Hot press molded body

By adjusting the chemical composition of the hot stamping steel plate and the B and O concentration distribution in the surface area, the problem of difficult to take into account the collision resistance characteristics of high tensile strength hot stamping members in the prior art is solved, and the hot stamping with high strength and excellent collision resistance characteristics is achieved Forming body.

CN118974296APending Publication Date: 2024-11-15NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029926.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-14
Filing Date
2023-04-03
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing hot stamping technology is difficult to improve the collision resistance characteristics of automobile components while maintaining high tensile strength. Especially when the tensile strength exceeds 1900 MPa, the collision resistance characteristics of the components are difficult to take into account.

Method used

By adjusting the chemical composition of the steel plate and the B and O concentration distribution in the surface area, the surface portion of the steel plate is softened, thereby improving the collision resistance of the hot stamped molded body. Specific measures include reducing the B concentration and increasing the O concentration in the surface area of ​​the steel plate, ensuring the combination of B and O, and forming appropriate hardenability to improve collision resistance.

Benefits of technology

A high-strength hot stamping molded body with a tensile strength of 1900 MPa or above is achieved, and its ability to not crack in the initial stage of deformation during collision is improved. It is suitable for automotive components such as columns and bumpers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974296A_ABST
    Figure CN118974296A_ABST
Patent Text Reader

Abstract

This hot-press molded body is provided with a steel plate having a prescribed chemical composition, and the average B concentration in a region from a depth of 5.0 [mu] m to a depth of 25.0 [mu] m from the surface of the steel plate is 0.700 times or less of the B concentration at a depth of 100 [mu] m from the surface. The average B concentration in a region from a depth of 0.5 [mu] m to a depth of 4.0 [mu] m from the surface is 1.600 times or more of the B concentration at a depth of 100 [mu] m from the surface, and the average O concentration in the region from a depth of 0.5 [mu] m to a depth of 4.0 [mu] m from the surface exceeds 0.0150 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a hot stamped body.

[0002] This application claims priority based on Japanese Patent Application No. 2022-067026 filed in Japan on April 14, 2022, and the contents are incorporated herein by reference. Background Art

[0003] In recent years, from the perspective of environmental protection and resource conservation, there is a demand for lightweight automobile bodies, and high-strength steel plates are used for automobile components. When high-strength steel plates are used, the thickness of the steel plates can be reduced to reduce the weight of the automobile body, and the desired strength can be given to the automobile body. Automobile components are manufactured by press-forming steel plates, but with the high strength of the steel plates, not only the forming load increases, but also the formability decreases, making it easy to crack and wrinkle. In addition, if the high-strength steel plate is press-formed, the shape of the component changes significantly due to springback when the component is taken out of the mold, so it becomes difficult to ensure the dimensional accuracy of the component. As a result, it is not easy to manufacture high-strength body components by press forming.

[0004] In order to solve the above-mentioned problems, a technology has been proposed so far, for example, as disclosed in Patent Document 1, which is to press-form a heated steel plate using a low-temperature pressing die. This technology is called hot stamping or hot pressing, and since a steel plate that is heated to a high temperature and in a soft state is press-formed, it is possible to manufacture components of complex shapes with high dimensional accuracy. In addition, since the steel plate is rapidly cooled by contact with the die, the strength can be greatly improved by quenching at the same time as press forming. Patent Document 1 discloses that by hot stamping a steel plate with a tensile strength of 500 to 600 MPa, a component with a tensile strength of 1400 MPa or more can be obtained.

[0005] The strength of hot stamping components can be further increased by increasing the C content of the steel plate. However, if the C content of the steel plate is increased, the deformation capacity of the component decreases as the strength of the component increases. When the component deforms during a collision, it becomes easy to crack at the beginning of the deformation. As a result, it is not easy to manufacture high-strength hot stamping components with excellent collision resistance, especially when the tensile strength of the component exceeds 1900MPa, it becomes difficult to balance strength and collision resistance.

[0006] As a technology for manufacturing hot stamping components with excellent collision resistance, Patent Document 2 discloses a high-strength pressed component having a tensile strength of 1300 MPa or more and high impact absorption and a method for manufacturing the same. In addition, Patent Document 3 discloses a hot stamping component for automobiles having a tensile strength of 1100 MPa or more and improved bending of the component from the perspective of impact energy absorption and a method for manufacturing the same. In the methods disclosed in Patent Documents 2 and 3, a hot stamping steel sheet having a decarburized layer in the surface portion is hot stamped under specified conditions to form a soft layer in the surface portion of the hot stamping component, thereby improving the collision resistance of the component.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2002-102980

[0010] Patent Document 2: Japanese Patent Application Publication No. 2015-30890

[0011] Patent Document 3: International Publication No. 2018 / 179839 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, according to the research of the inventors of the present invention, it is known that if a steel sheet whose surface portion is decarburized is used for hot stamping, then during the heating process of hot stamping, C flows from the inside of the steel sheet into the surface portion, thereby increasing the C concentration in the decarburized layer, and the surface portion of the component does not soften, and there is a possibility that the collision resistance characteristics may not be sufficiently improved.

[0014] The present invention has been made in view of the above-mentioned actual situation, and an object of the present invention is to provide a hot stamped body having a high strength of a tensile strength of 1900 MPa or more and excellent collision resistance.

[0015] Means for solving problems

[0016] The gist of the present invention is as follows.

[0017] (1) A hot stamped product according to one embodiment of the present invention is a hot stamped product comprising a steel plate, wherein the chemical composition of all or part of the steel plate contains, in terms of mass %, the following:

[0018] C: more than 0.32% and less than 0.70%,

[0019] Si: less than 2.00%,

[0020] Mn: 0.01~3.00%,

[0021] P: 0.200% or less,

[0022] S: 0.0200% or less,

[0023] Sol.Al: 0.001~1.000%,

[0024] N: 0.0200% or less,

[0025] O: 0.0005~0.0200%,

[0026] B: 0.0005~0.0200%,

[0027] Cr: 0~2.00%,

[0028] Mo: 0-2.00%,

[0029] W: 0~2.00%,

[0030] Cu: 0-2.00%,

[0031] Ni: 0-2.00%,

[0032] Ti: 0~0.200%,

[0033] Nb: 0~0.200%,

[0034] V: 0~0.200%、

[0035] Zr: 0~0.200%,

[0036] Ca: 0~0.1000%,

[0037] Mg: 0~0.1000%,

[0038] REM: 0~0.1000%、

[0039] Sn: 0~0.200%,

[0040] As: 0~0.100%, and

[0041] Bi: 0~0.0500%,

[0042] The rest contains Fe and impurities.

[0043] The tensile strength is above 1900MPa.

[0044] The average B concentration in the region of the steel sheet at a depth of 5.0 μm to 25.0 μm from the surface is 0.700 times or less the B concentration at a depth of 100 μm from the surface.

[0045] The average B concentration in the region at a depth of 0.5 μm to 4.0 μm from the surface is 1.600 times or more the B concentration at the position at a depth of 100 μm from the surface,

[0046] The average O concentration in the region at a depth of 0.5 μm to 4.0 μm from the surface exceeds 0.0150 mass %.

[0047] (2) The hot stamped body according to (1) above, wherein the chemical composition may contain, in terms of mass %, one or more of the following element groups:

[0048] Cr: 0.01~2.00%,

[0049] Mo: 0.01~2.00%,

[0050] W: 0.01~2.00%,

[0051] Cu: 0.01-2.00%,

[0052] Ni: 0.01-2.00%,

[0053] Ti: 0.001~0.200%,

[0054] Nb: 0.001~0.200%,

[0055] V: 0.001~0.200%,

[0056] Zr: 0.001~0.200%,

[0057] Ca: 0.0001~0.1000%,

[0058] Mg: 0.0001~0.1000%,

[0059] REM: 0.0001~0.1000%、

[0060] Sn: 0.001~0.200%,

[0061] As: 0.001~0.100%, and

[0062] Bi: 0.0001~0.0500%.

[0063] Effects of the Invention

[0064] According to the above scheme of the present invention, a hot stamping formed body having a high strength and excellent collision resistance with a tensile strength of more than 1900 MPa can be provided. The hot stamping formed body of the above scheme has excellent collision resistance and will not crack in the initial stage of deformation during collision, so it can be suitably applied to automobile components such as pillars and bumpers. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 It is a figure which shows the hat-shaped member manufactured in Example.

[0066] Figure 2 This is a diagram showing a test body for a three-point bending test produced in Examples.

[0067] Figure 3 This is a diagram for explaining the three-point bending test performed in Examples. DETAILED DESCRIPTION

[0068] The inventors of the present invention studied a method for suppressing the occurrence of cracks in the early stage of deformation during collision in a hot stamped product having a tensile strength of 1900 MPa or more, and as a result, obtained the following findings.

[0069] (A) The impact resistance of the hot stamped body is improved by softening the surface layer portion of the hot stamped body.

[0070] (B) In order to soften the surface of the hot stamped body, it is effective to use a hot stamping steel sheet having a decarburized layer in the surface for hot stamping. However, in the process of heating the hot stamping steel sheet, C diffuses from the inside of the steel sheet to the surface, causing a phenomenon in which the C concentration in the surface increases (called carburization phenomenon). Therefore, it is possible that the surface of the hot stamped body will not be sufficiently softened, and the collision resistance of the hot stamped body cannot be fully improved.

[0071] (C) In a hot stamped body, by (a) reducing the average B concentration in a region at a depth of 5.0 μm to 25.0 μm from the surface of a steel sheet constituting the hot stamped body; (b) increasing the average B concentration in a region at a depth of 0.5 μm to 4.0 μm from the surface; and (c) increasing the average O concentration in the region at a depth of 0.5 μm to 4.0 μm from the surface, the collision resistance of the hot stamped body can be improved even if carburization occurs during the heating process of hot stamping.

[0072] (D) The reason is not clear, but it is presumed that: (a) in the region of 5.0 μm depth from the surface to 25.0 μm depth from the surface of the steel sheet constituting the hot stamped formed body, the average B concentration is reduced, thereby reducing the hardenability of the steel sheet; and (b) in the region of 0.5 μm depth from the surface to 4.0 μm depth from the surface, B combines with O to reduce the hardenability of the steel sheet, so that even if the C concentration in the surface portion of the hot stamped formed body is increased by the carburization phenomenon, the surface portion is softened.

[0073] Based on the above-mentioned understandings (A) to (D), the inventors of the present invention discovered that in the surface portion of the hot stamped body (including the surface region and the outermost region described later), by adjusting the B concentration and the O concentration to a specific range, a hot stamped body having a tensile strength of more than 1900 MPa and excellent collision resistance can be obtained.

[0074] Hereinafter, the hot stamped body of the present embodiment will be described in detail. First, the reasons for limiting the chemical composition of the steel sheet constituting the hot stamped body of the present embodiment will be described.

[0075] All or part of the steel sheet included in the hot stamped body of the present embodiment has the following chemical composition. When the hot stamped body is made of only the steel sheet, it can be said that all or part of the hot stamped body has the chemical composition shown below.

[0076] It should be noted that, for the numerical ranges described below with "to", the lower limit and upper limit are included in the range. For the numerical values ​​expressed as "lower than" or "exceeding", the values ​​are not included in the numerical range. All "%" about chemical composition means "mass %".

[0077] When the hot stamped body includes a portion having a tensile strength of 1900 MPa or more and a portion having a tensile strength of less than 1900 MPa, at least the portion having a tensile strength of 1900 MPa or more may have the following chemical composition.

[0078] The chemical composition of all or part of the steel plate possessed by the hot stamping formed body of the present embodiment includes, by mass%, C: more than 0.32% and less than 0.70%, Si: less than 2.00%, Mn: 0.01-3.00%, P: less than 0.200%, S: less than 0.0200%, sol.Al: 0.001-1.000%, N: less than 0.0200%, O: 0.0005-0.0200%, B: 0.0005-0.0200%, and the remainder: Fe and impurities.

[0079] Each element is described below.

[0080] C: more than 0.32% and less than 0.70%

[0081] C is an element that increases the tensile strength of the steel sheet after hot stamping (the steel sheet constituting the hot stamping body). When the C content is less than 0.32%, the tensile strength of the steel sheet after hot stamping becomes less than 1900 MPa, so that the strength of the hot stamping body is insufficient. In addition, the collision resistance of the hot stamping body deteriorates. Therefore, the C content is set to more than 0.32%. The C content is preferably more than 0.34%, more than 0.38%, more than 0.42% or more than 0.45%.

[0082] On the other hand, when the C content exceeds 0.70%, the strength of the hot stamped body becomes too high and excellent collision resistance characteristics cannot be obtained. Therefore, the C content is set to 0.70% or less. Preferably, the C content is 0.65% or less, 0.60% or less, 0.55% or less, or 0.50% or less.

[0083] Si: less than 2.00%

[0084] Si is an element that may be contained in steel as an impurity and make the steel embrittled. If the Si content exceeds 2.00%, its adverse effect becomes particularly large. Therefore, the Si content is set to less than 2.00%. The Si content is preferably less than 1.00%, less than 0.75%, less than 0.50%, or less than 0.20%.

[0085] The lower limit of the Si content is not particularly limited, but may be 0%. Since excessive reduction of the Si content may lead to an increase in steelmaking costs, the Si content is preferably set to 0.001% or more. In addition, Si may be actively contained because it has the effect of improving the hardenability of steel. From the viewpoint of improving hardenability, the Si content is preferably 0.05% or more, 0.10% or more, or 0.15% or more.

[0086] Mn: 0.01~3.00%

[0087] Mn is an element that combines with S as an impurity to form MnS and suppresses the disadvantages caused by S. If the Mn content is less than 0.01%, the above effect cannot be obtained. Therefore, the Mn content is set to 0.01% or more. In addition, Mn is an element that improves the hardenability of steel, and is an element that forms a metal structure with martensite as the main body inside the steel plate after hot stamping, and is effective in ensuring the strength of the hot stamped formed body. From the viewpoint of ensuring strength, the Mn content is preferably 0.50% or more, 0.75% or more, 1.00% or more, or 1.25% or more.

[0088] On the other hand, when the Mn content exceeds 3.00%, excellent collision resistance cannot be obtained in the hot stamped body. Therefore, the Mn content is set to 3.00% or less. The Mn content is preferably 2.50% or less, 2.00% or less, or 1.50% or less.

[0089] P: 0.200% or less

[0090] P is an element that may be contained in steel as an impurity and make the steel brittle. If the P content exceeds 0.200%, its adverse effect becomes particularly large, and the weldability also deteriorates significantly. Therefore, the P content is set to 0.200% or less. The P content is preferably less than 0.100%, less than 0.050%, or less than 0.020%.

[0091] The P content may be 0%, but if the P content is reduced to less than 0.001%, the P removal cost increases significantly, which is not economically preferable. Therefore, it may be set to 0.001% or more or 0.005% or more.

[0092] S: 0.0200% or less

[0093] S is an element that may be contained in steel as an impurity and make the steel brittle. If the S content exceeds 0.0200%, its adverse effect becomes particularly large. Therefore, the S content is set to 0.0200% or less. The S content is preferably less than 0.0050%, less than 0.0020%, or less than 0.0010%.

[0094] The S content may be 0%, but if the S content is reduced to less than 0.0001%, the S removal cost increases significantly, which is not economically preferable. Therefore, it may be set to 0.0001% or more or 0.0002% or more.

[0095] Sol.Al: 0.001~1.000%

[0096] Al is an element that has the function of deoxidizing molten steel. If the sol.Al content (acid-soluble Al content) is less than 0.001%, deoxidation becomes insufficient. Therefore, the sol.Al content is set to 0.001% or more. The sol.Al content is preferably 0.005% or more, 0.010% or more, or 0.020% or more.

[0097] On the other hand, if the sol.Al content is too high, it is difficult to heat the steel sheet to a temperature exceeding the Ac 3 point in the heating process of hot stamping due to the increase in the phase transformation point. In addition, the strength and collision resistance of the hot stamped body deteriorate. Therefore, the sol.Al content is set to 1.000% or less. The sol.Al content is preferably less than 0.500%, less than 0.100%, less than 0.060% or less than 0.040%.

[0098] N: 0.0200% or less

[0099] N is an element that may be contained in steel as an impurity and form nitrides during continuous casting of steel. The nitrides deteriorate the ductility of the steel sheet after hot stamping, so the N content is preferably low. If the N content exceeds 0.0200%, its adverse effects become particularly large. Therefore, the N content is set to 0.0200% or less. The N content is preferably less than 0.0100%, less than 0.0080%, or less than 0.0050%.

[0100] The N content may be 0%, but if the N content is too low, the cost of removing N increases significantly, which is not economically preferable. Therefore, the N content may be set to 0.0005% or more, 0.0010% or more, or 0.0020% or more.

[0101] O: 0.0005~0.0200%

[0102] O is an element that forms B oxide by combining with B and reduces the hardenability of steel. It is an effective element for softening the surface of the steel plate after hot stamping. If the O content is less than 0.0005%, the surface of the steel plate after hot stamping does not soften, and the collision resistance in the hot stamping body deteriorates. Therefore, the O content is set to 0.0005% or more. The O content is preferably 0.0010% or more, 0.0015% or more, or 0.0020% or more.

[0103] On the other hand, if the O content exceeds 0.0200%, a large amount of coarse oxide inclusions are formed in the steel. As a result, the collision resistance of the hot stamped body deteriorates. Therefore, the O content is set to 0.0200% or less. The O content is preferably 0.0150% or less, 0.0100% or less, 0.0060% or less, or 0.0040% or less.

[0104] B: 0.0005~0.0200%

[0105] B is an element that improves the hardenability of steel. It is an element that forms a metal structure with martensite as the main body inside the steel plate after hot stamping, and is effective in ensuring the strength of the hot stamped body. If the B content is less than 0.0005%, the desired strength cannot be obtained in the hot stamped body. In addition, the collision resistance of the hot stamped body deteriorates. Therefore, the B content is set to 0.0005% or more. The B content is preferably 0.0010% or more, 0.0015% or more, or 0.0020% or more.

[0106] On the other hand, if the B content exceeds 0.0200%, carboride is formed in the hot stamped body, and the hardenability improvement effect of B is impaired. Therefore, the B content is set to 0.0200% or less. The B content is preferably less than 0.0050%, less than 0.0040%, or less than 0.0030%.

[0107] The remainder of the chemical composition of the steel plate constituting the hot stamping body of the present embodiment may also be Fe and impurities. As impurities, elements that are inevitably mixed from steel raw materials or scrap and / or during the steelmaking process and are allowed within the range that does not hinder the characteristics of the hot stamping body of the present embodiment can be exemplified.

[0108] The steel sheet constituting the hot stamped body of the present embodiment may contain the following elements as optional elements in place of a portion of Fe. The content of the following optional elements when not contained is 0%.

[0109] Cr: 0.01~2.00%

[0110] Cr is an element that improves the strength of hot stamped parts by improving the hardenability of steel. In order to reliably obtain this effect, the Cr content is preferably set to 0.01% or more. The Cr content is more preferably 0.05% or more or 0.10% or more.

[0111] On the other hand, if the Cr content exceeds 2.00%, the collision resistance of the hot stamped body deteriorates. Therefore, the Cr content is set to 2.00% or less. The Cr content is preferably less than 0.50%, less than 0.40%, or less than 0.30%.

[0112] Mo: 0.01~2.00%

[0113] Mo is an element that improves the strength of hot stamped parts by improving the hardenability of steel. In order to reliably obtain this effect, the Mo content is preferably set to 0.01% or more. The Mo content is more preferably 0.05% or more, 0.10% or more, or 0.15% or more.

[0114] On the other hand, if the Mo content exceeds 2.00%, the collision resistance of the hot stamped body deteriorates. Therefore, the Mo content is set to 2.00% or less. The Mo content is preferably less than 0.50%, less than 0.40%, or less than 0.30%.

[0115] W: 0.01~2.00%

[0116] W is an element that improves the strength of hot stamped parts by improving the hardenability of steel. In order to reliably obtain this effect, the W content is preferably set to 0.01% or more. The W content is more preferably 0.05% or more or 0.10% or more.

[0117] On the other hand, if the W content exceeds 2.00%, the collision resistance of the hot stamped body deteriorates. Therefore, the W content is set to 2.00% or less. The W content is preferably less than 0.50%, less than 0.40%, or less than 0.30%.

[0118] Cu: 0.01~2.00%

[0119] Cu is an element that improves the strength of hot stamped parts by improving the hardenability of steel. In order to reliably obtain these effects, the Cu content is preferably set to 0.01% or more. The Cu content is more preferably set to 0.10% or more.

[0120] On the other hand, if the Cu content exceeds 2.00%, the collision resistance of the hot stamped body deteriorates. Therefore, the Cu content is set to 2.00% or less. The Cu content is preferably less than 1.00% or less than 0.50%.

[0121] Ni: 0.01~2.00%

[0122] Ni is an element that improves the strength of hot stamped parts by improving the hardenability of steel. In order to reliably obtain this effect, the Ni content is preferably set to 0.01% or more. The Ni content is more preferably set to 0.10% or more.

[0123] On the other hand, if the Ni content exceeds 2.00%, the collision resistance of the hot stamped body deteriorates. Therefore, the Ni content is preferably set to 2.00% or less. The Ni content is preferably less than 1.00% or less than 0.50%.

[0124] Ti: 0.001~0.200%

[0125] Ti is an element that forms carbonitrides in steel and improves the strength of hot stamping parts by precipitation strengthening. In addition, Ti is an element that improves the collision resistance of hot stamping parts by refining the metal structure. In order to reliably obtain these effects, the Ti content is preferably set to 0.001% or more. The Ti content is more preferably 0.005% or more or 0.010% or more.

[0126] On the other hand, if the Ti content exceeds 0.200%, a large amount of coarse carbonitrides are generated in the steel, and the collision resistance of the hot stamped body is deteriorated. Therefore, the Ti content is set to 0.200% or less. The Ti content is preferably less than 0.050% or less than 0.030%.

[0127] Nb: 0.001~0.200%

[0128] Nb is an element that forms carbonitrides in steel and improves the strength of hot stamping parts by precipitation strengthening. In addition, Nb is an element that improves the collision resistance of hot stamping parts by refining the metal structure. In order to reliably obtain these effects, the Nb content is preferably set to 0.001% or more. The Nb content is more preferably 0.005% or more or 0.010% or more.

[0129] On the other hand, if the Nb content exceeds 0.200%, a large amount of coarse carbonitrides are generated in the steel, and the collision resistance of the hot stamped body is deteriorated. Therefore, the Nb content is set to 0.200% or less. The Nb content is preferably less than 0.050%, less than 0.030%, or less than 0.020%.

[0130] V: 0.001~0.200%

[0131] V is an element that forms carbonitrides in steel and improves the strength of hot stamped parts by precipitation strengthening. In addition, V is an element that improves the collision resistance of hot stamped parts by refining the metal structure. In order to reliably obtain these effects, the V content is preferably set to 0.001% or more. The V content is more preferably 0.005% or more or 0.010% or more.

[0132] On the other hand, if the V content exceeds 0.200%, a large amount of coarse carbonitrides are generated in the steel, and the collision resistance of the hot stamped body is deteriorated. Therefore, the V content is set to 0.200% or less. The V content is preferably less than 0.100% or less than 0.050%.

[0133] Zr: 0.001~0.200%

[0134] Zr is an element that forms carbonitrides in steel and improves the strength of hot stamped parts by precipitation strengthening. In addition, Zr is an element that improves the collision resistance of hot stamped parts by refining the metal structure. In order to reliably obtain these effects, it is preferred that the Zr content be set to 0.001% or more. The Zr content is more preferably 0.005% or more or 0.010% or more.

[0135] On the other hand, if the Zr content exceeds 0.200%, a large amount of coarse carbonitrides are generated in the steel, and the collision resistance of the hot stamped body is deteriorated. Therefore, the Zr content is set to 0.200% or less. The Zr content is preferably less than 0.100% or less than 0.050%.

[0136] Ca: 0.0001~0.1000%

[0137] Ca is an element that improves the ductility of the steel sheet after hot stamping by adjusting the shape of inclusions. In order to reliably obtain this effect, the Ca content is preferably set to 0.0001% or more.

[0138] On the other hand, even if a large amount of Ca is contained, the above-mentioned effect is saturated, and excessive cost is incurred, so the Ca content is set to 0.1000% or less. The Ca content is preferably less than 0.0100%.

[0139] Mg: 0.0001~0.1000%

[0140] Mg is an element that improves the ductility of the steel sheet after hot stamping by adjusting the shape of inclusions. In order to reliably obtain these effects, the Mg content is preferably set to 0.0001% or more.

[0141] On the other hand, even if a large amount of Mg is contained, the above-mentioned effect is saturated, and excessive cost is incurred, so the Mg content is set to 0.1000% or less. The Mg content is preferably less than 0.0100%.

[0142] REM: 0.0001~0.1000%

[0143] REM is an element that improves the ductility of the steel sheet after hot stamping by adjusting the shape of inclusions. In order to reliably obtain this effect, the REM content is preferably set to 0.0001% or more.

[0144] On the other hand, even if REM is contained in a large amount, the above-mentioned effect is saturated, and excessive cost is incurred, so the REM content is set to 0.1000% or less. The REM content is preferably less than 0.0100%.

[0145] It should be noted that in the present embodiment, REM refers to a total of 17 elements including Sc, Y, and lanthanoid elements, and the content of REM refers to the total content of these elements.

[0146] Sn: 0.001~0.200%

[0147] Sn is an element that has the effect of improving the corrosion resistance of hot stamped parts. In order to reliably obtain this effect, the Sn content is preferably set to 0.001% or more. The Sn content is more preferably 0.005% or more, 0.015% or more, or 0.030% or more.

[0148] On the other hand, even if Sn is contained in a large amount, the above-mentioned effect is saturated, and excessive cost is incurred, so the Sn content is set to 0.200% or less. The Sn content is preferably 0.150% or less or 0.100% or less.

[0149] As: 0.001~0.100%

[0150] As is an element having the effect of improving the strength of a hot stamped body. In order to reliably obtain this effect, the As content is preferably set to 0.001% or more.

[0151] On the other hand, even if a large amount of As is contained, the above-mentioned effect is saturated, and excessive cost is incurred, so the As content is made 0.100% or less.

[0152] Bi: 0.0001~0.0500%

[0153] Bi is an element that improves the collision resistance of a hot stamped body by refining the solidified structure. In order to reliably obtain this effect, the Bi content is preferably set to 0.0001% or more.

[0154] On the other hand, even if Bi is contained in a large amount, the above-mentioned effect is saturated, and excessive cost is incurred, so the Bi content is set to 0.0500% or less. The Bi content is preferably 0.0100% or less or 0.0050% or less.

[0155] Regarding the chemical composition of the steel plate constituting the above-mentioned hot stamping body, it is sufficient to collect a test piece from the steel plate constituting the hot stamping body, remove the coating when the steel plate is coated, and then determine the average element content of the entire plate thickness by a general analysis method. For example, the measurement can be performed using inductively coupled plasma emission analysis or inductively coupled plasma mass spectrometry. It should be noted that C and S can be measured using the combustion-infrared absorption method, and O and N can be measured using the inert gas melting-infrared absorption method or the inert gas melting-thermal conductivity method. In the case where the surface of the steel plate constituting the hot stamping body has a coating, the coating can be removed and the chemical composition can be measured.

[0156] As described above, in the case where the hot stamped body has a portion having a tensile strength of 1900 MPa or more and a portion having a tensile strength of less than 1900 MPa, at least the portion having a tensile strength of 1900 MPa or more has the above-mentioned chemical composition. In order to analyze the chemical composition of the portion having a tensile strength of 1900 MPa or more, the tensile test described later is performed, and a test piece for chemical composition analysis is collected from a tensile test piece having a tensile strength of 1900 MPa or more or from a portion adjacent to the portion from which the tensile test piece is collected.

[0157] Next, the B concentration distribution and the O concentration distribution in the sheet thickness direction of the steel sheet constituting the hot stamped body of the present embodiment will be described.

[0158] In the present embodiment, in the process of heating the steel plate for hot stamping, by heating the steel plate for hot stamping under specific conditions, B existing in the surface region can be diffused to the outermost region, and B and O can be combined in the outermost region, thereby improving the collision resistance of the hot stamped body.

[0159] In the hot stamped body of the present embodiment, the average B concentration in the region at a depth of 5.0 μm from the surface to a depth of 25.0 μm from the above surface of the steel sheet constituting the hot stamped body is less than 0.700 times the B concentration at a position at a depth of 100 μm from the above surface, the average B concentration in the region at a depth of 0.5 μm from the above surface to a depth of 4.0 μm from the above surface is more than 1.600 times the above B concentration at the above position at a depth of 100 μm from the above surface, and the average O concentration in the above region at a depth of 0.5 μm from the above surface to a depth of 4.0 μm from the above surface exceeds 0.0150 mass %.

[0160] It should be noted that the region of the steel plate at a depth of 5.0 μm to 25.0 μm from the surface can be replaced by a region starting from a position of 5.0 μm from the surface and ending at a position of 25.0 μm from the surface. In addition, the region of the steel plate at a depth of 0.5 μm to 4.0 μm from the surface can be replaced by a region starting from a position of 0.5 μm from the surface and ending at a position of 4.0 μm from the surface.

[0161] When the hot stamped body has a portion having a tensile strength of 1900 MPa or more and a portion having a tensile strength of less than 1900 MPa, at least the portion having a tensile strength of 1900 MPa or more may have the following B concentration distribution and O concentration distribution.

[0162] Each regulation is described below.

[0163] Average B concentration in the region from 5.0 μm to 25.0 μm from the surface: 0.700 times or less the B concentration at a depth of 100 μm from the surface

[0164] If the average B concentration in the region from 5.0 μm to 25.0 μm from the surface (hereinafter sometimes referred to as the surface region) exceeds 0.700 times the B concentration at a depth of 100 μm from the surface, the surface region does not soften, and the desired collision resistance characteristics cannot be obtained in the hot stamping formed body. Therefore, the average B concentration in the surface region is set to be less than 0.700 times the B concentration at a depth of 100 μm from the surface. The average B concentration in the surface region is preferably less than 0.700 times the B concentration at a depth of 100 μm from the surface and less than 0.0015 mass%. It is further preferred that the average B concentration in the surface region is less than 0.500 times or less than 0.300 times the B concentration at a depth of 100 μm from the surface. In addition, the average B concentration in the surface region is further preferably less than 0.0010 mass% or less than 0.0006 mass%.

[0165] The lower limit is not particularly specified, but even if it is excessively reduced, not only the above effect is saturated but also the strength of the hot stamped body is reduced. Therefore, the average B concentration in the surface layer region may be set to 0.0002 mass % or more.

[0166] It should be noted that the surface refers to the surface of the steel sheet constituting the hot stamped body. When the hot stamped body has a plating layer on the surface, the surface refers to the interface between the plating layer and the steel sheet.

[0167] Average B concentration in the region from 0.5 μm to 4.0 μm from the surface: 1.600 times or more the B concentration at a depth of 100 μm from the surface

[0168] If the average B concentration in the region at a depth of 0.5 μm to 4.0 μm from the surface (hereinafter sometimes referred to as the outermost region) is lower than 1.600 times the B concentration at a depth of 100 μm from the surface, then as described below, B and O will not be fully combined in the outermost region, and the outermost region will not soften. As a result, the desired collision resistance characteristics cannot be obtained in the hot stamping formed body. Therefore, the average B concentration in the outermost region is set to be 1.600 times or more of the B concentration at a depth of 100 μm from the surface. The average B concentration in the outermost region is preferably 1.600 times or more of the B concentration at a depth of 100 μm from the surface and is 0.0040 mass % or more. It is further preferred that the average B concentration in the outermost region is 2.000 times or more, 3.000 times or more, or 4.000 times or more of the B concentration at a depth of 100 μm from the surface. Furthermore, the average B concentration in the outermost layer region is more preferably 0.0050 mass % or more, 0.0060 mass % or more, or 0.0070 mass % or more.

[0169] The upper limit is not particularly specified, but if the average B concentration in the outermost layer region is excessively increased, not only the above effect is saturated but also the productivity of the hot stamped body is greatly impaired, so it can be made 0.2000 mass % or less.

[0170] Average O concentration in the region from 0.5 μm to 4.0 μm from the surface: more than 0.0150 mass%

[0171] If the average O concentration in the region (topmost region) at a depth of 0.5 μm to 4.0 μm from the surface is less than 0.0150 mass%, the amount of O combined with B is insufficient, the amount of B in the solid solution state increases, and the topmost region does not soften. As a result, the desired collision resistance cannot be obtained in the hot stamping body. Therefore, the average O concentration in the topmost region is set to exceed 0.0150 mass%. The average O concentration in the topmost region is preferably more than 0.0200 mass%, more than 0.0300 mass%, or more than 0.0400 mass%.

[0172] The upper limit is not particularly specified, but if the average O concentration in the outermost layer region is excessively increased, not only the above effect is saturated but also the productivity of the hot stamped body is greatly impaired, so it can be made 1.0000 mass % or less.

[0173] The average B concentration in the surface region, the average B concentration and the average O concentration in the outermost region, and the B concentration at a depth of 100 μm from the surface were measured by the following method.

[0174] The test piece was collected from the hot stamped body, and after the coating was removed when the steel plate was coated, the concentration (mass %) of each element was measured from the measurement start surface to a depth position of 100 μm or more in the depth direction (plate thickness direction) by glow discharge optical emission spectroscopy (GDS analysis). It should be noted that the so-called "measurement start surface" here is different from the "surface of the steel plate".

[0175] In the GDS analysis, the measurement interval is adjusted so that the measurement points from the surface of the steel plate to the position at a depth of 100 μm are 1200 to 1800 points. In order to eliminate the influence of foreign matter such as oil attached to the measurement start surface, the depth at which the Fe concentration initially becomes 95% or more of the "Fe concentration at a depth of 100 μm from the measurement start surface" from the start of the measurement is defined as the surface of the steel plate. In addition, in the case where the hot stamped body has a coating on the surface, the depth at which the Fe concentration initially becomes 95% or more of the "Fe concentration at a depth of 100 μm from the measurement start surface" is defined as the interface between the coating and the steel plate, that is, the surface of the steel plate.

[0176] The average B concentration in the surface region is obtained by calculating the average value of the B concentration in the region from 5.0 μm depth to 25.0 μm depth from the surface of the steel plate from the obtained measurement results. In addition, the average B concentration and the average O concentration in the outermost region are obtained by respectively calculating the average values ​​of the B concentration and the O concentration in the region from 0.5 μm depth to 4.0 μm depth from the surface of the steel plate. In addition, the B concentration at a position 100 μm depth from the surface of the steel plate is obtained by calculating the B concentration at a position 100 μm depth from the surface. It should be noted that when there is no measured value of the GDS analysis at a position 100 μm depth from the surface of the steel plate, the initial measured value exceeding the position 100 μm depth from the surface can be used as the B concentration at a position 100 μm depth from the surface.

[0177] GDS analysis is preferably performed on tests collected from more than 3 locations of the hot stamped formed body, and the average value of the obtained results is used as the above-mentioned B concentration and the above-mentioned O concentration. It should be noted that, as for the test piece, as long as the tensile test described later is performed, it is sufficient to collect from a portion adjacent to the portion where the tensile test piece with a tensile strength of 1900 MPa or more is collected.

[0178] The metal structure of the steel sheet constituting the hot stamped body is not particularly limited as long as desired strength and collision resistance characteristics can be obtained, but it preferably has the following metal structure.

[0179] All or part of the steel sheet constituting the hot stamped body of the present embodiment preferably has a metal structure containing martensite in the amount shown below. In the following description of the metal structure, "%" means "volume %". In the case where the hot stamped body has a portion having a tensile strength of 1900 MPa or more and a portion having a tensile strength of less than 1900 MPa, it is sufficient as long as at least the portion having a tensile strength of 1900 MPa or more has the following metal structure.

[0180] Metal structure in the inner area

[0181] The metal structure of the inner layer region (the region from a depth of 100 μm from the surface to the center of the plate thickness (a position of 1 / 2 the plate thickness) of the steel plate constituting the hot stamped body) preferably contains more than 90.0% of martensite.

[0182] Since martensite is an effective structure for improving the tensile strength of the steel sheet after hot stamping, the volume fraction of martensite in the area from 100 μm depth from the surface to the center of the plate thickness (hereinafter sometimes referred to as the inner layer area) of the steel sheet constituting the hot stamped body is preferably greater than 90.0%. If the volume fraction of martensite in the inner layer area is less than 90.0%, it is possible that the tensile strength of the hot stamped body becomes lower than 1900 MPa, resulting in insufficient strength. Therefore, it is preferred to set the volume fraction of martensite in the inner layer area to more than 90.0%. The volume fraction of martensite in the inner layer area is more preferably greater than 91.0%, greater than 93.0% or greater than 95.0%.

[0183] The upper limit of the volume fraction of martensite in the inner layer region does not need to be specifically specified, but in order to greatly increase the volume fraction of martensite, it is necessary to excessively increase the heating temperature of the hot stamping steel sheet and excessively increase the cooling rate in the hot stamping process, which greatly impairs the productivity of the hot stamped body. Therefore, the volume fraction of martensite in the inner layer region is preferably set to 99.0% or less or 98.0% or less.

[0184] In the present embodiment, the martensite includes not only fresh martensite that has not been tempered but also tempered martensite that has been tempered and has iron carbides inside.

[0185] The remainder of the metal structure in the inner layer region may also include ferrite, pearlite, bainite or retained austenite, and may further include cementite, oxides and other precipitates that exist independently. Since it is not necessary to contain ferrite, pearlite, bainite, retained austenite and precipitates, the lower limits of the volume ratios of ferrite, pearlite, bainite, retained austenite and precipitates are all 0%.

[0186] Retained austenite has the effect of improving the ductility of the steel sheet after hot stamping. In order to obtain this effect, the volume fraction of retained austenite in the inner layer region is preferably set to 0.5% or more, 1.0% or more, or 2.0% or more.

[0187] On the other hand, in order to excessively increase the volume fraction of retained austenite, it is necessary to perform austenite isothermal quenching at high temperature after hot stamping, which greatly reduces the productivity of the hot stamped body. In addition, if retained austenite is contained excessively, the collision resistance of the hot stamped body may deteriorate. Therefore, it is preferred to set the volume fraction of retained austenite in the inner layer region to less than 9.0%, less than 7.0%, less than 5.0% or less than 4.0%.

[0188] Metal structure in the outermost layer

[0189] The metal structure of the outermost layer region preferably contains more than 5.0% of ferrite.

[0190] Ferrite is soft and has the effect of improving the collision resistance of the hot stamping formed body. In order to obtain this effect, the volume fraction of ferrite in the outermost region is preferably set to more than 5.0%. The volume fraction of ferrite in the outermost region is more preferably set to more than 10.0%, more than 20.0%, more than 40.0% or more than 60.0%.

[0191] In this embodiment, the ferrite includes not only polygonal ferrite but also acicular ferrite or bainitic ferrite with high dislocation density. In order to effectively improve the collision resistance of the hot stamped body, it is more preferred that the softest polygonal ferrite is included in the uppermost layer region at the above volume ratio.

[0192] The remaining part of the metal structure in the outermost region may also include pearlite, bainite, retained austenite or martensite, and may further include precipitates such as cementite and oxides that exist alone. Since it is not necessary to contain pearlite, bainite, retained austenite, martensite and precipitates, the lower limits of the volume ratios of pearlite, bainite, retained austenite, martensite and precipitates are all 0%. If martensite is contained excessively, the outermost region is hardened, and the collision resistance of the hot stamping formed body may be deteriorated. Therefore, it is preferred to set the volume ratio of martensite in the outermost region to less than 90.0%, less than 40.0%, less than 10.0% or less than 5.0%.

[0193] Bainite is softer than martensite and has the effect of improving the collision resistance of the hot stamping body. In order to obtain this effect, it is preferred to set the volume fraction of bainite in the outermost region to more than 10.0%. The volume fraction of bainite in the outermost region is more preferably set to more than 20.0% or more than 40.0%. On the other hand, if bainite is contained excessively, the outermost region hardens and the collision resistance of the hot stamping body may deteriorate. Therefore, it is preferred to set the volume fraction of bainite in the outermost region to less than 80.0% or less than 60.0%.

[0194] In the present embodiment, the volume ratio of each tissue is measured by the following method.

[0195] First, a test piece was collected from the hot stamping body, and after polishing the longitudinal section (plate thickness section) of the steel plate, the organization was observed in the inner layer area and the outermost layer area. The inner layer area is the area from 100 μm depth from the surface to the center of the plate thickness (1 / 2 position of the plate thickness) of the steel plate constituting the hot stamping body. The outermost layer area is the area from 0.5 μm depth from the surface to 4.0 μm depth from the surface of the steel plate.

[0196] Specifically, after the ground surface is nitric acid etched or electrolytically polished, an optical microscope and a scanning electron microscope (SEM) are used to take a tissue photograph, and the obtained tissue photograph is subjected to different image analysis based on the brightness difference or the morphology of the iron carbide present in the phase, thereby obtaining the area ratio of ferrite, pearlite, bainite, tempered martensite and precipitates. Afterwards, after Lepera corrosion is performed on the same observation position, an optical microscope and a scanning electron microscope (SEM) are used to take a tissue photograph, and the obtained tissue photograph is subjected to image analysis, thereby calculating the total area ratio of "retained austenite and primary martensite".

[0197] In addition, for the same observation position, the longitudinal cross section was electrolytically polished, and the area ratio of retained austenite was measured using a SEM equipped with an electron beam backscattering pattern analyzer (EBSP device). It should be noted that the area ratio of the region where the crystal structure is fcc is calculated from the crystal orientation information obtained by EBSP analysis, thereby obtaining the area ratio of retained austenite.

[0198] The area ratio of fresh martensite is obtained by subtracting the area ratio of retained austenite from the sum of the area ratios of “retained austenite and fresh martensite” described above.

[0199] Based on these results, the area ratios of ferrite, pearlite, bainite, martensite (tempered martensite and fresh martensite), retained austenite, and precipitates were obtained. The area ratio was then set equal to the volume ratio, and the obtained area ratio was regarded as the volume ratio of each structure.

[0200] In the microstructure observation, tempered martensite can be distinguished from fresh martensite in that iron carbides are present inside. In addition, tempered martensite can be distinguished from bainite in that the iron carbides present inside are not in a single direction but are elongated in multiple directions. It should be noted that elongation in a single direction means that the difference in the elongation direction is within 5°.

[0201] Plate thickness

[0202] The plate thickness of the hot stamped body of this embodiment (the plate thickness of the steel plate when the hot stamped body is made only of steel plate) is not particularly limited, but from the perspective of lightweight vehicle body, it is preferably set to less than 2.5 mm, less than 2.0 mm, less than 1.8 mm or less than 1.6 mm.

[0203] On the other hand, from the viewpoint of ensuring the impact absorption amount, the plate thickness is preferably set to 0.4 mm or more, 0.6 mm or more, 0.8 mm or more, or 1.0 mm or more.

[0204] tensile strength

[0205] The tensile strength of all or part of the hot stamped body of the present embodiment is 1900 MPa or more. Therefore, the tensile strength of all or part of the steel plate constituting the hot stamped body of the present embodiment needs to be 1900 MPa or more. In the case where the tensile strength of at least a part of the hot stamped body is not more than 1900 MPa, it becomes impossible to ensure the deformation load of the hot stamped body. As a result, the collision resistance of the hot stamped body deteriorates. Therefore, the tensile strength of all or part of the hot stamped body is set to be more than 1900 MPa. Preferably, in all or part of the hot stamped body, the tensile strength is more than 2000 MPa, more than 2100 MPa, more than 2300 MPa or more than 2500 MPa.

[0206] On the other hand, since excessively increasing the strength of the hot stamped body may cause a decrease in collision resistance characteristics, the tensile strength of the hot stamped body is preferably set to less than 3000 MPa or less than 2800 MPa.

[0207] The hot stamped parts of this embodiment may also have a tensile strength of 1900 MPa or more (the whole of the hot stamped parts), but parts with a tensile strength of 1900 MPa or more and parts with a tensile strength of less than 1900 MPa may be mixed in the hot stamped parts. By setting parts with different strengths, the deformation state of the hot stamped parts during collision can be controlled. The hot stamped parts with parts with different strengths can be manufactured by the following methods: a method of hot stamping after joining two or more steel plates with different chemical compositions; a method of partially changing the heating temperature of the steel plate or the cooling rate after hot stamping during the hot stamping process; and a method of partially reheating the hot stamped parts, etc.

[0208] The tensile strength of the hot stamped body is obtained by collecting a small long piece from the hot stamped body, processing it into a tensile test piece without grinding the surface of the steel plate, and conducting a tensile test. Specifically, it is preferred to collect a No. 13B plate test piece from the hot stamped body in accordance with JIS Z 2241:2011, and conduct a tensile test at a tensile speed of 10 mm / min. In the case where a No. 13B plate test piece cannot be collected due to the small size or complex shape of the hot stamped body, a small long piece with a parallel portion of any width can also be collected, and a tensile test can be conducted at a tensile speed of 10 mm / min, and the tensile strength can be calculated from the maximum test force and the original cross-sectional area of ​​the parallel portion.

[0209] In addition, when the hot stamped formed body contains a mixture of high-strength portions and low-strength portions, a tensile test piece is collected from the high-strength portion.

[0210] The hot stamped body of this embodiment may also have a coating on the surface. By having a coating on the surface, the corrosion resistance can be improved after hot stamping. As the type of coating, a zinc coating or an aluminum coating can be listed. The hot stamped body having these coatings is obtained by hot stamping using a zinc-coated steel sheet or an aluminum-coated steel sheet. The coating can be formed on both sides of the hot stamped body or on a single side. The coating of the hot stamped body can be formed by hot stamping using a coated steel sheet having a coating. However, the coating of the coated steel sheet will hinder the formation of the preferred B concentration distribution and O concentration distribution in the surface area and the outermost area of ​​the hot stamped body in the process of manufacturing the hot stamped body, so it is necessary to more strictly control the manufacturing method, and it is possible that the productivity of the hot stamped body is greatly reduced. Therefore, from the perspective of productivity, the hot stamped body preferably does not have a coating on the surface.

[0211] Next, a hot stamping steel sheet which is preferable for obtaining the hot stamped body according to the present embodiment will be described.

[0212] Since the change in chemical composition caused by hot stamping is so small that it can be ignored, the chemical composition of the hot stamping steel sheet only needs to be the same as the chemical composition of the hot stamping formed body. As for the chemical composition of the hot stamping steel sheet, it is sufficient to collect a test piece from the hot stamping steel sheet and measure it by the same method as the hot stamping formed body.

[0213] The average B concentration in the area (surface area) of the steel plate at a depth of 5.0 μm to 25.0 μm from the surface of the steel plate for hot stamping is preferably less than 0.850 times the B concentration at a depth of 100 μm from the surface of the steel plate. If the average B concentration in the surface area exceeds 0.850 times the B concentration at a depth of 100 μm from the surface of the steel plate, even if the hot stamping conditions described later are applied, the B concentration distribution and the O concentration distribution cannot be preferably controlled in the surface area and the outermost area of ​​the hot stamped body. As a result, the desired collision resistance characteristics cannot be obtained in the hot stamped body. It should be noted that when the steel plate for hot stamping has a coating, the so-called surface refers to the interface between the coating and the steel plate.

[0214] The B concentration distribution in the plate thickness direction of the steel plate for hot stamping can be obtained by collecting a test piece from the steel plate for hot stamping and performing GDS analysis in the same manner as in the case of the hot stamped formed body.

[0215] Hereinafter, a method for producing a hot stamping steel sheet for obtaining a hot stamped body according to the present embodiment will be described.

[0216] The steel sheet for hot stamping is manufactured by a manufacturing method including the following steps: a hot rolling step of hot rolling a slab having the above-mentioned chemical composition to obtain a hot-rolled steel sheet; a cold rolling step of cold rolling the hot-rolled steel sheet to obtain a cold-rolled steel sheet; and an annealing step of annealing the cold-rolled steel sheet to obtain an annealed steel sheet.

[0217] The manufacturing method of the slab to be used in the manufacturing method of the steel plate for hot stamping is not particularly limited. The steel having the above-mentioned chemical composition is melted by a known means and then made into an ingot by a continuous casting method, or is made into a billet by a method such as opening a billet after being made into an ingot by any casting method. In the continuous casting process, in order to suppress the occurrence of surface defects caused by inclusions, it is preferred to generate an external additional flow such as electromagnetic stirring in the molten steel in the casting mold. The ingot or billet can be temporarily cooled and then reheated for hot rolling, or the ingot in a high temperature state after continuous casting or the billet in a high temperature state after opening a billet can be directly supplied to hot rolling, or kept warm for hot rolling, or subjected to auxiliary heating for hot rolling. Such ingots and billets are collectively referred to as "slabs" as raw materials for hot rolling.

[0218] To prevent austenite from coarsening, the heating temperature of the slab for hot rolling is preferably set to less than 1250° C., more preferably less than 1200° C. If the slab heating temperature is low, rolling becomes difficult, so the slab heating temperature may be set to 1050° C. or higher.

[0219] The heated slab is hot rolled to obtain a hot rolled steel sheet. In order to refine the metal structure of the hot rolled steel sheet by transforming the austenite phase after rolling, the hot rolling is preferably carried out at an Ar 3 The temperature is above the point.

[0220] When the hot-rolled steel sheet is coiled after hot rolling, the coiling temperature is preferably set to less than 550° C. If the coiling temperature is 550° C. or higher, thermally stable iron carbides may be generated, and the collision resistance of the hot stamped body may be deteriorated.

[0221] On the other hand, if the coiling temperature is too low, the hot-rolled steel sheet becomes excessively hardened and becomes difficult to cold-roll. Therefore, the coiling temperature is preferably set to be higher than 500°C.

[0222] After hot rolling and coiling, the hot-rolled steel sheet is pickled according to a conventional method, and then cold rolled according to a conventional method to become a cold-rolled steel sheet. In the cold rolling process, it is preferable to set the cumulative reduction rate in cold rolling to 40% or more. If the cumulative reduction rate is less than 40%, the metal structure of the steel sheet for hot stamping may coarsen. If the metal structure of the steel sheet for hot stamping is coarse, the metal structure of the hot stamped formed body after hot stamping will coarsen, which will cause the collision resistance of the formed body to decrease.

[0223] On the other hand, since excessively increasing the cumulative reduction ratio increases the load on the rolling equipment and causes a decrease in productivity, the cumulative reduction ratio is preferably set to less than 70%. After cold rolling, degreasing and other treatments may be performed according to conventional methods.

[0224] The cold rolled steel sheet is annealed to become an annealed steel sheet. In the annealing process, in order to refine the metal structure of the annealed steel sheet (hot stamping steel sheet) by recrystallization, it is preferable to set the soaking temperature to more than 700°C. If the soaking temperature is below 700°C, it is possible that the B concentration distribution cannot be preferably controlled in the surface layer region of the hot stamping steel sheet. As a result, it is possible that the desired collision resistance characteristics cannot be obtained in the hot stamping formed body.

[0225] On the other hand, if the heating rate is too slow, the soaking temperature is too high, or the soaking time is too long, the metal structure of the annealed steel sheet may be coarsened by grain growth, and the collision resistance of the hot stamping formed body may be reduced. Therefore, it is preferred to set the average heating rate until the soaking temperature to 1°C / second or more, the soaking temperature is preferably set to 800°C or less, and the soaking time (holding time at the soaking temperature) is preferably set to less than 600 seconds. In addition, it is preferred to set the dew point of the atmosphere in the annealing furnace to above -20°C and below 0°C, and to above 700°C and below (Ac 3The residence time in the temperature range (point -30°C) is set to be more than 360 seconds and less than 600 seconds. In addition, the atmosphere in the annealing furnace is preferably set to a nitrogen-hydrogen atmosphere containing 1 volume % or more and less than 4 volume % of hydrogen.

[0226] If the dew point is below -20℃ or above 0℃, or above 700℃ and below (Ac 3 If the residence time in the temperature range (0.1°C -30°C) is 360 seconds or less, the B concentration distribution in the surface layer region of the hot stamping steel sheet may not be properly controlled. As a result, the desired collision resistance characteristics may not be obtained in the hot stamped body.

[0227] On the other hand, if the residence time in the above temperature range is 600 seconds or more, excessive decarburization may occur in the hot stamping steel sheet, and the strength of the hot stamping formed body after hot stamping may be insufficient. The annealed steel sheet manufactured by the above method may be plated in a conventional manner to form a plated steel sheet. The annealed steel sheet or plated steel sheet obtained by such operation may also be tempered in a conventional manner.

[0228] It should be noted that the so-called Ac 3 The point is the temperature at which ferrite disappears in the metal structure when the raw steel sheet is heated, and can be obtained from the change in thermal expansion when the cold-rolled steel sheet is heated at a heating rate of 8° C. / sec.

[0229] The hot stamping formed body of the present embodiment can be obtained by a manufacturing method including the following steps: a heating step of heating a hot stamping steel sheet (annealed steel sheet or plated steel sheet) manufactured by the above method; and a hot stamping step of hot stamping the heated hot stamping steel sheet. In order to stably obtain the hot stamping formed body of the present embodiment, hot stamping is preferably performed by the following method.

[0230] In the heating process, the hot stamping steel sheet having the above-mentioned chemical composition and B concentration distribution in the sheet thickness direction is heated before the hot stamping process. In the heating process, it is preferred that the hot stamping steel sheet be heated by using a gas combustion furnace using a combustible gas including propane gas and setting the air ratio to 0.84 or less. It is preferred that the heating temperature be set to a temperature exceeding 950°C and exceeding Ac 3 The holding time at the heating temperature is set to be more than 360 seconds. It should be noted that the so-called air ratio refers to the relative theoretical air volume (A 0 ) The ratio of the actual air volume (A) (A / A 0 ). In addition, Ac in the heating process 3 Point is the Ac of the inner layer area of ​​the hot stamping steel sheet. 3point, as long as it is set to the same value as the Ac of the cold-rolled steel sheet obtained by the above method. 3 Just click the same value.

[0231] If the air ratio exceeds 0.84, the heating temperature is 950°C or less, or the holding time is 360 seconds or less, the B concentration distribution and the O concentration distribution in the surface layer and the outermost layer of the hot stamped body may not be controlled preferably. 3 Below this point, the volume fraction of martensite in the metal structure of the inner layer region of the hot stamped body may be insufficient, and the strength of the hot stamped body may be reduced.

[0232] On the other hand, if the heating temperature is too high or the holding time at the heating temperature is too long, the metal structure of the hot stamping body may coarsen, the collision resistance of the hot stamping body may decrease, and the strength may decrease. Therefore, the heating temperature is preferably set to less than 1050°C and the holding time is preferably set to less than 600 seconds.

[0233] In the hot stamping process, it is preferred that the hot stamping be started in a temperature range exceeding 750°C after the heated hot stamping steel sheet is taken out of the heating furnace and cooled in the atmosphere. If the starting temperature of the hot stamping is below 750°C, ferrite may be excessively generated in the metal structure of the inner layer region of the hot stamped body, and the strength of the hot stamped body may be reduced. After forming by hot stamping, the hot stamped body is cooled while being held in the die and / or the hot stamped body is taken out of the die and cooled by any method.

[0234] If the cooling rate is low, the volume fraction of martensite in the metal structure of the inner layer area of ​​the hot stamping body may be insufficient, and the strength of the hot stamping body may be reduced. Therefore, the average cooling rate from the hot stamping start temperature to 400°C is preferably set to 30°C / second or more, 60°C / second or more, or 90°C / second or more. In addition, if the cooling stop temperature is high, the volume fraction of martensite in the metal structure of the inner layer area of ​​the hot stamping body may be insufficient, and the strength of the hot stamping body may be reduced. Therefore, the cooling stop temperature using the above cooling is preferably set to less than 90°C.

[0235] The hot stamping formed body of the present embodiment is obtained by the above method. It should be noted that after hot stamping, reheating treatment can also be performed within a range that can ensure the strength of the hot stamping formed body. In the case of reheating treatment, the heating temperature is preferably set to be lower than (Ac 3 point -100℃). If the heating temperature of the reheating treatment is (Ac 3If the temperature is above -100°C, the surface area and the outermost area of ​​the hot stamping body may not be fully softened, and the collision resistance of the hot stamping body may be reduced. It is also possible to reheat a part of the hot stamping body by laser irradiation or the like to partially set a softened area. In addition, the hot stamping body may be sandblasted, or painted and baked.

[0236] Example

[0237] Next, the embodiment of the present invention will be described, but the conditions in the embodiment are a conditional example adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this conditional example. As long as it does not deviate from the gist of the present invention and achieves the purpose of the present invention, the present invention can adopt various conditions.

[0238] The molten steel was cast using a vacuum melting furnace to obtain a steel having the chemical composition shown in Table 1. The obtained steel was heated to 1200°C and maintained for 60 minutes, and then hot rolled 10 times in a temperature range above 900°C to obtain a hot-rolled steel plate with a thickness of 3.5 mm. After hot rolling, the hot-rolled steel plate was cooled to 540°C by water spray. The cooling end temperature was set to the coiling temperature, and the hot-rolled steel plate was loaded into an electric heating furnace maintained at the coiling temperature for 60 minutes. After that, the hot-rolled steel plate was furnace cooled to room temperature at an average cooling rate of 20°C / hour to simulate slow cooling after coiling. The hot-rolled steel plate after furnace cooling was pickled and then cold rolled to obtain a cold-rolled steel plate with a thickness of 1.4 mm. The cumulative reduction rate during cold rolling was set to 60%.

[0239] It should be noted that “-” in Table 1 indicates that the content of the element is lower than the detection limit.

[0240] Ac in Table 1 3 The point was obtained from the change in thermal expansion when the cold-rolled steel sheets of Steels A to N were heated at 8° C. / sec.

[0241] The obtained cold-rolled steel sheet was annealed using a continuous annealing simulator under the annealing conditions shown in Table 2A and Table 2B. It should be noted that the steel sheet was heated to the soaking temperature described in Table 2A and Table 2B at an average heating rate of 8°C / second. The atmosphere in the annealing furnace was set to a nitrogen-hydrogen atmosphere containing 3% hydrogen by volume, and the dew point was set as described in Table 2A and Table 2B. After soaking, the steel sheet was cooled to room temperature to obtain an annealed steel sheet (steel sheet for hot stamping).

[0242] GDS analysis test pieces were collected from 3 locations of the obtained hot stamping steel plate, and the surface of the test piece was set as the measurement start surface. By the above method, GDS analysis was performed from the measurement start surface along the plate thickness direction to a depth position of 120 μm. Thus, the average B concentration in the area (surface area) with a depth of 5.0 μm to 25.0 μm from the surface of the hot stamping steel plate and the B concentration at a depth position of 100 μm from the surface were obtained. The measurement points from the surface of the steel plate to the depth position of 100 μm were set to 1500 points. The obtained results are shown in Table 2.

[0243] Next, a raw material sheet for hot stamping having a width of 240 mm and a length of 800 mm was collected from the obtained hot stamping steel sheet and hot stamped to obtain Figure 1 A hat-shaped component (hot stamped formed body) of the shape shown in . In the hot stamping process, a gas combustion furnace is used to heat the raw material plate for hot stamping under the conditions shown in Table 3. Specifically, propane gas is used as the combustion gas, and the heating temperature, holding time, and air ratio are set to the conditions shown in Table 3. Thereafter, the raw material plate for hot stamping is taken out of the heating furnace and cooled, and then clamped in a mold equipped with a cooling device, and the forming start temperature is set to above 770°C to perform hat-shaped forming. Next, the average cooling rate from the forming start temperature to 400°C is set to above 50°C / second, and the mold is cooled to a cooling stop temperature of below 80°C. In addition, the oxide scale (iron oxide) generated on the surface of the hat-shaped component is removed by shot peening.

[0244] A test piece was collected from the vertical wall portion of the obtained hat-shaped member, and the chemical composition was measured by the above-mentioned method.

[0245] The tensile strength was determined by sampling a No. 13B plate-shaped test piece from the vertical wall portion of the hat-shaped member along the longitudinal direction of the hat-shaped member in accordance with JIS Z 2241:2011 and performing a tensile test at a tensile speed of 10 mm / min.

[0246] When the obtained tensile strength is 1900 MPa or more, it is judged as having high strength and is passed. On the other hand, when the obtained tensile strength is less than 1900 MPa, it is judged as not having high strength and is failed.

[0247] In addition, GDS analysis test pieces were collected from three locations of the vertical wall of the hat-shaped member, and the surface of the test piece was set as the measurement start surface. By the above method, GDS analysis was performed from the measurement start surface along the plate thickness direction to a depth of 120 μm. Thus, the average B concentration in the area with a depth of 5.0 μm to 25.0 μm from the surface (surface area), the average B concentration and the average O concentration in the area with a depth of 0.5 μm to 4.0 μm from the surface (topmost area), and the B concentration at a depth of 100 μm from the surface were obtained. The measurement points from the surface of the steel plate to the depth of 100 μm were set to 1500 points.

[0248] In addition, a test piece for tissue observation was collected from the longitudinal wall portion of the hat-shaped component. After the longitudinal section of the test piece was polished, the metal structure in the area with a depth of 0.5 μm to 4.0 μm from the surface (the outermost area) and the area with a depth of 100 μm to 1 / 2 of the plate thickness (the inner layer area) was observed by the above-mentioned method.

[0249] In addition, if Figure 2 As shown in , a test piece for a three-point bending test was obtained by welding a closing plate having a thickness of 1.4 mm, a width of 130 mm, and a length of 800 mm to a hat-shaped member. A steel plate having a tensile strength of 1553 MPa was used for the closing plate.

[0250] For the obtained test body, Figure 3 As shown in the figure, a test piece with a length of 800 mm was placed on two support rollers arranged with a roller interval of 700 mm in a manner such that the closing plate was at the bottom, and a three-point bending test was performed at a test speed of 2 m / s. Thus, the maximum load and the displacement from the time when the test piece came into contact with the impactor until cracks began to occur in the test piece (crack occurrence displacement) were obtained.

[0251] When the tensile strength of the steel sheet constituting the hot stamping formed body is less than 2300 MPa, the case where the maximum load is 18.0 kN or more and the displacement caused by cracking is 50 mm or more is judged as having excellent collision resistance characteristics and is qualified. In addition, when the tensile strength is 2300 MPa or more, the case where the maximum load is 23.0 kN or more and the displacement caused by cracking is 35 mm or more is judged as having excellent collision resistance characteristics and is qualified. The case that does not meet these conditions is judged as not having excellent collision resistance characteristics and is unqualified.

[0252] Tables 4A and 4B show the results of measuring the chemical composition of the hot stamped bodies, the results of measuring the mechanical properties of the hot stamped bodies, the results of measuring the concentration distribution of B and O in the hot stamped bodies, and the results of evaluating the collision resistance characteristics of the hot stamped bodies.

[0253] In addition, the contents of elements other than C in the hot stamped formed body are the same as the contents of the elements shown in Table 1, and thus are omitted.

[0254] [Table 1]

[0255]

[0256] [Table 2A]

[0257]

[0258] [Table 2B]

[0259]

[0260] [Table 3]

[0261]

[0262] The underline indicates that the manufacturing conditions are not preferred.

[0263] [Table 4A]

[0264]

[0265] [Table 4B]

[0266]

[0267] The hot stamped formed body of the present invention has a tensile strength of 1900 MPa or more, which is high in strength. In addition, the average B concentration in the surface layer is low, and the average B concentration and average O concentration in the outermost layer are high, which is excellent in collision resistance.

[0268] The metal structure of the hot stamped body of the present invention example has a volume fraction of martensite of 91.0% or more in the inner layer region, and a total volume fraction of structures other than martensite of 9.0% or less.

[0269] Furthermore, in the outermost surface region, the volume fraction of ferrite is 6.0% or more, and the total volume fraction of structures other than ferrite is 94.0% or less.

[0270] In contrast, in the comparative examples (test numbers 1, 5 and 17) in which the chemical composition of the hot stamped bodies deviates from the scope of the invention, the C content is too low or the sol.Al content is too high, so the tensile strength of the hot stamped bodies becomes lower than 1900 MPa, resulting in poor strength, and the maximum load is low, resulting in poor collision resistance.

[0271] Test No. 15 had too high a C content, so the hot stamped body had low crack generation displacement and poor collision resistance. In addition, in the tensile test, premature fracture occurred and the tensile strength could not be determined, and the fracture strength was less than 1900 MPa.

[0272] Test No. 16 has a low B content, so the tensile strength of the hot stamped body is less than 1900 MPa and the strength is poor. In addition, the average B concentration and average O concentration in the outermost layer region are low, the maximum load and cracking displacement are low, and the collision resistance is poor.

[0273] In the comparative examples of test numbers 3, 4, 7, 8, 10, 11, 13, 14, 24, 25 and 27, in which the chemical composition of the hot stamped body is within the preferred range but the manufacturing conditions are out of the preferred conditions, at least one of the average B concentration in the surface region, the average B concentration in the outermost region and the average O concentration in the outermost region is out of the scope of the invention. Therefore, the hot stamped body has a low crack initiation displacement, or a low maximum load and a low crack initiation displacement, and the collision resistance is poor.

[0274] Industrial Applicability

[0275] According to the above aspects of the present invention, it is possible to provide a hot stamped body having high strength and excellent collision resistance.

Claims

1. A hot stamping formed body, characterized in that: The hot stamped body comprises a steel plate, the chemical composition of all or part of the steel plate containing, in mass %, the following: C: more than 0.32% and less than 0.70%, Si: less than 2.00%, Mn: 0.01~3.00%, P: 0.200% or less, S: 0.0200% or less, Sol.Al: 0.001~1.000%, N: 0.0200% or less, O:0.0005~0.0200%、 B:0.0005~0.0200%、 Cr:0~2.00%、 Mo: 0-2.00%, W:0~2.00%、 Cu: 0-2.00%, Ni: 0-2.00%, Ti: 0~0.200%, Nb: 0~0.200%, V:0~0.200%、 Zr:0~0.200%、 Ca: 0~0.1000%, Mg: 0~0.1000%, REM: 0~0.1000%、 Sn: 0~0.200%, As: 0~0.100%, and Bi: 0~0.0500%, The rest contains Fe and impurities. The tensile strength is above 1900MPa. The average B concentration in the region of the steel sheet at a depth of 5.0 μm to 25.0 μm from the surface is 0.700 times or less the B concentration at a depth of 100 μm from the surface, The average B concentration in the region at a depth of 0.5 μm to 4.0 μm from the surface is 1.600 times or more the B concentration at the position at a depth of 100 μm from the surface, The average O concentration in the region at a depth of 0.5 μm to 4.0 μm from the surface exceeds 0.0150 mass %.

2. The hot stamped body according to claim 1, characterized in that: The chemical composition contains one or more of the following elements in mass %: Cr:0.01~2.00%、 Mo: 0.01~2.00%, W:0.01~2.00%、 Cu: 0.01-2.00%, Ni: 0.01-2.00%, Ti: 0.001~0.200%, Nb: 0.001~0.200%, V:0.001~0.200%、 Zr:0.001~0.200%、 Ca: 0.0001~0.1000%, Mg: 0.0001~0.1000%, REM: 0.0001~0.1000%、 Sn: 0.001~0.200%, As: 0.001~0.100%, and Bi: 0.0001~0.0500%.