high reheating temperature, rough rolling end temperature, and finish rolling end temperature in the hot rolling process, so the average grain size was higher than the range of the present invention, and the yield stress and / or tensile strength and Charpy impact value did not reach the desired values.

[0257] In the hot-rolled steel sheet and electric-resistance welded steel pipe of Comparative Example No. 13, the total reduction ratio of finish rolling was low, so the volume ratio of grains with a grain size of 40.0 μm or more exceeded the range of the present invention, and the Charpy impact value did not reach the desired value.

[0258] In the electric resistance welded steel pipe No. 14 of Comparative Example, the air cooling time in the weld heat treatment step was long, so the average grain size of the electric resistance welded portion was higher than the range of the present invention, and the Vickers hardness and flattening value did not reach the desired values.

[0259] In the electric resistance welded steel pipe No. 15 of Comparative Example, the heating temperature in the weld heat treatment step was high, so the volume fraction of ferrite and the total volume fraction of ferrite and bainite were lower than the range of the present invention, and the flattening value did not reach the desired value.

[0260] Explanation of symbols

[0261] 1. Parent material department

[0262] 2Heat affected zone

[0263] 3Joint

Claims

1. A hot-rolled steel plate having the following composition: Contains, by mass%, C: 0.020% to 0.200%, Si: 0.02% to 1.00%, Mn: 0.10% to 2.50%, P: 0.050% or less, S: 0.0200% or less, Al: 0.005% to 0.100%, N: 0.0100% or less, and Ti: 0.030% to 0.200%, with the remainder being Fe and unavoidable impurities, The steel structure having the following structure at the center of the plate thickness: the volume fraction of bainite is 90% or more, and the remainder comprises one or more of ferrite, pearlite, martensite and austenite, Furthermore, in the steel structure at the center of the plate thickness, the average crystal grain size is 10.0 μm or less, the volume ratio of grains with a grain size of 40.0 μm or more is 40% or less, and the number density of Ti-based inclusions with a long diameter of 5.0 μm or more is 20 / mm. 2 the following.

2. The hot rolled steel sheet according to claim 1, wherein: The component composition further contains, in mass %, one or more of Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less, and B: 0.0050% or less.

3. A method for manufacturing a hot-rolled steel sheet, which is the method for manufacturing a hot-rolled steel sheet according to claim 1 or 2, comprising the following steps: A casting process, wherein the molten steel is cast at an average cooling rate of 0.30°C / s or more from the solidification point of the molten steel to 1200°C to form a steel billet; A hot rolling process, wherein the steel billet is heated to a heating temperature in the range of 1150° C. to 1300° C., and then hot rolled at a rough rolling end temperature of 950° C. to 1180° C., a finish rolling end temperature of 850° C. to 1000° C., and a total finish rolling reduction of 50% to 80%; A cooling process, after the hot rolling process, is performed at an average cooling rate of 10°C / s to 60°C / s at the center of the plate thickness and a cooling stop temperature of 400°C to 580°C at the center of the plate thickness; The winding step is performed at 400°C to 580°C after the cooling step.

4. An electric welded steel pipe having a base metal portion, a weld portion and a weld heat affected zone, The base material portion has the following composition: in mass %, it contains C: 0.020% to 0.200%, Si: 0.02% to 1.00%, Mn: 0.10% to 2.50%, P: 0.050% or less, S: 0.0200% or less, Al: 0.005% to 0.100%, N: 0.0100% or less, and Ti: 0.030% to 0.200%, and the remainder is Fe and unavoidable impurities. The base material portion has the following steel structure at the center of the wall thickness: the volume fraction of bainite is 90% or more, and the remainder includes one or more of ferrite, pearlite, martensite and austenite, Furthermore, in the steel structure at the center of the wall thickness of the base material portion, the average crystal grain size is 10.0 μm or less, the volume ratio of grains with a grain size of 40.0 μm or more is 40% or less, and the number density of Ti-based inclusions with a long diameter of 5.0 μm or more is 20 / mm 2 the following, The weld portion has a steel structure at the center of the wall thickness as follows: the volume fraction of ferrite is 10% or more, the volume fraction of ferrite and bainite is 60% to 98% in total, and the remainder includes one or more of pearlite, martensite and austenite, Furthermore, in the steel structure at the center of the wall thickness of the welded portion, the average crystal grain size is 15.0 μm or less.

5. The electric-welded steel pipe according to claim 4, wherein: The component composition of the base material portion further contains, in mass %, one or more of Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, Mo: 0.50% or less, Nb: 0.050% or less, V: 0.050% or less, Ca: 0.0050% or less, and B: 0.0050% or less.

6. A method for manufacturing an electric-welded steel pipe, which is the method for manufacturing an electric-welded steel pipe according to claim 4 or 5, comprising the following steps: In the pipe making process, the hot-rolled steel sheet is formed into a cylindrical shape by cold rolling, and both ends of the cylindrical shape are butted and resistance welded; A heat treatment process for the welded portion, after the pipe making process, heating the position where the resistance welding is performed to 850°C to 1050°C, further air cooling for 5s to 50s, and then water cooling to below 200°C; The sizing step is to adjust the outer diameter of the pipe by sizing rollers after the heat treatment step of the welded part.

Citation Information

Patent Citations

  • Steel plate for low yield ratio thick-walled circular steel pipe having tensile strength of 780 mpa or more, method for manufacturing the same, and low yield ratio thick-walled circular steel pipe having tensile strength of 780 mpa or more

    JP2013057105A

  • Hot rolled steel sheet and production method therefor

    JP2017057472A

  • As-rolled electric resistance welded steel pipe for torsion beam

    WO2019220577A1