Cold-rolled steel sheet and method for producing cold-rolled steel sheet

By optimizing the chemical composition and heat treatment process of cold-rolled steel plates, ensuring the volume ratio and Mn distribution of tempered martensite and bainite in metallographic structure, the problem of insufficient strength and pore reaming in the prior art is solved, and the problem of steel plates is insufficient in the prior art is realized. High strength and excellent hole reaming effect.

CN118974295APending Publication Date: 2024-11-15NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029296.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-20
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

It is difficult for the prior art to provide cold-rolled steel plates with high strength and excellent pore reaming properties, especially in applications in automotive parts and other fields, where there is still room for improvement in the processability and pore reaming properties of the steel plates.

Method used

By optimizing the chemical composition and heat treatment process of cold-rolled steel plates, the volume ratios of tempered martensite and bainite in metallographic structures can be ensured to reach more than 85%, and Mn concentration is evenly distributed in the cross-section of the steel plate to suppress MA Generate, thereby improving pore reamability. Specific processes include heat treatment after hot rolling and heat treatment after cold rolling, controlling the temperature and cooling speed to generate appropriate metallographic structure.

Benefits of technology

It achieves high strength and excellent hole reaming, improves the tensile strength and elongation of break of the steel plate, and significantly improves the processing performance of the steel plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005053833560000111
    Figure BDA0005053833560000111
  • Figure BDA0005053833560000121
    Figure BDA0005053833560000121
  • Figure BDA0005053833560000142
    Figure BDA0005053833560000142
Patent Text Reader

Abstract

Provided is a cold-rolled steel sheet having high strength and excellent hole expandability. The cold-rolled steel sheet has a chemical composition comprising, in mass%, 0.10-0.30% of C, 2.50% or less of Si, 0.50-3.50% of Mn, 0.100% or less of P, 0.020% or less of S, 0.010-0.100% of Al, 0.0100% or less of N, 0-0.100% of Ti, 0-0.100% of Nb, 0-0.50% of V, 0-0.50% of Mo, 0-0.50% of W, 0-0.0050% of B, 0-0.0100% of Ca, 0-0.0100% of Mg, and 0-0.0100% of REM, with the balance being Fe and impurities, and has a metallographic structure containing a total of 85 vol% or more of tempered martensite and bainite, a structure other than tempered martensite, bainite and ferrite being 5 and a region in which the Mn concentration is 8.0 mass% or more in the metallographic structure is 0.05-1.5 area%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a cold-rolled steel sheet and a method for manufacturing the cold-rolled steel sheet. Background Art

[0002] Steel sheets used for automobile parts and the like are required to have high strength and excellent workability.

[0003] International Publication No. 2018 / 030502 discloses a high-strength steel sheet having a tensile strength of 980 MPa or more and good formability. The steel sheet contains a predetermined amount of Cr and Mo, the average grain size of the ferrite phase is 1.5 μm or less, the area ratio of the ferrite phase is 2% or more and 15% or less, the area ratio of the tempered martensite phase is 75% or more and 96% or less, and the total value of the interface length between the untempered martensite phase and the ferrite phase and the interface length between the untempered martensite phase and the tempered martensite phase per unit area is 6.3×10 8 μm / m 2 Above and 5.0×10 11 μm / m 2 the following.

[0004] Japanese Patent Application Publication No. 2016-194139 discloses a high-strength cold-rolled steel sheet having a tensile strength of 980 MPa or more, good workability evaluated by ductility and flangeability, and excellent collision characteristics. When the metallographic structure at a position of 1 / 4 of the plate thickness of the steel sheet is observed using a scanning electron microscope, the area ratio of ferrite relative to the entire metallographic structure is greater than 10% and less than 65%, and the remainder is quenched martensite and retained austenite, and is a hard phase composed of at least one selected from the group consisting of bainitic ferrite, bainite, and tempered martensite.

[0005] Japanese Patent Publication No. 2015-193897 discloses a high-strength cold-rolled steel sheet having a tensile strength of 980 MPa or more and excellent ductility and bendability. When observing the structure of the steel sheet at a position 1 / 4 of the thickness of the steel sheet using a scanning electron microscope, the area ratio of ferrite relative to the entire structure is 5% or more and less than 50%, and the remainder is a hard phase. Moreover, when analyzed using an electron beam microprobe analyzer, there are more than 5% by area of ​​the area where the Mn concentration is concentrated to more than 1.2 times the Mn concentration in the steel sheet, and the standard deviation of the fraction of the area where the Mn concentration is concentrated to more than 1.2 times the Mn concentration in the steel sheet in the 2 μm square partition is more than 4.0% when 100 partitions are measured.

[0006] International Publication No. 2008 / 042982 describes a method for processing an iron-based alloy, which includes: a step of setting an iron-based alloy having a first microstructure capable of transforming into a second microstructure to an austenite transformation temperature; a step of rapidly heating the iron-based alloy to a temperature higher than the austenite transformation temperature; and a step of immediately quenching at least a portion of the iron-based alloy using a quenching device adjacent to the heating device.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2018 / 030502

[0010] Patent Document 2: Japanese Patent Application Publication No. 2016-194139

[0011] Patent Document 3: Japanese Patent Application Publication No. 2015-193897

[0012] Patent Document 4: International Publication No. 2008 / 042982 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] An object of the present invention is to provide a cold-rolled steel sheet having high strength and excellent workability, and more specifically, to provide a cold-rolled steel sheet having high strength and excellent hole expandability.

[0015] Solutions for solving problems

[0016] The chemical composition of the cold-rolled steel sheet according to one embodiment of the present invention is, by mass%, C: 0.10-0.30%, Si: 2.50% or less, Mn: 0.50-3.50%, P: 0.100% or less, S: 0.020% or less, Al: 0.010-0.100%, N: 0.0100% or less, Ti: 0-0.100%, Nb: 0-0.100%, V: 0-0.50%, Mo: 0-0.50%, W: 0-0 .50%, B: 0-0.0050%, Ca: 0-0.0100%, Mg: 0-0.0100%, REM: 0-0.0100%, balance: Fe and impurities, the metallographic structure of the cold-rolled steel sheet contains tempered martensite and bainite totaling more than 85 volume%, the structure other than tempered martensite, bainite and ferrite is less than 5 volume%, and the region with Mn concentration of more than 8.0 mass% in the metallographic structure is 0.05-1.5 area%.

[0017] A method for manufacturing a cold-rolled steel sheet according to one embodiment of the present invention is a method for manufacturing the above-mentioned cold-rolled steel sheet, which includes the following steps:

[0018] A step of heat treating the hot-rolled steel sheet by keeping it in a temperature range of 620 to 700° C. for more than 10 minutes;

[0019] A step of cold rolling the heat-treated steel plate;

[0020] The step of maintaining the cold-rolled steel sheet in a temperature range of 880 to 1050° C. for 10 seconds or more and then cooling the steel sheet to a temperature of 450° C. or less at a cooling rate of 20° C. / second or more; and

[0021] After cooling to a temperature of 450° C. or less in the cooling step, the step of performing any one of the following treatments (A) and (B) is performed:

[0022] (A) After cooling to a temperature of 350°C or less and below the martensitic transformation start temperature (Ms point), the material is reheated and maintained in a temperature range of 300 to 450°C.

[0023] (B) A treatment in which the temperature is maintained in the range of 300 to 450° C. during cooling without reheating.

[0024] Effects of the Invention

[0025] According to the present invention, a cold-rolled steel sheet having high strength and excellent hole expandability can be obtained. DETAILED DESCRIPTION

[0026] The present inventors conducted various studies to solve the above-mentioned problems and obtained the following findings.

[0027] In order to make the cold-rolled steel sheet high-strength, it is necessary to perform appropriate heat treatment, and the metallographic structure needs to be set to a metallographic structure based on tempered martensite and bainite. In addition, in order to obtain excellent hole expansion, it is effective to make the distribution of Mn in the metallographic structure uniform. By making the distribution of Mn uniform, it is possible to suppress the generation of MA (martensite-austenite constituent: Martensite-Austenite Constituent) during heat treatment. Hardenability is improved in the region where Mn is enriched, and therefore, it is easy to generate MA. MA is a very hard structure, which is easy to become the starting point of cracks in hole expansion processing. By suppressing the generation of MA, hole expansion can be improved.

[0028] Specifically, the metallographic structure is set to contain a total of more than 85% by volume of tempered martensite and bainite, and in the cross section of the steel plate, the area ratio of the region where the Mn concentration in the metallographic structure is 8.0% by mass or more is set to 0.05-1.5% by area. The small area ratio of the region where the Mn concentration is more than 8.0% by mass (hereinafter referred to as the "Mn-rich region") means that Mn is uniformly distributed. By reducing the area ratio of the Mn-rich region, the generation of MA can be suppressed and the hole expansion property can be improved. On the other hand, if the Mn-rich region is completely eliminated, excellent elongation cannot be obtained. By leaving only a small area ratio (more than 0.05% by area) in the Mn-rich region, work hardening during steel processing is promoted, and the elongation of the steel is improved.

[0029] In order to obtain such a metallographic structure, the following heat treatment is effective. First, a heat treatment is performed by keeping the hot-rolled steel plate in a temperature range of 620 to 700°C for more than 10 minutes. As a result, cementite is generated in the steel, and generally, more than 10% by mass of Mn is enriched in the cementite. After the steel plate is cold rolled, it is kept at a temperature of 880 to 1050°C, so that the Mn in the metallographic structure diffuses and the distribution of Mn is uniform. By cooling the steel plate to a temperature below 450°C at a cooling rate of more than 20°C / second, martensite and bainite are generated.

[0030] As a preferred embodiment, the metallographic structure further contains 5 volume % or more of ferrite, and the average grain size of the ferrite is 10.0 μm or less. By using a metallographic structure containing 5 volume % or more of ferrite, the elongation can be further improved.

[0031] The present invention has been accomplished based on the above findings. Hereinafter, a cold-rolled steel sheet according to an embodiment of the present invention will be described.

[0032] [Cold rolled steel sheet]

[0033] [Chemical composition]

[0034] The cold-rolled steel sheet according to one embodiment of the present invention has the chemical composition described below. In the following description, "%" of the content of an element means mass %.

[0035] C: 0.10~0.30%

[0036] Carbon (C) increases the strength of steel. On the other hand, if the C content is too high, the elongation of steel decreases. Therefore, the C content is 0.10 to 0.30%. The lower limit of the C content is preferably 0.12%, and more preferably 0.15%. The upper limit of the C content is preferably 0.25%, and more preferably 0.20%.

[0037] Si: 2.50% or less

[0038] Silicon (Si) is a solid solution strengthening element. If it is contained in excess, the hot workability of the steel will decrease. Therefore, the Si content is 2.50% or less. The upper limit of the Si content is preferably 2.00%, and more preferably 1.50%. The lower limit of the Si content is preferably 0.10%, and more preferably 0.30%.

[0039] Mn: 0.50~3.50%

[0040] Manganese (Mn) improves the hardenability of steel and improves the strength of steel. On the other hand, if the Mn content is too high, the elongation of steel decreases. Therefore, the Mn content is 0.50-3.50%. The lower limit of the Mn content is preferably 0.80%, more preferably 1.20%, more preferably 1.55%, and more preferably 1.60%. The upper limit of the Mn content is preferably 3.30%, more preferably 3.00%, and more preferably 2.80%.

[0041] P: 0.100% or less

[0042] Phosphorus (P) is an impurity. P segregates at grain boundaries and reduces the elongation of steel. Therefore, the P content is 0.100% or less. The P content is preferably 0.050% or less, and more preferably 0.030% or less.

[0043] S: 0.020% or less

[0044] Sulfur (S) is an impurity. S reduces the hot workability of steel. Therefore, the S content is 0.020% or less. The S content is preferably 0.015% or less, and more preferably 0.010% or less.

[0045] Al: 0.010~0.100%

[0046] Aluminum (Al) is contained as a deoxidizer. On the other hand, if the Al content is too high, inclusions are generated and the elongation of the steel decreases. Therefore, the Al content is 0.010 to 0.100%. The lower limit of the Al content is preferably 0.015%, and more preferably 0.020%. The upper limit of the Al content is preferably 0.080%, and more preferably 0.060%.

[0047] N: 0.0100% or less

[0048] Nitrogen (N) is an impurity. N reduces the elongation of steel. Therefore, the N content is 0.0100% or less. The upper limit of the N content is preferably 0.0060%, and more preferably 0.0040%. On the other hand, if N is excessively reduced, the manufacturing cost increases. The lower limit of the N content is preferably 0.0005%, and more preferably 0.0010%.

[0049] The chemical composition of the cold-rolled steel sheet of the present embodiment may also contain one or more elements selected from the group consisting of Ti, Nb, V, Mo, W, B, Ca, Mg, and REM. These elements are all optional elements. That is, the chemical composition of the cold-rolled steel sheet of the present embodiment may not contain part or all of Ti, Nb, V, Mo, W, B, Ca, Mg, and REM.

[0050] Ti: 0~0.100%

[0051] Nb: 0~0.100%

[0052] V: 0~0.50%

[0053] Mo: 0~0.50%

[0054] W: 0~0.50%

[0055] Titanium (Ti), niobium (Nb), vanadium (V), molybdenum (Mo) and tungsten (W) all have the effect of forming carbides to improve the strength of steel. This effect can be achieved as long as a small amount of Ti, Nb, V, Mo and W is contained. On the other hand, if the content of Ti, Nb, V, Mo and W is excessive, the elongation of the steel decreases. Therefore, the content of Ti and Nb is 0-0.100%, and the content of V, Mo and W is 0-0.50%. The lower limit of Ti and Nb is preferably 0.005%. The upper limit of Ti and Nb is preferably 0.060%, and more preferably 0.040%. The lower limit of V, Mo and W is preferably 0.01%. The upper limit of V, Mo and W is preferably 0.40%, and more preferably 0.30%.

[0056] B: 0~0.0050%

[0057] Boron (B) improves the hardenability and improves the strength of the steel. This effect can be achieved as long as a small amount of B is contained. On the other hand, if the B content is excessive, the elongation of the steel decreases. Therefore, the B content is 0 to 0.0050%. The lower limit of the B content is preferably 0.0003%. The upper limit of the B content is preferably 0.0040%, and more preferably 0.0030%.

[0058] Ca: 0~0.0100%

[0059] Mg: 0~0.0100%

[0060] REM: 0~0.0100%

[0061] Calcium (Ca), magnesium (Mg), and rare earth elements (REM) all improve the hot workability of steel. This effect can be achieved as long as a small amount of Ca, Mg, and REM is contained. On the other hand, if the content of Ca, Mg, and REM is excessive, inclusions are generated and the elongation of the steel decreases. Therefore, the content of Ca, Mg, and REM is 0 to 0.0100%. The lower limit of the content of Ca, Mg, and REM is preferably 0.0001%. The upper limit of the content of Ca, Mg, and REM is preferably 0.0060%, and more preferably 0.0040%. In addition, REM is a general term for a total of 17 elements including Sc, Y, and lanthanide elements, and the content of REM refers to the total amount of the above elements.

[0062] The balance of the chemical composition of the cold-rolled steel sheet of this embodiment is Fe and impurities. The so-called impurities here refer to elements mixed from ore and waste materials used as raw materials for steel, or elements mixed from the environment of the manufacturing process, etc. Impurities are not limited to these, and examples include Cu, Ni, Cr, and O.

[0063] [Metallurgical structure]

[0064] The metallographic structure of the cold-rolled steel sheet of the present embodiment contains a total of more than 85% by volume of tempered martensite and bainite. When the total volume ratio of tempered martensite and bainite is less than 85%, the required strength cannot be obtained. In addition, the above-mentioned "bainite" is set to bainite containing tempered bainite. The bainite in the metallographic structure of the cold-rolled steel sheet of the present embodiment is partially tempered. In addition, cementite exists in the tempered martensite and bainite, but the cementite in the tempered martensite and bainite is not regarded as an independent structure, but is set to be cementite contained in the total volume of the tempered martensite and bainite.

[0065] The average grain size of cementite contained in tempered martensite and bainite is greater than 30nm. For the average grain size of cementite, a replica film is collected and extracted from a cold-rolled steel sheet, and the measurement is performed based on the results of observing more than three fields of view at an observation magnification of 10,000 to 100,000 times using transmission electron microscopy (accelerating voltage 200kV). The average grain size is set to the equivalent circle diameter. In the case where the metallographic structure is mainly composed of martensite that does not contain cementite (i.e., in the case where the quenched martensite is the main body), sufficient hole expansion cannot be obtained. The average grain size of cementite is preferably greater than 50nm.

[0066] The area with a Mn concentration of 8.0% by mass or more in the metallographic structure of the cold-rolled steel sheet of the present embodiment is 0.05 to 1.5% by area. The area ratio of the area with a Mn concentration of 8.0% by mass or more (hereinafter referred to as the "Mn-rich area") is small, which means that Mn is evenly distributed. By reducing the area ratio of the Mn-rich area, the generation of MA can be suppressed and the hole expansion property can be improved. On the other hand, if the Mn-rich area is completely eliminated, excellent elongation cannot be obtained. By leaving only 0.05% by area or more of the Mn-rich area, work hardening during steel processing can be promoted, and the elongation of the steel is improved.

[0067] The lower limit of the Mn-rich region is preferably 0.10 area %, more preferably 0.20 area %. The upper limit of the Mn-rich region is preferably 1.0 area %.

[0068] The metallographic structure of the cold-rolled steel sheet of the present embodiment preferably also contains ferrite of 5 volume % or more, and the average grain size of the ferrite is 10.0 μm or less. By setting the metallographic structure containing ferrite of 5 volume % or more, the elongation can be further improved. The lower limit of the volume fraction of ferrite is more preferably 10%. However, if the average grain size of ferrite is too large, the effect of improving the elongation cannot be obtained. The upper limit of the average grain size of ferrite is more preferably 5.0 μm.

[0069] The metallographic structure of the cold-rolled steel sheet of the present embodiment includes pearlite, MA, retained austenite, etc., but is not limited thereto. The volume ratio of the metallographic structure of the cold-rolled steel sheet of the present embodiment, excluding martensite, tempered martensite, and ferrite, is 5% or less. The upper limit of the volume ratio of the remainder is preferably 3%.

[0070] The tensile strength of the cold-rolled steel sheet of the present embodiment is preferably 980 MPa or more. The lower limit of the tensile strength is more preferably 1050 MPa, and further preferably 1180 MPa. The upper limit of the tensile strength is not particularly limited, and is, for example, 1450 MPa.

[0071] The cold-rolled steel sheet of the present embodiment preferably has a breaking elongation of 8.0% or more, and the lower limit of the breaking elongation is more preferably 10.0%.

[0072] [Method for producing cold-rolled steel sheet]

[0073] Next, an example of the method for producing the cold-rolled steel sheet described above will be described. The production method described below is for illustrative purposes only and is not intended to limit the method for producing the cold-rolled steel sheet of the present embodiment.

[0074] A hot-rolled steel sheet having the above-mentioned chemical composition is prepared. For example, a slab having the above-mentioned chemical composition is hot-rolled and coiled by a common method to produce a hot-rolled steel sheet. The rolling rate of hot rolling, the thickness of the sheet after rolling, the cooling method to room temperature, the coiling conditions, etc. are not particularly limited.

[0075] The hot-rolled steel sheet is kept in a temperature range of 620 to 700°C for more than 10 minutes. Hereinafter, this heat treatment is referred to as "heat treatment after hot rolling". Due to the heat treatment after hot rolling, cementite is generated in the steel, and Mn is enriched in the cementite. If the holding temperature is too low or the holding time is too short, Mn is not sufficiently enriched, and in the final cold-rolled steel sheet structure, the area ratio of the Mn-enriched region cannot be made to be 0.05 area % or more. On the other hand, if the holding temperature is too high, austenite is generated in a part of the structure, and the enrichment of Mn becomes insufficient. The lower limit of the holding temperature of the heat treatment after hot rolling is preferably 630°C. The upper limit of the holding temperature of the heat treatment after hot rolling is preferably 680°C. The lower limit of the holding time of the heat treatment after hot rolling is preferably 30 minutes, and more preferably 60 minutes. The upper limit of the holding time of the heat treatment after hot rolling is not particularly limited, for example, 300 minutes. The cooling rate after holding can be any speed.

[0076] In addition, if the post-hot rolling heat treatment is performed at about 600°C due to the thermodynamic properties of cementite, the concentration of Mn enriched in cementite may become excessively high. Therefore, when the temperature of the post-hot rolling heat treatment is less than 620°C, the local Mn concentration may become excessively high, and Mn may not be sufficiently diffused in the post-cold rolling heat treatment, and the area ratio of the Mn-enriched region may not be reduced to less than 1.5%.

[0077] The steel sheet subjected to the heat treatment after the hot rolling is subjected to cold rolling. The thickness reduction rate of the cold rolling is, for example, 30 to 80%.

[0078] After the cold-rolled steel sheet is held in a temperature range of 880 to 1050° C. for 10 seconds or more, it is cooled to a temperature of 450° C. or less at a cooling rate of 20° C. / second or more. Hereinafter, this heat treatment is referred to as “post-cold rolling heat treatment”.

[0079] By keeping the steel plate in a temperature range of 880 to 1050°C for more than 10 seconds, Mn in the metallographic structure diffuses and the concentration distribution of Mn is uniformed. If the holding temperature is too low or the holding time is too short, Mn is not fully diffused, and the area ratio of the Mn-rich region in the final cold-rolled steel plate structure cannot be less than 1.5 area%. On the other hand, if the holding temperature is too high, the concentration of the Mn-rich region decreases due to the diffusion of Mn elements, and is lower than the lower limit concentration of Mn. The lower limit of the holding temperature of the heat treatment after cold rolling is preferably 900°C, and more preferably 920°C. The upper limit of the holding temperature of the heat treatment after cold rolling is preferably 1000°C. The lower limit of the holding time of the heat treatment after cold rolling is preferably 20 seconds, and more preferably 30 seconds. The upper limit of the holding time of the heat treatment after cold rolling is not particularly limited, for example, 300 seconds.

[0080] After the steel plate is maintained in a temperature range of 880 to 1050°C, the steel plate is cooled to a temperature below 450°C at a cooling rate of more than 20°C / second. At this time, part of the structure is transformed into martensite. By setting the cooling rate at this time to a relatively low speed of 20 to 30°C / second, a metallographic structure containing more than 5% by volume of ferrite is obtained. If the cooling rate is less than 20°C / second, there is a situation where ferrite is excessively generated, and in the final structure of the cold-rolled steel plate, the total volume fraction of tempered martensite and bainite cannot be more than 85%. The upper limit of the cooling rate is not particularly limited, for example, it is 200°C / second.

[0081] After cooling to a temperature below 450°C, any of the following treatments are also performed: (A) after temporarily cooling to a temperature below 350°C and below the martensitic transformation start temperature (Ms point), reheating and maintaining the temperature in the temperature range of 300 to 450°C for a predetermined time (preferably more than 100 seconds) (quenching-partitioning treatment); and (B) not reheating, but maintaining the temperature in the temperature range of 300 to 450°C during cooling for a predetermined time (preferably more than 100 seconds) (isothermal quenching (Austempering) treatment).

[0082] The cementite precipitated in the hot rolling post-heat treatment is temporarily melted due to the cold rolling post-heat treatment. The melting amount of cementite at this time is more than 90 volume % of the cementite before the cold rolling post-heat treatment, preferably more than 95 volume %. After the cold rolling post-heat treatment and the cooling of the cold rolling post-heat treatment, any one of the above-mentioned (A) and (B) is processed, so that cementite is precipitated again in the metallographic structure. Thus, it is possible to obtain a metallographic structure containing a total of more than 85 volume % of tempered martensite and bainite. In addition, when the holding temperature is less than 300 ℃, there is a situation where cementite is not fully precipitated (the average grain size of cementite is not more than 30nm).

[0083] The cold-rolled steel sheet of the present embodiment is manufactured by the above process. According to the above manufacturing method, the following cold-rolled steel sheet can be obtained: having a metallographic structure containing a total of 85 volume % or more of tempered martensite and bainite, a structure other than tempered martensite, bainite and ferrite of 5 volume % or less, and a region in which the Mn concentration in the metallographic structure is 8.0 mass % or more is 0.05 to 1.5 area %.

[0084] A cold-rolled steel sheet and a method for producing the same according to an embodiment of the present invention have been described above. According to this embodiment, a cold-rolled steel sheet having high strength and excellent hole expandability can be obtained.

[0085] Example

[0086] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited to these examples.

[0087] A 180 kg steel ingot having the chemical composition shown in Table 1 was melted in a high frequency vacuum melting furnace and hot forged into a 30 mm thick slab. The obtained slab was hot rolled in a hot rolling test machine at a finishing temperature of 850 to 900°C to form a hot rolled steel sheet with a thickness of 2.0 mm. After the hot rolling was completed and 3 to 10 seconds had passed, the steel sheet was cooled to a coiling temperature of 200 to 650°C, and then cooled to below 200°C at a cooling rate of 20°C / second as a coiling simulation of the steel sheet to form a hot rolled steel sheet.

[0088] [Table 1]

[0089] Table 1

[0090]

[0091] After the hot-rolled steel sheets were heat treated at the temperature and holding time shown in Table 2 (heat treatment after hot rolling), they were cold rolled at a thickness reduction rate (cold rolling rate) of 50% to obtain steel billets with a thickness of 1.0 mm.

[0092] [Table 2]

[0093] Table 2

[0094]

[0095] A test piece having a width of 160 mm and a length of 230 mm was collected from the obtained steel billet. Heat treatment (annealing) was performed on each of the collected test pieces under the conditions described in the column "Heat treatment after cold rolling" in Table 2.

[0096] Specifically, the test material was heated to the temperature shown in Table 2, and the test material was held for the holding time shown in Table 2. After the holding, the test material was cooled to a temperature below 450°C at the cooling rate shown in Table 2. Then, the test materials of test numbers 1 to 7, 12 to 15, 17 to 21, 26 to 29, and 31 were cooled to room temperature by the following treatment: after temporarily cooling to a temperature below 350°C and below the martensitic transformation start temperature (Ms point), they were reheated and held in a temperature range of 350 to 400°C for 300 seconds (quenching-partitioning treatment). The test materials of test numbers 8 to 11, 16, 22, 24, 25, 30, and 32 were cooled to room temperature by the following treatment: without reheating, they were held in a temperature range of 350 to 400°C for 300 seconds in the middle of cooling (isothermal quenching treatment). The test material of test number 23 was cooled to room temperature without any of the above treatments.

[0097] The test specimens after heat treatment were subjected to microstructure observation, tensile test and hole expansion test.

[0098] In order to evaluate the tensile properties, two JIS 5 test pieces were collected from the heat-treated test material with the direction parallel to the rolling direction (L direction) as the length direction, and the test was carried out at a tensile speed of 10 mm / min. The tensile strength (TS / MPa) and elongation at break (tEL / %) were obtained from the test results. The tensile strength and elongation at break were set as the average value of the two tensile test pieces.

[0099] In order to measure the hole expansion rate, two test pieces of 90mm×90mm were collected from the test material after heat treatment, and a punch hole with an initial hole diameter d0=10mm was set in the center of the test piece. The hole was expanded using a conical punch with a front end angle of 60°. Cracks occurred at the punching end and the expansion was stopped at the moment of penetrating the plate thickness to remove the load. The hole diameter of the test piece was measured in the direction parallel to the rolling direction, the vertical direction, and the direction inclined at 45° (2 directions), and the average value was set as the hole diameter d after hole expansion. The hole expansion rate HER was evaluated using the following formula. The hole expansion rate HER was set as the average value of the two test pieces.

[0100] HER(%)=(d-d0) / d0×100

[0101] The metallographic structure of the test sample after the heat treatment was measured by the following method.

[0102] First, the observation sample was collected from the heat-treated test material in a manner such that the cross section parallel to the rolling direction and the plate thickness direction became the observation surface. EBSD (Electron Backscatter Diffraction) analysis was performed in the 200μmL×100μmT area of ​​the L cross section (the cross section parallel to the rolling direction and the plate thickness direction) of the test material. The scanning interval was set to 0.1μm, and the measurement points were set to a hexagonal grid.

[0103] When the EBSD data is analyzed and the crystal phase is identified from the EBSD pattern of the measurement point, the area identified as the BCC phase is regarded as any one of tempered martensite, bainite, and ferrite, the area identified as the FCC phase is regarded as retained austenite, and the area where the structure cannot be identified (for example, in the EBSD system of TSL Co., Ltd., the confidence factor (Confidential Index) value is less than 0.1, etc.) is regarded as cementite contained in MA or pearlite.

[0104] Furthermore, the region recognized as the BCC phase is classified into ferrite and other than ferrite (tempered martensite or bainite) as follows.

[0105] In EBSD data, the boundary with a crystal orientation difference of 15° or more is defined as a grain boundary, and the area surrounded by the grain boundary is regarded as a grain. In a BCC phase grain, when there are m EBSD measurement points inside the grain, the rotation matrix P representing the crystal orientation of each measurement point is j (j=1...m), the crystal orientation differences Δθ (unit: degree) between adjacent measurement points are calculated for all combinations using the following formula, and the average value M of these orientation differences is determined.

[0106] [Mathematical formula 1]

[0107] D=R k ·P i ·P j

[0108] Δθ=cos -1 ((D[1,1]+D[2,2]+D[3,3]-1) / 2)

[0109] P i or P j is a rotation matrix that can be calculated using the Euler angles of each measurement point obtained by EBSD measurement. i The Euler angle of the i-th measurement point (i=1···m) obtained by EBSD measurement is Substitute into the following formula to obtain.

[0110] [Mathematical formula 2]

[0111]

[0112] R k (k=1···24) is the rotation matrix for transforming the specified axis of the cubic crystal, with R k ·P i ·P j k is selected in such a way that the rotation angle is minimized. Adjacent measurement points are selected for the i-th measurement point and the j-th measurement point. D[i, i] represents the value of the component in the i-th row and i-th column of the 3×3 matrix D. BCC grains with an average value M of the crystal orientation difference of 0.5° or less are regarded as ferrite, and grains with an average value M of more than 0.5° are regarded as tempered martensite or bainite.

[0113] Based on the structure classification in this way, the ratio of the measurement points determined to be BCC phases (tempered martensite or bainite) other than ferrite and the measurement points determined to be ferrite to all the measurement points was calculated, and they were respectively defined as the total volume fraction of tempered martensite and bainite and the volume fraction of ferrite. The remaining regions contained pearlite, MA, and retained austenite (regions identified as FCC phases based on EBSD), and they were classified into other regions.

[0114] The average grain size of ferrite was determined by calculating the average value d of the equivalent circle diameters from the following formula in the EBSD measurement: However, the case where the volume fraction of ferrite was less than 5% was excluded from the evaluation.

[0115] [Mathematical formula 3]

[0116]

[0117] Among them, A i is the area of ​​the i-th ferrite analyzed in the EBSD data, d i is the equivalent circle diameter of the i-th ferrite. The equivalent circle diameter refers to the area of ​​the i-th ferrite (=A i ) are the diameters of circles of equal area.

[0118] In the same observation sample as above, the Mn concentration in the tissue was measured using EPMA (Electron Probe Micro Analyzer). JXA-8530F manufactured by JEOL Ltd. was used, the electron beam acceleration voltage was set to 7 kV, the irradiation current was set to 20 nA, and the 30 μm × 30 μm area of ​​the observation surface was divided into 500 points × 500 points (arranged in a square grid) and the electron beam was scanned, and the Mn fluorescent X-ray (Kα line) generated from each point was measured using a wavelength resolution detector.

[0119] The concentration X of Mn at each point was calculated from the obtained count number I of fluorescent X-rays using the following evaluation formula based on ZAF correction: Mn .

[0120] X Mn =I / I0×Z×A×F

[0121] Here, I0 represents the number of counts of fluorescent X-rays (Kα line) that can be obtained when EPMA measurement is performed under the same electron beam conditions using a standard sample of pure Mn in advance. Z, A, and F represent atomic number correction, absorption correction factor, and fluorescence correction factor, respectively, and their values ​​are based on known values ​​determined by the EPMA electron beam irradiation conditions and the component values ​​of the steel material with reference to Keiyoshi Soejima, "Electron Microscopic Analysis", Nikkan Kogyo Shimbun.

[0122] From the obtained Mn concentration distribution, the ratio of measurement points with a Mn concentration of 8.0 mass % or more to all measurement points (250,000 points) was determined and defined as the area ratio of the region with a Mn concentration of 8.0 mass % or more.

[0123] The results are shown in Table 3. In Table 3, "TM+B" represents the total volume fraction of tempered martensite and bainite, and "α" represents the volume fraction of ferrite. * ” represents the area ratio of the region where the Mn concentration is 8.0 mass % or more.

[0124] [Table 3]

[0125] Table 3

[0126]

[0127] A * : Area ratio of the region where the Mn concentration is 8.0 mass % or more

[0128] As shown in Tables 1 to 3, the test materials of test numbers 1 to 16 have a metallographic structure containing a total of more than 85% by volume of tempered martensite and bainite, and a structure other than tempered martensite, bainite and ferrite of less than 5% by mass, and the region in the metallographic structure where the Mn concentration is more than 8.0% by mass is 0.05 to 1.5% by area. The average grain size of cementite contained in the tempered martensite and bainite of these test materials is greater than 50nm. The tensile strength of these test materials is more than 980MPa, the elongation is more than 8.0%, and the hole expansion rate is more than 40.0%. In particular, the test materials of test numbers 6, 7, 11 and 12 have a metallographic structure that also contains more than 5% by volume of ferrite, and the average grain size of ferrite is less than 10.0μm. These test materials have particularly excellent elongation.

[0129] In contrast, the area in which the Mn concentration in the metallographic structure of the test materials of test numbers 17, 19, 21, 22, 24 to 26, 29 and 30 is 8.0 mass% or more is larger than 1.5 area%, and the hole expansion rate is less than 40.0%. It is believed that the reason why the area ratio of the Mn-rich area of ​​the test materials of test numbers 17, 19, 24, 25, 27, 29 and 30 is large is that the holding temperature of the heat treatment after cold rolling is too low. It is believed that the reason why the area ratio of the Mn-rich area of ​​the test materials of test numbers 21 and 26 is large is that the holding time of the heat treatment after cold rolling is too short. It is believed that the reason why the area ratio of the Mn-rich area of ​​the test material of test number 22 is large is that the temperature of the heat treatment after hot rolling is around 600°C.

[0130] The area with a Mn concentration of 8.0 mass% or more in the metallographic structure of the test materials of test numbers 18 and 27 was less than 0.05 area%, and the hole expansion ratio was less than 40.0%. It is believed that the reason why the area ratio of the Mn-enriched area in these test materials was small is that the temperature of the heat treatment after hot rolling was too low, and Mn was not enriched in the cementite in the steel.

[0131] The total volume ratio of tempered martensite and bainite of the test materials of test numbers 20, 28, 31 and 32 is less than 85%, and the tensile strength is less than 980 MPa. It is believed that the reason why the total volume ratio of tempered martensite and bainite of the test materials of test numbers 20 and 28 is less than 85% is that the cooling rate of heat treatment after cold rolling is too low. In addition, in these test materials, due to the influence of excessive generation of ferrite, the hole expansion ratio is less than 40.0%. It is believed that the reason why the total volume ratio of tempered martensite and bainite of the test materials of test numbers 31 and 32 is less than 85% is that the Mn content or C content of the steel billet is too low.

[0132] The total volume ratio of tempered martensite and bainite of the test material of test number 23 was less than 85%, and the hole expansion ratio was less than 40.0%. It is believed that the reason why the total volume ratio of tempered martensite and bainite of the test material of test number 23 was less than 85% was that the test material was cooled to room temperature without any quenching-partitioning treatment or austempering treatment, so most of the structure became martensite without precipitation of cementite.

[0133] Although the embodiments of the present invention have been described above, the above embodiments are merely examples for implementing the present invention. Therefore, the present invention is not limited to the above embodiments, and the above embodiments can be appropriately modified and implemented within the scope of the present invention.

Claims

1. A cold-rolled steel sheet, the chemical composition of which is C: 0.10-0.30% by mass, Si: 2.50% or less, Mn: 0.50~3.50%, P: 0.100% or less, S: 0.020% or less, Al:0.010~0.100%、 N: 0.0100% or less, Ti: 0~0.100%, Nb: 0~0.100%, V:0~0.50%、 Mo: 0~0.50% W:0~0.50%、 B:0~0.0050%、 Ca: 0~0.0100%, Mg: 0~0.0100%, REM: 0~0.0100%、 Balance: Fe and impurities, The metallographic structure of the cold-rolled steel sheet contains a total of 85 volume % or more of tempered martensite and bainite, and a structure other than tempered martensite, bainite and ferrite accounts for 5 volume % or less, The area in the metallographic structure where the Mn concentration is 8.0 mass % or more is 0.05 to 1.5 area %.

2. The cold-rolled steel sheet according to claim 1, wherein: The metallographic structure also contains more than 5 volume % of ferrite, The average grain size of the ferrite is 10.0 μm or less.

3. The cold-rolled steel sheet according to claim 1 or 2, wherein: The chemical composition contains, in mass%, selected from Ti: 0.005~0.100%, Nb: 0.005~0.100%, V:0.01~0.50%、 Mo: 0.01~0.50%, and W: one or more selected from the group consisting of 0.01 to 0.50%.

4. The cold-rolled steel sheet according to claim 1 or 2, wherein: The chemical composition contains, by mass%, 0.0003 to 0.0050% B.

5. The cold-rolled steel sheet according to claim 1 or 2, wherein: The chemical composition contains, in mass%, selected from Ca: 0.0001~0.0100%, Mg: 0.0001 to 0.0100%, and REM: One or more kinds selected from the group consisting of 0.0001 to 0.0100%.

6. The cold-rolled steel sheet according to claim 1 or 2, wherein: The tempered martensite and bainite of the metallographic structure contain cementite with an average grain diameter greater than 30 nm.

7. A method for manufacturing a cold-rolled steel sheet, which is a method for manufacturing the cold-rolled steel sheet according to claim 1 or 2, comprising the following steps: A step of heat treating the hot-rolled steel sheet by keeping it in a temperature range of 620 to 700° C. for more than 10 minutes; A step of cold rolling the heat-treated steel plate; The step of maintaining the cold-rolled steel sheet in a temperature range of 880 to 1050° C. for 10 seconds or more and then cooling the steel sheet to a temperature of 450° C. or less at a cooling rate of 20° C. / second or more; and After cooling to a temperature of 450° C. or less in the cooling step, the step of performing any one of the following treatments (A) and (B) is performed: (A) After cooling to a temperature of 350°C or less and below the martensitic transformation start temperature (Ms point), the material is reheated and maintained in a temperature range of 300 to 450°C. (B) A treatment in which the temperature is maintained in the range of 300 to 450° C. during cooling without reheating.